High-strength anti-aging PPO plastic particles and preparation method thereof

By using specific raw materials and granulation module design, the existing plastic particles have been solved, and the preparation of high-strength anti-aging PPO plastic particles is achieved, which extends the material life and improves the preparation efficiency.

CN118909426AInactive Publication Date: 2024-11-08ANHUI JIANGDIAN NEW MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411068076.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing plastic particles have low strength and poor anti-aging effects, resulting in short service life of materials, resulting in waste of resources and environmental pollution. At the same time, the preparation efficiency is low and the plastic particles of different sizes cannot be prepared as needed.

Method used

Using PPO resin, ABS resin, PP resin, wear-resistant additive, composite anti-aging agent and nano zinc oxide, etc., high-strength anti-aging PPO plastic particles are prepared through specific mixing and heating processes, and the injection materials of the granulation module are used. -Cooling-Release design improves preparation efficiency and can adjust particle size according to demand.

Benefits of technology

It significantly improves the strength and anti-aging properties of plastic particles, extends the service life of materials, reduces resource waste and environmental pollution, and improves the preparation efficiency of plastic particles, so that particles of different sizes can be prepared as needed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909426A_ABST
    Figure CN118909426A_ABST
Patent Text Reader

Abstract

The invention relates to high-strength anti-aging PPO plastic particles and a preparation method thereof. The high-strength anti-aging PPO plastic particles are prepared from the following components: PPO resin, ABS resin, PP resin, a wear-resistant additive, a composite anti-aging agent, hexamethylphosphoramide, a compatilizer and a reinforcing agent. The composite anti-aging agent is prepared from the following components: calcium silicate, stearic acid, unsaturated polyester resin, an ultraviolet light absorber, nano zinc oxide, polyethylene, an interface modifier, a plasticizer, a dispersion lubricant and nano titanium dioxide; the calcium silicate, the stearic acid, the unsaturated polyester resin, the ultraviolet light absorber, the nano zinc oxide, the polyethylene, the interface modifier, the plasticizer, the dispersion lubricant and the nano titanium dioxide are prepared into the composite anti-aging agent, so that the impact strength and the anti-aging capability of the plastic can be effectively improved, and the service life of the material is prolonged; and great waste of resources and serious environmental pollution caused by plastic aging are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of plastic particle preparation, and in particular to a high-strength anti-aging PPO plastic particle and a preparation method thereof. Background Art

[0002] Plastics are widely used in life because of their light weight, corrosion resistance, and good insulation. Plastic products can be seen everywhere in daily life. Their application fields are very wide, and each field is inseparable from plastic products. Existing plastic products have poor antioxidant properties. With the passage of time, plastic products will change color, become brittle, and have reduced smoothness due to oxidation during use, which affects the appearance and performance of plastic products.

[0003] The existing technology can also realize the function of preparing plastic particles, but when preparing plastic particles, the strength of the plastic is low and the anti-aging effect is poor, resulting in a short service life of the material and a large amount of waste, causing a huge waste of resources and serious environmental pollution; secondly, the preparation effect of plastic particles is poor, and usually a method of preparing them into strips and then cooling and cutting them is adopted, which makes the processing efficiency of plastic particles low, and it is impossible to prepare plastic particles of the required size according to the use requirements; based on this, there is still room for improvement on the basis of the existing plastic particle preparation. Summary of the invention

[0004] In order to accurately prepare high-strength anti-aging PPO plastic particles and accurately granulate plastic particles, the present application provides high-strength anti-aging PPO plastic particles and a preparation method thereof.

[0005] The high-strength anti-aging PPO plastic particles provided in this application adopt the following technical solutions: In a first aspect, the present application provides a high-strength anti-aging PPO plastic particle, comprising the following raw materials in parts by weight: 42-48 parts of PPO resin, 32-35 parts of ABS resin, 10-12 parts of PP resin, 3-8 parts of wear-resistant additive, 0.6-1.2 parts of composite anti-aging agent, 0.6-1.2 parts of hexamethylphosphoric triamide, 0.6-0.8 parts of compatibilizer, and 0.4-0.7 parts of reinforcing agent; Preferably, the composite anti-aging agent is composed of the following raw materials in parts by weight: 13-17 parts of calcium silicate, 11-15 parts of stearic acid, 14-16 parts of unsaturated polyester resin, 8-10 parts of ultraviolet absorber, 11-13 parts of nano zinc oxide, 8-10 parts of polyethylene, 4-8 parts of interface modifier, 12-18 parts of plasticizer, 5-7 parts of dispersing lubricant, and 10-14 parts of nano titanium dioxide.

[0006] Preferably, the particle size of the nano titanium dioxide is 20-40 nm.

[0007] In a second aspect, the present application provides a method for preparing high-strength anti-aging PPO plastic particles, comprising the following steps: Step S1, under the protection of inert gas, mixing and stirring the required weight of calcium silicate, stearic acid, and unsaturated polyester resin, and then heating to 80-100° C., adding nano zinc oxide and polyethylene while hot, stirring at high speed, adding interface modifier and plasticizer, continuing to heat to 120-140° C., stirring evenly, keeping warm for 15-25 minutes, and then cooling to room temperature, then adding dispersing lubricant, ultraviolet absorber and nano titanium dioxide to the above mixture, reheating to a molten state, keeping warm and stirring at high speed for 20-30 minutes, and then naturally cooling to room temperature to obtain a composite anti-aging agent; Step S2, adding PPO resin, ABS resin, PP resin, wear-resistant additive, composite anti-aging agent, hexamethylphosphoric acid triamide, compatibilizer and reinforcing agent into a high-speed mixer and mixing for 2 minutes, and then standing at 40-50° C. in vacuum for 2-4 hours to obtain a blend; Step S3, transferring the blended material to a granulation module, and the granulation module extrude and granulate the molten blended material to obtain high-strength anti-aging PPO plastic particles.

[0008] Preferably, the inert gas in step S1 is nitrogen or carbon dioxide.

[0009] Preferably, the granulation module includes: a storage barrel, which is a cylindrical hollow structure, and an annular storage cavity is arranged in the middle of the storage barrel; a driving assembly, which is installed inside the storage barrel; a plurality of injection assemblies, which are evenly installed on the outer side of the lower end of the storage barrel, and the upper end of the injection assembly is connected with the annular storage cavity inside the storage barrel; a granulation assembly, which is installed at the lower end of the driving assembly, the granulation assembly is a cylindrical structure, and the outer side surface of the granulation assembly is evenly provided with depth-adjustable granulation holes along its circumference, the inner side surface of the injection assembly is in close contact with the outer surface of the granulation assembly, the driving assembly is used to drive the granulation assembly to rotate at a uniform speed, and the injection assembly is configured to extrude the molten mixture into the granulation hole, and drive the mixture inside the granulation hole to cool and shape, and then push it out to prepare PPO plastic particles.

[0010] Preferably, the driving assembly includes a driving motor, a supporting frame, a rotating shaft and a stirring frame. The supporting frame is installed at the upper end of the storage barrel, the driving motor is installed at the upper end of the supporting frame, the rotating shaft is installed on the output shaft of the driving motor, the stirring frame is evenly installed on the upper end of the rotating shaft, the stirring frame is located inside the annular storage cavity, and the lower end of the rotating shaft is connected to the granulation assembly.

[0011] Preferably, the injection assembly includes an injection rack, a spiral feed rack, a partition, a cleaning piece and a scraper. The injection rack is in a rectangular long strip structure, the injection rack is arranged vertically downward, a feed trough is provided in the middle of the injection rack, a spiral feed rack is installed inside the feed trough, the upper end of the spiral feed rack extends into the annular storage cavity, the spiral feed rack is used to transport the molten blend in the annular storage cavity downward along the feed trough, a partition is provided on the outside of the feed trough, the inner side of the partition is in close contact with the surface of the granulation assembly, through holes are evenly provided on the partition, and two vertical downward mounting grooves are also provided on the injection rack, the two mounting grooves are symmetrically arranged about the feed trough, and the cleaning piece and the scraper are respectively installed in the mounting grooves.

[0012] Preferably, a cooling component is also provided on the outer side of the granulation component, and the cooling component is slidably arranged up and down at a position between adjacent injection components. The cooling component includes a sliding plate slidably arranged on the side wall of the injection component and an arc plate evenly arranged between the two sliding plates, and cooling nozzles for cooling the extruded molten blend are evenly arranged on the inner concave surface of the arc plate.

[0013] Preferably, the granulation assembly includes a granulation roller, a granulation frame, a feeding mechanism, a guide frame and an adjusting mechanism, which is a cylindrical hollow structure. The granulation roller is installed at the lower end of the driving assembly. Rectangular through grooves are evenly arranged on the outer side of the granulation roller. A granulation frame is installed on the outer side of the rectangular through groove. The granulation holes are evenly arranged on the granulation frame. A feeding mechanism is installed on the inner side of the rectangular through groove. An adjusting mechanism is arranged inside the granulation roller. The upper end of the adjusting mechanism is installed on the lower end surface of the storage barrel. Guide frames are evenly arranged on the outer side of the adjusting mechanism. The inner side of the feeding mechanism is in close contact with the guide frame. The guide frame is used to adjust the depth of the granulation holes and push out the cooled and formed blended material through the feeding mechanism.

[0014] Preferably, the ejecting mechanism includes a mounting plate, a push plate, a ejector rod, a connecting spring and a ejector plate, a mounting plate is installed on the inner side of the rectangular through groove, circular holes are evenly arranged on the mounting plate, ejector rods are slidably arranged in the circular holes, an ejector rod is installed on the inner side surface of the ejector rod, the inner side surface of the ejector rod is a smooth arc-shaped surface, a connecting spring is arranged on the ejector rod, a push plate is installed between the outer side surfaces of the ejector rod, ejector plates are evenly installed on the push plate, and the ejector plates correspond one-to-one to the granulation holes.

[0015] Preferably, the guide frame is in a circular ring structure, and step grooves and ejection protrusions are evenly arranged inside the guide frame. The step grooves and the ejection protrusions are smoothly connected. The step grooves include a plurality of arc grooves with gradually decreasing depths, and adjacent arc grooves are smoothly connected.

[0016] Preferably, the adjustment mechanism includes a fixed frame, a connecting plate and a sliding sleeve. There are multiple fixed frames, and the fixed frames are rectangular frames arranged vertically downward. The upper ends of adjacent fixed frames are connected by connecting plates, and the connecting plates are connected to the storage barrel by screws. A vertical downward sliding groove is provided on the outside of the fixed frame, and an electric slider is installed in the sliding groove. The sliding sleeve is sleeved on the outside of the fixed frame, the fixed frame is connected to the electric slider, and the guide frame is installed on the outside of the sliding sleeve.

[0017] In the above technical scheme, the present invention provides a high-strength anti-aging PPO plastic particle. The composite anti-aging agent provided by the present invention has excellent strength and anti-aging effect, prolongs the service life of the material, and avoids the great waste of resources and serious environmental pollution caused by plastic aging; at the same time, the injection component and the granulation component are used in conjunction with each other, so that the granulation component can accurately granulate the plastic, and the granulation adopts the design method of injection-cooling-pushing, which greatly improves the preparation efficiency of the plastic particles, and the size of the plastic particles can be adjusted according to the use requirements, which is convenient for the subsequent use of the plastic particles. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0019] Figure 1 It is a three-dimensional structural schematic diagram of this application.

[0020] Figure 2 It is a schematic diagram of the cutaway structure of this application.

[0021] Figure 3 It is a schematic diagram of the longitudinal cross-sectional structure of the present application.

[0022] Figure 4 It is a schematic diagram of the transverse cross-sectional structure of the present application.

[0023] Figure 5 It is a schematic diagram of the three-dimensional structure between the material storage barrel, the driving assembly and the injection assembly of the present application.

[0024] Figure 6 It is a schematic diagram of the cross-sectional structure of the injection component of the present application.

[0025] Figure 7 It is a schematic diagram of the three-dimensional structure between the injection component and the granulation component of the present application.

[0026] Figure 8 It is a schematic diagram of the cross-sectional structure of the granulation component of the present application.

[0027] Fig. 9 It is a schematic diagram of the cross-sectional structure between the granulation frame, the ejecting mechanism and the guide frame of the present application.

[0028] Fig.10 It is a schematic diagram of the three-dimensional structure between the guide frame and the adjustment mechanism of the present application.

[0029] Fig.11 It is a three-dimensional structural schematic diagram of the guide frame of the present application.

[0030] Explanation of the accompanying drawings: 1. Storage barrel; 2. Driving assembly; 21. Driving motor; 22. Support frame; 23. Rotating shaft; 24. Stirring frame; 3. Injection assembly; 31. Injection frame; 32. Spiral feed frame; 33. Partition; 34. Cleaning piece; 35. Scraping piece; 4. Granulation assembly; 40. Cooling piece; 401. Sliding plate; 402. Arc plate; 41. Granulation roller; 42. Granulation frame; 43. Ejection mechanism; 431. Mounting plate; 432. Push plate; 433. Ejector rod; 434. Connecting spring; 435. Ejector plate; 44. Guide frame; 441. Step groove; 442. Ejection protrusion; 45. Adjustment mechanism; 451. Fixed frame; 452. Connecting plate; 453. Sliding sleeve. DETAILED DESCRIPTION

[0031] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings.

[0032] In the embodiment of the present invention, the plasticizer is phthalate plasticizer, the dispersing lubricant is liquid paraffin, the ultraviolet absorber is UV-0, the wear-resistant additive is nano calcium carbonate, the compatibilizer is a cyclic anhydride type reactive compatibilizer, the reinforcing agent is DH-2 reinforcing agent, and the interface modifier is silane coupling agent KH550.

[0033] Example 1: A high-strength anti-aging PPO plastic particle, the preparation method of which is as follows: Under nitrogen protection, 13 parts of calcium silicate, 11 parts of stearic acid, and 14 parts of unsaturated polyester resin were mixed and stirred evenly, and then heated to 80°C. While hot, 11 parts of nano zinc oxide and 8 parts of polyethylene were added, and after high-speed stirring, 4 parts of interface modifier and 12 parts of plasticizer were added. The temperature was continued to rise to 120°C, stirred evenly, and kept warm for 15 minutes, and then cooled to room temperature. Then, 5 parts of dispersing lubricant, 8 parts of ultraviolet absorber and 10 parts of nano titanium dioxide were added to the above mixture. The particle size of the nano titanium dioxide was 20nm, and the mixture was reheated to a molten state, and kept warm at high speed. After stirring for 20 minutes, naturally cool to room temperature to obtain a composite anti-aging agent; add 42 parts of PPO resin, 32 parts of ABS resin, 10 parts of PP resin, 3 parts of wear-resistant additive, 0.6 parts of composite anti-aging agent, 0.6 parts of hexamethylphosphoric triamide, 0.6 parts of compatibilizer and 0.4 parts of reinforcing agent into a high-speed mixer and mix for 2 minutes, and then stand at 40°C in vacuum for 2 hours to obtain a blend; transfer the blend to a granulation module, and the granulation module extrude and granulate the molten blend to obtain high-strength anti-aging PPO plastic particles.

[0034] Example 2: A high-strength anti-aging PPO plastic particle, the preparation method of which is as follows: Under nitrogen protection, 15 parts of calcium silicate, 13 parts of stearic acid and 15 parts of unsaturated polyester resin were mixed and stirred evenly, and then heated to 90°C. 12 parts of nano zinc oxide and 9 parts of polyethylene were added while hot, and 6 parts of interface modifier and 15 parts of plasticizer were added after high-speed stirring. The temperature was continued to rise to 130°C, stirred evenly, and kept warm for 20 minutes, and then cooled to room temperature. 6 parts of dispersing lubricant, 9 parts of ultraviolet absorber and 2 parts of nano titanium dioxide were added to the above mixture, and the particle size of the nano titanium dioxide was 30nm. The mixture was reheated to a molten state, and kept warm and stirred at high speed for 2 minutes. After 5 minutes, it was naturally cooled to room temperature to obtain a composite anti-aging agent; 45 parts of PPO resin, 33.5 parts of ABS resin, 11 parts of PP resin, 5.5 parts of wear-resistant additives, 0.9 parts of composite anti-aging agents, 0.9 parts of hexamethylphosphoric triamide, 0.7 parts of compatibilizers and 0.55 parts of reinforcing agents were added into a high-speed mixer and mixed for 2 minutes, and then allowed to stand in vacuum at 45°C for 3 hours to obtain a blend; the blend was transferred to a granulation module, and the granulation module extruded and granulated the molten blend to obtain high-strength anti-aging PPO plastic particles.

[0035] Example 3: A high-strength anti-aging PPO plastic particle, the preparation method of which is as follows: Under the protection of carbon dioxide gas, 17 parts of calcium silicate, 15 parts of stearic acid and 16 parts of unsaturated polyester resin were mixed and stirred evenly, and then heated to 100°C. 13 parts of nano zinc oxide and 10 parts of polyethylene were added while hot, and 8 parts of interface modifier and 18 parts of plasticizer were added after high-speed stirring. The temperature was continued to rise to 140°C, stirred evenly, and kept warm for 25 minutes, and then cooled to room temperature. 7 parts of dispersing lubricant, 10 parts of ultraviolet absorber and 14 parts of nano titanium dioxide were added to the above mixture, and the particle size of the nano titanium dioxide was 40nm. The mixture was reheated to a molten state and kept warm for 25 minutes. After high-speed stirring at high temperature for 30 minutes, it is naturally cooled to room temperature to obtain a composite anti-aging agent; 48 parts of PPO resin, 35 parts of ABS resin, 12 parts of PP resin, 8 parts of wear-resistant additives, 1.2 parts of composite anti-aging agent, 1.2 parts of hexamethylphosphoric triamide, 0.8 parts of compatibilizer and 0.7 parts of reinforcing agent are added into a high-speed mixer and mixed for 2 minutes, and then vacuum-stirred at 50°C for 4 hours to obtain a blend; the blend is transferred to a granulation module, and the granulation module extrudes and granulates the molten blend to obtain high-strength anti-aging PPO plastic particles.

[0036] Example 4: A high-strength anti-aging PPO plastic particle, the preparation method of which is as follows: Under the protection of carbon dioxide gas, 17 parts of calcium silicate, 15 parts of stearic acid and 16 parts of unsaturated polyester resin were mixed and stirred evenly, and then heated to 100°C. 14 parts of nano zinc oxide and 10 parts of polyethylene were added while hot, and 8 parts of interface modifier and 17 parts of plasticizer were added after high-speed stirring. The temperature was continued to rise to 140°C, stirred evenly, and kept warm for 25 minutes, and then cooled to room temperature. 7 parts of dispersing lubricant, 10 parts of ultraviolet absorber and 14 parts of nano titanium dioxide were added to the above mixture, and the particle size of the nano titanium dioxide was 40nm. The mixture was reheated to a molten state and kept warm for 25 minutes. After high-speed stirring at high temperature for 30 minutes, it is naturally cooled to room temperature to obtain a composite anti-aging agent; 48 parts of PPO resin, 35 parts of ABS resin, 12 parts of PP resin, 8 parts of wear-resistant additives, 1.1 parts of composite anti-aging agent, 1.2 parts of hexamethylphosphoric triamide, 0.8 parts of compatibilizer and 0.6 parts of reinforcing agent are added into a high-speed mixer and mixed for 2 minutes, and then vacuum-stirred at 50°C for 4 hours to obtain a blend; the blend is transferred to a granulation module, and the granulation module extrudes and granulates the molten blend to obtain high-strength anti-aging PPO plastic particles.

[0037] Comparative Example 1: A high-strength anti-aging PPO plastic particle, the preparation method of which is: Under nitrogen protection, 20 parts of calcium silicate, 18 parts of stearic acid, and 11 parts of unsaturated polyester resin were mixed and stirred evenly, and then heated to 70°C. 13 parts of nano zinc oxide and 8 parts of polyethylene were added while hot, and 8 parts of interface modifier and 13 parts of plasticizer were added after high-speed stirring. The temperature was continued to rise to 150°C, stirred evenly, and kept warm for 30 minutes, and then cooled to room temperature. 5 parts of dispersing lubricant, 6 parts of ultraviolet absorber and 16 parts of nano titanium dioxide were added to the above mixture, and the particle size of the nano titanium dioxide was 60nm. The mixture was reheated to a molten state, and kept warm at high speed. After stirring for 30 minutes, naturally cool to room temperature to obtain a composite anti-aging agent; add 42 parts of PPO resin, 35 parts of ABS resin, 13 parts of PP resin, 6 parts of wear-resistant additives, 0.5 parts of composite anti-aging agent, 0.5 parts of hexamethylphosphoric triamide, 0.7 parts of compatibilizer and 0.5 parts of reinforcing agent into a high-speed mixer and mix for 2 minutes, and then stand at 30°C in vacuum for 3 hours to obtain a blend; transfer the blend to a granulation module, and the granulation module extrude and granulate the molten blend to obtain high-strength anti-aging PPO plastic particles.

[0038] Comparative Example 2: A high-strength anti-aging PPO plastic particle, the preparation method of which is as follows: Under the protection of carbon dioxide gas, 15 parts of calcium silicate, 14 parts of stearic acid and 15 parts of unsaturated polyester resin were mixed and stirred evenly, and then heated to 80°C. While hot, 10 parts of nano zinc oxide and 10 parts of polyethylene were added, and after high-speed stirring, 4-8 parts of interface modifier and 12-18 parts of plasticizer were added. The temperature was continued to rise to 120-140°C, stirred evenly, and kept warm for 15 minutes, and then cooled to room temperature. Then 6 parts of dispersing lubricant, 10 parts of ultraviolet absorber and 10 parts of nano titanium dioxide were added to the above mixture. The particle size of nano titanium dioxide was 80nm, and the mixture was reheated until it melted. state, keep warm and stir at high speed for 30 minutes, then cool naturally to room temperature to obtain a composite anti-aging agent; add 40 parts of PPO resin, 33 parts of ABS resin, 15 parts of PP resin, 8 parts of wear-resistant additives, 0.3 parts of composite anti-aging agent, 1.5 parts of hexamethylphosphoric triamide, 0.8 parts of compatibilizer and 0.4 parts of reinforcing agent into a high-speed mixer and mix for 2 minutes, then stand still at 60°C in vacuum for 3 hours to obtain a blend; transfer the blend to a granulation module, and the granulation module extrude and granulate the molten blend to obtain high-strength anti-aging PPO plastic particles.

[0039] Impact strength test: refer to the method in "Plastics. Determination of impact properties of simply supported beams. Part 1" GB / T1043.1-2008.

[0040] Aging resistance test: Refer to "Plastic Laboratory Light Source Exposure Test Method" GB / T16422.2-2014, simulate sunlight, use a filter to filter the xenon arc lamp, and after irradiation for 600 hours, test the impact strength according to the above impact strength test method. The test results are shown in Table 1.

[0041] Impact strength retention rate = impact strength after aging / impact strength before aging × 100%; The test results are shown in Table 1: project <![CDATA[Izod impact strength before aging (kJ / m 2 )]]> <![CDATA[Izod impact strength after aging (kJ / m 2 )]]> Impact strength retention rate (%) Example 1 14.4 13.3 92.4 Example 2 15.8 14.7 93.0 Example 3 15.5 14.4 92.9 Example 4 15.3 14.3 93.5 Comparative Example 1 13.7 10.3 75.2 Comparative Example 2 12.7 9.2 72.4 Comparative Example 3 11.2 8.0 71.4 It can be seen from Table 1 that the impact strength and aging resistance of Examples 1-4 are significantly higher than those of the comparative example. The present invention can prepare high-strength aging-resistant PPO plastic particles.

[0042] See also Figure 1-11 As shown, as the preferred technical solution of this embodiment, the granulation module includes: a storage barrel 1, which is a cylindrical hollow structure, and an annular storage cavity is arranged in the middle of the storage barrel 1; a driving component 2, which is installed inside the storage barrel 1; an injection component 3, which is multiple in number, and the injection components 3 are evenly installed on the outer side of the lower end of the storage barrel 1, and the upper end of the injection component 3 is connected with the annular storage cavity inside the storage barrel 1; a granulation component 4, which is installed at the lower end of the driving component 2, the granulation component 4 is a cylindrical structure, and the outer surface of the granulation component 4 is evenly provided with depth-adjustable granulation holes along its circumference, the inner side surface of the injection component 3 is in close contact with the outer surface of the granulation component 4, the driving component 2 is used to drive the granulation component 4 to rotate at a uniform speed, and the injection component 3 is configured to extrude the molten blend into the granulation hole, and drive the blend inside the granulation hole to cool and shape and then push it out to prepare PPO plastic particles.

[0043] In the above technical scheme, the prepared molten blend is added into the storage barrel 1, and the injection component 3 drives the blend to be transported downward. When the blend fills the injection component 3, the blend is extruded from the inside of the injection component 3. At the same time, the driving component 2 can drive the granulation component 4 to rotate at a constant speed. When the granulation hole outside the granulation component 4 moves to the inside of the injection component 3, the molten blend will be squeezed into the granulation hole. When the granulation hole moves out from the inside of the injection component 3, the blend inside the granulation hole is pushed out after cooling and shaping, so as to accurately form high-strength and anti-aging PPO plastic particles of the same size.

[0044] It should be noted that the depth of the granulation holes on the outer surface of the granulation component 4 is adjustable. When plastic particles of different sizes are needed, the depth of the granulation holes can be adjusted to obtain the functions of plastic particles of different sizes, thereby meeting different usage requirements.

[0045] See also Figure 5As shown, as the preferred technical solution of this embodiment, the driving assembly 2 includes a driving motor 21, a support frame 22, a rotating shaft 23 and a stirring frame 24. The support frame 22 is installed at the upper end of the storage barrel 1, and the driving motor 21 is installed at the upper end of the support frame 22. The rotating shaft 23 is installed on the output shaft of the driving motor 21, and the stirring frame 24 is evenly installed on the upper end of the rotating shaft 23. The stirring frame 24 is located inside the annular storage cavity, and the lower end of the rotating shaft 23 is connected to the granulation assembly 4.

[0046] In the above technical solution, the driving motor 21 can drive the stirring frame 24 to rotate through the rotating shaft 23 to prevent the molten copolymer inside the annular storage chamber from solidifying. At the same time, the rotating shaft 23 can drive the granulation component 4 to rotate at a uniform speed, so that the injection component 3 can squeeze the molten copolymer into the surface of the granulation component 4, which is beneficial to the continuous preparation of plastic particles.

[0047] See also Figure 5-6 As shown, as the preferred technical solution of this embodiment, the injection assembly 3 includes an injection frame 31, a spiral feed frame 32, a partition 33, a cleaning piece 34 and a scraper 35. The injection frame 31 is a rectangular long strip structure, the injection frame 31 is arranged vertically downward, a feed trough is arranged in the middle of the injection frame 31, a spiral feed frame 32 is installed inside the feed trough, the upper end of the spiral feed frame 32 extends into the inside of the annular storage cavity, the spiral feed frame 32 is used to transport the molten blend in the annular storage cavity downward along the feed trough, a partition 33 is arranged on the outside of the feed trough, the inner side of the partition 33 is in close contact with the surface of the granulation assembly 4, the partition 33 is evenly provided with through holes, and two vertical downward mounting grooves are also provided on the injection frame 31, the two mounting grooves are symmetrically arranged about the feed trough, and the cleaning piece 34 and the scraper 35 are respectively installed in the mounting grooves.

[0048] In the above technical solution, the spiral feed frame 32 is connected to the output shaft of the motor. When the motor is working, the motor drives the spiral feed frame 32 to rotate at a high speed, so that the molten blend inside the annular storage chamber is transported downward along the feed trough. When the copolymer fills the feed trough, the copolymer is evenly extruded outward through the through holes on the partition 33, so that the copolymer can be accurately squeezed into the granulation holes on the surface of the granulation component 4. When the granulation holes continue to rotate after filling, the scraper 35 will scrape the surface of the granulation component 4 to prevent the copolymer from accumulating on the surface of the granulation component 4 and avoid the plastic particles between adjacent granulation holes from sticking together.

[0049] It should be noted that when the granulation hole on the granulation component 4 rotates and enters the inner side of the injection rack 31, the cleaning piece 34 will clean the surface of the granulation component 4, so that impurities that may adhere to the surface of the granulation component 4 will be cleaned, avoiding the accumulation of impurities on the outer surface of the granulation component 4.

[0050] As a preferred embodiment of the present invention, the cleaning piece 34 is a cleaning plate that reciprocates up and down, and bristles are evenly arranged on the inner side of the cleaning plate. When the outer side of the granulation component 4 rotates to the inner side of the injection rack 31, the cleaning plate reciprocates up and down to brush and clean the outer side of the granulation component 4 to prevent plastic impurities from accumulating on the outer side of the granulation component 4.

[0051] As a preferred embodiment of the present invention, the scraper 35 is an arc-shaped scraper made of flexible rubber material. When the copolymer in a molten state is extruded onto the outer surface of the granulation component 4, the copolymer will be squeezed into the granulation hole, but the excess copolymer is still on the outer surface of the granulation component 4. Therefore, when the granulation hole on the granulation component 4 is turned out from the inside of the injection rack 31, the arc-shaped scraper will scrape off the excess copolymer to prevent the copolymer from adhering to the outer surface of the granulation component 4, reduce the waste of plastic raw materials, and prevent the plastic raw materials from accumulating and adhering to the surface of the granulation component 4.

[0052] See also Figure 4 As shown, as a preferred technical solution of this embodiment, a cooling component 40 is also provided on the outer side of the granulation component 4, and the cooling component 40 is slidably arranged up and down at a position between adjacent injection components 3. The cooling component 40 includes a sliding plate 401 slidably arranged on the side wall of the injection component 3 and an arc plate 402 evenly arranged between the two sliding plates 401, and cooling nozzles for cooling the extruded molten blend are evenly arranged on the inner concave surface of the arc plate 402.

[0053] In the above technical solution, after the molten copolymer is transferred out through the granulation hole, the cooling nozzle on the inner side of the arc plate 402 sprays cooling water, and the cooling water moves up and down to form a mist curtain to quickly cool the copolymer, so that the molten copolymer can be quickly cooled and shaped, which is convenient for the accurate preparation of plastic particles.

[0054] See also Figure 7-8 As shown, as the preferred technical solution of this embodiment, the granulation component 4 includes a granulation roller 41, a granulation frame 42, a feeding mechanism 43, a guide frame 44 and an adjusting mechanism 45, which is a cylindrical hollow structure. The granulation roller 41 is installed at the lower end of the driving component 2, and rectangular through grooves are evenly arranged on the outer side of the granulation roller 41. The granulation frame 42 is installed on the outer side of the rectangular through groove. The granulation holes are evenly arranged on the granulation frame 42, and the feeding mechanism 43 is installed on the inner side of the rectangular through groove. The adjusting mechanism 45 is arranged inside the granulation roller 41, and the upper end of the adjusting mechanism 45 is installed on the lower end surface of the storage barrel 1. The guide frame 44 is evenly arranged on the outer side of the adjusting mechanism 45. The inner side of the feeding mechanism 43 is in close contact with the guide frame 44, and the guide frame 44 is used to adjust the depth of the granulation hole and push out the cooled and formed blended material through the feeding mechanism 43.

[0055] In the above technical scheme, the granulation roller 41 drives the granulation frame 42 to move at a constant speed. When the granulation frame 42 moves to the inner side of the injection frame 31, the copolymer in a molten state enters the granulation hole inside the granulation frame 42. When the granulation frame 42 moves out from the inner side of the injection frame 31, the copolymer in a molten state can accurately fill the granulation hole. The cooling element 40 can quickly cool and shape the copolymer in a molten state. Afterwards, through the cooperation between the guide frame 44 and the ejection mechanism 43, the molded plastic particles can be accurately ejected, which is convenient for the subsequent collection of the plastic particles.

[0056] At the same time, the adjustment mechanism 45 can adjust the height of the guide frame 44, and the guide frame 44 can adjust the extension length of the ejection mechanism 43 inside the granulation hole, so that the injection depth inside the granulation hole can be adjusted, which is convenient for processing plastic particles of different sizes.

[0057] It should be noted that when the granulation rack 42 gradually moves toward the inner side of the injection rack 31, at this time, the outer end of the ejection mechanism 43 is in a state flush with the surface of the granulation rack 42, and then the cleaning piece 34 can clean the surface of the granulation rack 42 and the outer end surface of the ejection mechanism 43 to prevent impurities from accumulating; when the granulation rack 42 completely enters the interior of the injection rack 31, the guide rack 44 drives the ejection mechanism 43 to move inward, so that the copolymer in the molten state can enter the interior of the granulation hole; when the granulation rack 42 rotates out from the inner side of the injection rack 31, at this time, the ejection mechanism 43 first remains stationary, and when the copolymer inside the granulation hole is cooled, the ejection mechanism 43 ejects the formed plastic particles.

[0058] See also Figure 8-9 As shown, as the preferred technical solution of this embodiment, the ejection mechanism 43 includes a mounting plate 431, a push plate 432, a ejector rod 433, a connecting spring 434 and a ejector plate 435, the mounting plate 431 is installed on the inner side of the rectangular through groove, circular holes are evenly arranged on the mounting plate 431, ejector rods 433 are slidably arranged in the circular holes, ejector rods 433 are installed on the inner side surface of the ejector rod 433, the inner side surface of the ejector rod 433 is a smooth arc-shaped surface, a connecting spring 434 is arranged on the ejector rod 433, push plates 432 are installed between the outer side surfaces of the ejector rod 433, ejector plates 435 are evenly installed on the push plates 432, and the ejector plates 435 correspond one-to-one to the granulation holes.

[0059] In the above technical scheme, when the granulation rack 42 rotates to enter the interior of the injection rack 31, the push rod 433 and the guide rack 44 cooperate with each other. The initial position of the push rod 433 can be adjusted by adjusting the height of the guide rack 44 up and down, so that the injection depth is adjustable, which is convenient for processing plastic particles of different sizes. After the copolymer on the granulation rack 42 is cooled, the guide rack 44 drives the top plate 435 to be ejected outward through the push rod 433, so that the top plate 435 can eject the molded plastic particles. At this time, the outer side surface of the top plate 435 is flush with the surface of the granulation rack 42. Afterwards, the top plate 435 follows the granulation rack 42 to enter the interior of the injection rack 31 again, so that the cleaning piece 34 cleans the top plate 435 and the surface of the granulation rack 42. When the granulation rack 42 completely enters the inner side of the cleaning piece 34, the guide rack 44 drives the top plate 435 to move inward, so that the top plate 435 can have the effect of pumping the copolymer in the molten state, so that the copolymer can accurately enter the granulation hole.

[0060] See also Figure 10-11 As shown, as a preferred technical solution of this embodiment, the guide frame 44 is in a circular ring structure, and the inside of the guide frame 44 is evenly provided with step grooves 441 and ejection protrusions 442, the step grooves 441 and the ejection protrusions 442 are smoothly connected, the step grooves 441 include a plurality of arc grooves with gradually decreasing depths, and adjacent arc grooves are smoothly connected.

[0061] In the above technical solution, when it is necessary to inject the molten copolymer into the granulation hole, at this time, the inner end of the push rod 433 slides inside the stepped groove 441. At this time, the depth of the granulation hole remains unchanged. After the molten copolymer inside the granulation hole is cooled and formed, the inner side of the push rod 433 moves from the stepped groove 441 to the ejection protrusion 442. The ejection protrusion 442 drives the push rod 433 to eject outward so that the molded plastic particles are pushed out from the inside of the granulation hole, thereby realizing the function of accurately granulating the molten copolymer.

[0062] It should be noted that the stepped groove 441 includes a plurality of arc grooves with gradually decreasing depths. When the guide frame 44 moves upward, the depth of the stepped groove gradually decreases, that is, the outward ejection length of the ejector rod 433 increases, and the injection depth inside the granulation hole can be adjusted. By moving the ejector rod 433 on arc grooves of different depths, the function of granulation processing can be achieved for plastic particles of different sizes.

[0063] See also Fig.10As shown, as the preferred technical solution of this embodiment, the adjustment mechanism 45 includes a fixed frame 451, a connecting plate 452 and a sliding sleeve 453. The number of the fixed frame 451 is multiple, and the fixed frame 451 is a rectangular frame arranged vertically downward. The upper ends of adjacent fixed frames 451 are connected by connecting plates 452, and the connecting plates 452 are connected to the storage barrel 1 by screws. A vertical downward sliding groove is arranged on the outer side of the fixed frame 451, and an electric slider is installed in the sliding groove. The sliding sleeve 453 is sleeved on the outer side of the fixed frame 451, and the fixed frame 451 is connected to the electric slider. The guide frame 44 is installed on the outer side of the sliding sleeve 453.

[0064] In the above technical solution, when it is necessary to reduce the length of the plastic particles, at this time, the sliding sleeve 453 drives the guide frame 44 to move upward, so that the ejection length of the ejector rod 433 is increased, and the injection depth of the injection hole is reduced, so that the length of the molded plastic particles is shorter. When it is necessary to increase the length of the plastic particles, at this time, the sliding sleeve 453 drives the guide frame 44 to move downward, so that the ejection length of the ejector rod 433 is reduced, and the injection depth of the injection hole is increased, so that the length of the molded plastic particles is longer.

[0065] The above description is only by way of illustration of certain exemplary embodiments of the present invention. It is undoubted that those skilled in the art can modify the described embodiments in various ways without departing from the spirit and scope of the present invention. Therefore, the above drawings and descriptions are illustrative in nature and should not be construed as limiting the scope of protection of the claims of the present invention.

Claims

1. A high-strength anti-aging PPO plastic granule, It is characterized in that The invention comprises the following raw materials in parts by weight: 42-48 parts of PPO resin, 32-35 parts of ABS resin, 10-12 parts of PP resin, 3-8 parts of wear-resistant additive, 0.6-1.2 parts of composite anti-aging agent, 0.6-1.2 parts of hexamethylphosphoric triamide, 0.6-0.8 parts of compatibilizer, and 0.4-0.7 parts of reinforcing agent; The composite anti-aging agent is composed of the following raw materials in parts by weight: 13-17 parts of calcium silicate, 11-15 parts of stearic acid, 14-16 parts of unsaturated polyester resin, 8-10 parts of ultraviolet absorber, 11-13 parts of nano zinc oxide, 8-10 parts of polyethylene, 4-8 parts of interface modifier, 12-18 parts of plasticizer, 5-7 parts of dispersing lubricant, and 10-14 parts of nano titanium dioxide; The particle size of the nano titanium dioxide is 20-40 nm.

2. A method for preparing high-strength anti-aging PPO plastic particles, It is characterized in that The following steps are involved: Step S1, under the protection of inert gas, mixing and stirring the required weight of calcium silicate, stearic acid, and unsaturated polyester resin, and then heating to 80-100° C., adding nano zinc oxide and polyethylene while hot, stirring at high speed, adding interface modifier and plasticizer, continuing to heat to 120-140° C., stirring evenly, keeping warm for 15-25 minutes, and then cooling to room temperature, then adding dispersing lubricant, ultraviolet absorber and nano titanium dioxide to the above mixture, reheating to a molten state, keeping warm and stirring at high speed for 20-30 minutes, and then naturally cooling to room temperature to obtain a composite anti-aging agent; Step S2, adding PPO resin, ABS resin, PP resin, wear-resistant additive, composite anti-aging agent, hexamethylphosphoric acid triamide, compatibilizer and reinforcing agent into a high-speed mixer and mixing for 2 minutes, and then standing at 40-50° C. in vacuum for 2-4 hours to obtain a blend; Step S3, transferring the blended material to a granulation module, and the granulation module extrude and granulate the molten blended material to obtain high-strength anti-aging PPO plastic particles.

3. A method for preparing high-strength anti-aging PPO plastic particles according to claim 2, It is characterized in that The inert gas in step S1 is nitrogen or carbon dioxide.

4. A method for preparing high-strength anti-aging PPO plastic particles according to claim 2, Features: The granulation module comprises: The material storage barrel (1) is a cylindrical hollow structure, and an annular material storage cavity is arranged in the middle of the material storage barrel (1); A driving assembly (2) installed inside the storage barrel (1); There are multiple injection assemblies (3), and the injection assemblies (3) are evenly installed on the outer side of the lower end of the storage barrel (1), and the upper end of the injection assemblies (3) is connected to the annular storage cavity inside the storage barrel (1); A granulation component (4) is installed at the lower end of a driving component (2). The granulation component (4) is in a cylindrical structure. Granulation holes with adjustable depths are evenly arranged on the outer surface of the granulation component (4) along its circumference. The inner side surface of the injection component (3) is in close contact with the outer surface of the granulation component (4). The driving component (2) is used to drive the granulation component (4) to rotate at a constant speed. The injection component (3) is configured to extrude a molten blend into the granulation hole and drive the blend in the granulation hole to cool and shape before being ejected to prepare PPO plastic particles.

5. A method for preparing high-strength anti-aging PPO plastic particles according to claim 4, Features: The injection assembly (3) comprises an injection frame (31), a spiral feed frame (32), a partition (33), a cleaning piece (34) and a scraper (35). The injection frame (31) is in a rectangular long strip structure. The injection frame (31) is arranged vertically downward. A feed trough is arranged in the middle of the injection frame (31). A spiral feed frame (32) is installed inside the feed trough. The upper end of the spiral feed frame (32) extends into the inside of the annular storage cavity. The spiral feed frame (32) is used to transport the molten blended material inside the annular storage cavity downward along the feed trough. A partition (33) is arranged outside the feed trough. The inner side surface of the partition (33) is in close contact with the surface of the granulation assembly (4). Through holes are evenly arranged on the partition (33). Two vertical downward mounting grooves are also arranged on the injection frame (31). The two mounting grooves are symmetrically arranged about the feed trough. The cleaning piece (34) and the scraper (35) are respectively installed inside the mounting grooves.

6. A method for preparing high-strength anti-aging PPO plastic particles according to claim 4, Features: The outer side surface of the granulation component (4) is also provided with a cooling component (40), and the cooling component (40) is slidably arranged up and down at a position between adjacent injection components (3). The cooling component (40) includes a sliding plate (401) slidably arranged on the side wall of the injection component (3) and an arc plate (402) evenly arranged between the two sliding plates (401), and cooling nozzles for cooling the extruded molten blend are evenly arranged on the inner concave surface of the arc plate (402).

7. A method for preparing high-strength anti-aging PPO plastic particles according to claim 4, Features: The granulation assembly (4) comprises a granulation roller (41), a granulation frame (42), a material ejection mechanism (43), a guide frame (44) and an adjustment mechanism (45). The granulation roller (41) is a cylindrical hollow structure. The granulation roller (41) is mounted on the lower end of the driving assembly (2). Rectangular through grooves are evenly arranged on the outer surface of the granulation roller (41). The granulation frame (42) is mounted on the outer side of the rectangular through groove. The granulation holes are evenly arranged on the granulation frame (42). The material ejection mechanism (43) is mounted on the inner side of the rectangular through groove. The adjustment mechanism (45) is arranged inside the granulation roller (41). The upper end of the adjustment mechanism (45) is mounted on the lower end surface of the storage barrel (1). The guide frame (44) is evenly arranged on the outer surface of the adjustment mechanism (45). The inner side of the material ejection mechanism (43) is in close contact with the guide frame (44). The guide frame (44) is used to adjust the depth of the granulation holes and push out the blended material after cooling and forming through the material ejection mechanism (43).

8. A method for preparing high-strength anti-aging PPO plastic particles according to claim 7, Features: The ejection mechanism (43) comprises a mounting plate (431), a push plate (432), an ejector rod (433), a connecting spring (434) and an ejector plate (435); the mounting plate (431) is mounted on the inner side of the rectangular through groove; circular holes are evenly arranged on the mounting plate (431); an ejector rod (433) is slidably arranged in the circular hole; an ejector rod (433) is mounted on the inner side surface of the ejector rod (433); the inner side surface of the ejector rod (433) is a smooth arc-shaped surface; a connecting spring (434) is arranged on the ejector rod (433); a push plate (432) is mounted between the outer side surfaces of the ejector rod (433); an ejector plate (435) is evenly mounted on the push plate (432); and the ejector plates (435) correspond to the granulation holes one by one.

9. The method for preparing high-strength anti-aging PPO plastic particles according to claim 7, Features: The guide frame (44) is in a circular ring structure, and the guide frame (44) is evenly provided with stepped grooves and ejection protrusions inside, and the stepped grooves and the ejection protrusions are smoothly connected. The stepped grooves include a plurality of arc grooves with gradually decreasing depths, and adjacent arc grooves are smoothly connected.

10. The method for preparing high-strength anti-aging PPO plastic particles according to claim 7, Features: The adjusting mechanism (45) comprises a fixing frame (451), a connecting plate (452) and a sliding sleeve (453). The fixing frames (451) are provided in plurality. The fixing frames (451) are rectangular frames arranged vertically downward. The upper ends of adjacent fixing frames (451) are connected by connecting plates (452). The connecting plates (452) are connected to the storage barrel (1) by screws. A vertical downward sliding groove is arranged on the outer side of the fixing frame (451). An electric slider is installed in the sliding groove. The sliding sleeve (453) is sleeved on the outer side of the fixing frame (451). The fixing frame (451) is connected to the electric slider. The guide frame (44) is installed on the outer side of the sliding sleeve (453).

Citation Information

Patent Citations

  • Modified PPO (Poly Phenylene Oxide) plastic alloy and preparation method thereof

    CN103525070A

  • Method for preparing ultraviolet-resistant aging-resistant plastic additive

    CN109422946A

  • Medical waste plastic recycling treatment technology

    CN111590780A