High-fluidity PA / PP composite material and application thereof
By using ester or amide flow modifiers generated by esterification or amidation reaction in PA/PP composite materials, the problem of insufficient processing fluidity and pad printing performance of PA materials in the prior art is solved, and high PP is achieved The significant fluidity and impact strength under the content meet the high filling flow modification needs of composite materials.
Patent Information
- Application Number
- CN202411402609.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-10-09
AI Technical Summary
In the prior art, in order to improve the low cost and mechanical properties of polyamide (PA) materials, it is often necessary to add reinforcement fillers or thermally conductive fillers, resulting in a decrease in processing fluidity, and the existing flow modifiers have limited modification effects on other materials. , it is difficult to meet the pad printing performance requirements under high PP addition amount.
采用R1-COOH与R2-(OH)m或(NH2)n-R2-(OH)m发生酯化或酰胺化反应产生的酯类或酰胺类流动改性剂,例如N-羟甲基硬脂 酰胺、硬脂酰胺MEA、硬脂酰胺DEA、乙二醇硬脂酸酯、单硬脂酸甘油酯等,作为PA/PP复合材料中的流动改性剂,提高材料的加工流动性和移印 Effect.
The processing fluidity and pad printing performance of PA/PP composite materials have been significantly improved. Especially under high PP content, the fluidity and impact strength of the material have been significantly improved, and the shear viscosity has been reduced, meeting the flow modification needs of high-filling materials.
Smart Images

Figure CN118909433A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer compositions, and in particular relates to a high-fluidity PA / PP composite material and an application thereof. Background Art
[0002] In recent years, with the increasing application of polyamide (PA) engineering plastics, higher requirements have been put forward for its modification, such as low cost, good mechanical properties, good processing fluidity, etc. In order to achieve low cost in the existing technology, on the one hand, a resin with lower cost will be selected instead, but it is often necessary to add more reinforcing fillers to maintain high mechanical properties or increase the thermal conductivity of the material. However, the more reinforcing fillers or thermal conductive fillers are added, the worse the processing fluidity of the material. Usually, the addition of flow modifiers is selected to improve the processing fluidity of the material. AF-21 is a super flow modifier specially developed for nylon. It is widely used to improve the fluidity of polyamide, but the choice is relatively single. The modification effect of other lubricants with partial flow modification function is relatively poor; or alloys (such as polypropylene, PP) are selected to improve the processing fluidity of alloy materials. However, the alloy may bring other problems (such as compatibility) due to the introduction of alloy resins. The situation is more complicated, and it is necessary to repeatedly proof whether the performance meets the indicators and eliminate other problems caused by the introduction of new resins. In addition, in some special needs (such as the addition of more PP, which will cause the pad printing performance of the product to deteriorate), the addition of PP is restricted and cannot meet the needs. Summary of the invention
[0003] In order to overcome the above-mentioned problems existing in the prior art, the object of the present invention is to provide a new formulation system to further improve the processing fluidity of PA / PP, which is specifically achieved through the following technical solutions: A high-fluidity PA / PP composite material, comprising the following components in parts by weight: PA 20-60 parts PP 1~20 pieces Functional filler 20~70 parts Flow modifier 0.5-2 parts Other additives 0-5 parts The PA is one or both of PA6 and PA66, and the functional filler is one or both of reinforcing filler and thermal conductive filler. The flow modifier is: R 1 -COOH and R 2 -(OH)m or (NH 2 )nR 2 -(OH)m undergoes esterification or amidation to produce esters or amides, wherein R 1 is a C15~C19 alkyl group, R2 is a C1-C6 alkyl group, m is an integer of 1 to 3, and n is an integer of 0 to 3.
[0004] About R 1 -COOH can be represented by a long-chain carbon substance with a carboxyl terminal, such as stearic acid; (NH 2 )nR 2 -(OH)m can be represented by a substance containing a terminal amino group and connected to one or more hydroxyl groups through an alkyl chain, including the case where a hydroxyl group also exists in the alkyl group of R2. For example, when n is 0, glycerol can be esterified with R1-COOH to obtain glycerol ester.
[0005] Optionally, the following components are included by weight: PA 30-50 parts PP 2-15 parts Thermally conductive filler 10-45 parts Reinforced filler 10-40 parts Compatibilizer 0-10 parts Other additives 0-5 parts Flow modifier 0.5-2 parts, The sum of the weight parts of the thermal conductive filler and the reinforcing filler is 20 to 65 parts.
[0006] Optionally, in the flow modifier, R1 is a C17 alkyl group.
[0007] Optionally, the flow modifier includes one or more of N-hydroxymethyl stearamide, stearamide MEA, stearamide DEA, ethylene glycol stearate, diethylene glycol monostearate, and glyceryl monostearate.
[0008] N-Hydroxymethyl stearamide CAS: 3370-35-2, the structural formula is as follows:
[0009] Stearamide MEA CAS: 111-57-9, the structural formula is as follows:
[0010] Stearamide DEA CAS: 93-82-3, the structural formula is as follows:
[0011] Ethylene glycol stearate CAS: 111-60-4, the structural formula is as follows:
[0012] Glyceryl monostearate CAS: 123-94-4, the structural formula is as follows:
[0013] Optionally, the thermally conductive filler includes one or more of magnesium hydroxide, calcium carbonate, magnesium oxide, aluminum oxide, aluminum nitride, boron nitride, silicon carbide, molybdenum disulfide, zinc sulfide, wollastonite, and talc.
[0014] Optionally, the reinforcing filler includes one or more of glass fiber, carbon fiber, and mineral powder.
[0015] Optionally, the other additives include one or more of an antioxidant, a lubricant, and a toner.
[0016] Optionally, the compatibilizer includes one or more of EPDM grafted maleic anhydride copolymer, polypropylene grafted maleic anhydride copolymer, and POE grafted maleic anhydride copolymer.
[0017] The present application also provides an application of the composite material according to the aforementioned solution, which is applied to a lamp housing of a thin-walled product with a wall thickness of less than 1.0 mm.
[0018] The present application also provides an application of a flow modifier for improving the processing flow properties of PA / PP composite materials, wherein the flow modifier is an ester or amide product produced by an esterification or amidation reaction of R1-COOH with R2-(OH)m or (NH2)n-R2-(OH)m, wherein R1 is an alkyl group of C15~C19, R2 is an alkyl group of C1-C6, m is an integer of 1~3, and n is an integer of 0~3.
[0019] Optionally, in the flow modifier, R1 is a C17 alkyl group.
[0020] Optionally, the flow modifier includes one or more of N-hydroxymethyl stearamide, stearamide MEA, stearamide DEA, ethylene glycol stearate, diethylene glycol monostearate, and glyceryl monostearate.
[0021] Compared with the prior art, the present invention unexpectedly discovered a class of flow modifiers that can greatly improve the processing flow properties of PA / PP. For example, the substances contained therein, such as stearamide MEA, stearamide DEA, ethylene glycol stearate, diethylene glycol monostearate, glyceryl monostearate, etc., are generally used as antistatic agents, lubricants, etc. in the prior art, and their special flowability improvement characteristics have not been found. In other words, the present application overcomes the technical prejudice in the prior art that it can only be used as an antistatic agent and a lubricant. In addition, the present application scheme can greatly improve the pad printing effect of the material at a higher PP content, and also has unexpected technical effects. The applicant believes that the possible principle is: when PP is present, R 1 -COOH R 1The long-chain carbon at the end tends to be in closer contact with PP, and the ester group or amide group and the additional hydroxyl group generated by the reaction tend to be in closer contact with polyamide, destroying and replacing the hydrogen bonding force between different molecular chains of polyamide, on the one hand, improving the fluidity of polyamide, on the other hand, through R 1 The binding force with PP can better embed PP into the molecular chains of polyamide, thereby enhancing the flow modification effect of PP on polyamide. Compared with other similar structures such as EBS, PETS, etc., none of them show the same level of flow modification effect as the scheme of this application. This application provides a flow modifier for PA / PP composite materials. The effect of the flow modifier used is difficult to predict, especially for highly filled materials, and a high-quality flow modifier is provided, which is a significant improvement. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a shear viscosity curve diagram of Examples 1-3 and Comparative Examples 1-3 at 270°C. DETAILED DESCRIPTION
[0023] The specific implementation methods of the present application are described in detail below through examples, but the specific implementation of the present application does not serve as a limitation on the technical solution of the present application. Any non-substantial changes such as replacing common technical solutions in the field with the technical solutions described in the examples of the present application are within the scope of protection of the present application.
[0024] It should be noted that: Introduction to the raw materials or specific substances used in each embodiment of this application: PA66: Wenzhou Huafeng Group, EP1107; PA6: Guangdong Xinhui Meida Acrylic Fiber Co., Ltd., M2000; PP: Yongjia rare 1450T; Fiberglass: Jushi Group Co., Ltd., ECS10-4 .5-560A; Calcium carbonate: Jiangxi Yongfa Chemical Co., Ltd.; Antioxidant: Antioxidant 1098; EBS (ethylene bisstearamide): Guangzhou Fenghua Chemical Technology Co., Ltd.; Ethylene glycol stearate CAS:111-60-4; Glyceryl monostearate CAS: 123-94-4; Stearic acid ethoxyamide CAS: 93-82-3; AF-21, Guangzhou Hecheng Industrial Co., Ltd.; PETS (Pentaerythritol Stearate) CAS: 115-83-3, Jiangsu Haian Petrochemical.
[0025] The material preparation methods of the embodiments and comparative examples are as follows: The melt blending and extrusion process is adopted for production. The raw material components except glass fiber are mixed and added into a twin-screw extruder through a main feed port. Glass fiber (if any) is added from a side feeder. After melt blending, the materials are extruded, cooled, air-dried and granulated to obtain the materials of each embodiment and comparative example.
[0026] Sample injection molding process: Add the materials of each embodiment and comparative example into an injection molding machine, set the injection molding temperature at 250-280 degrees Celsius, and inject each test sample according to the requirements of each test method.
[0027] The performance test method is as follows: Notched impact strength: tested according to ISO179-1 standard (23°C, 1J); Unnotched impact strength: tested according to ISO179-1 standard (23°C, 4J); Pad printing effect: Use a dyne pen to scratch the surface of the sample, observe the dispersion of the dyne pen solution on the sample surface with the naked eye, evaluate the surface tension and thus reflect the pad printing effect. The grades are divided into 1 to 5, with 1 being the lowest (almost no effect) and 5 being the highest (clear effect). The dyne pen can quickly and intuitively detect whether the material is suitable for printing (including pad printing); Processing fluidity: 1) ISO 1133 measures the melt index (270 ℃ 2.16kg) to evaluate the processing fluidity of the material; 2) GB / T25278-2010 (270℃) measures the shear viscosity to evaluate the processing fluidity of the material. Under the same shear rate conditions, the lower the shear viscosity, the better the actual processing fluidity.
[0028] The formulations and performance data of the embodiments and comparative examples are shown in Tables 1 to 3.
[0029] Table 1 is the formula (weight parts) and performance data of Examples 1 to 3 and Comparative Examples 1 to 3
[0030] Table 2 is the formula (weight parts) and performance data of Examples 4, 5 and Comparative Examples 4 to 9
[0031] Table 3 is the formula (weight parts) and performance data of Examples 6 to 12
[0032] From the data in Table 1, Table 2 and Table 3, we can see that: By comparing Comparative Example 1 with Example 2, the applicant unexpectedly found that compared with the blank control group, the ethylene glycol stearate of the present application improved the notched impact strength of the simply supported beam, the unnotched impact strength of the simply supported beam, and the melt index performance by 79%, 29%, and 48%, respectively. The substantial improvement of various indicators is an unexpected technical effect and a significant improvement.
[0033] By comparing Comparative Examples 2 and 3 with Examples 1 and 2: On the one hand, AF-21 (AF-21 is a super flow modifier specially developed for nylon, the main component of which is adipic acid), which is often used as a flow modifier in polyamide, has a far less effect on improving the flow of the material than adding the ethylene glycol stearate described in this application. On the other hand, the simply supported beam notched impact strength and simply supported beam unnotched impact strength of the material are also greatly improved. Specifically, when 0.5 parts are added, the simply supported beam notched impact strength, simply supported beam unnotched impact strength and melt index performance are increased by 51%, 38% and 4% respectively. When 1 part is added, the simply supported beam notched impact strength, simply supported beam unnotched impact strength and melt index performance are increased by 74%, 24% and 36% respectively. Unexpected results have been achieved, and there is also significant progress.
[0034] Comparison of Example 2 with Comparative Examples 6 and 7: Compared with 1 part of PETS, the addition of 1 part of ethylene glycol stearate increases the melt index by 35%, and compared with 1 part of EBS, the notched impact strength of the simply supported beam, the unnotched impact strength of the simply supported beam and the melt index performance increase by 59%, 13% and 60% respectively. It has unexpected technical effects. In particular, the substantial improvement in the melt index is a significant improvement.
[0035] Comparison of Example 6 with Comparative Examples 8 and 9: The resin is PA66, and 1 part of ethylene glycol stearate is added. Compared with the blank control, the notched impact strength, unnotched impact strength and melt index performance of the simple supported beam are increased by 51%, 17% and 26% respectively. Compared with 1 part of AF-21, the notched impact strength, unnotched impact strength and melt index performance of the simple supported beam are increased by 43%, 21% and 39% respectively. It has unexpected technical effects. Especially compared with the commonly used flow modifier AF-21, it has significant improvement.
[0036] Compared with Comparative Examples 1 and 3, Examples 7 and 8 show that stearic acid ethoxyamide and glyceryl monostearate can also achieve the same technical effect as ethylene glycol stearate. Compared with the blank control and the addition of flow modifier AF-21, the notched impact strength, unnotched impact strength and melt index of the simple supported beam are greatly improved, which is a significant improvement.
[0037] It can be seen from the data in Tables 1 to 3 that the pad printing performance of the PA / PP alloy material can be greatly improved by adding ethylene glycol stearate, stearic acid ethoxyamide and glyceryl monostearate of the present application.
[0038] Table 4 Shear viscosity performance test data of Examples 1, 2, 3 and Comparative Examples 1, 2, 3
[0039] Table 4 shows the shear viscosity performance test data of Examples 1, 2, 3 and Comparative Examples 1, 2, 3. Figure 1 is a curve chart based on the data in Table 4. Figure 1 As shown, compared with comparative examples 1, 2, 3, the shear viscosity curves of Examples 1, 2, 3 are lower than those of the comparative examples, especially Examples 2 and 3, which are significantly lower than those of the comparative examples 1, 2, 3, indicating that the processing fluidity of the formula with the addition of ethylene glycol stearate is better than that of the blank and AF-21, and has an unexpected technical effect.
[0040] It should be noted that the above contents described in this specification are merely examples of the technical solution of the present invention. Any simple changes or equivalent changes made based on the features and principles described in the patent concept of the present invention are included in the protection scope of the patent of the present invention.
Claims
1. A high-fluidity PA / PP composite material, characterized in that: By weight, it includes the following components: PA 20-60 parts PP 1~20 pieces Functional filler 20~70 parts Flow modifier 0.5-2 parts Other additives 0-5 parts The PA is one or both of PA6 and PA66, and the functional filler is one or both of reinforcing filler and thermal conductive filler. The flow modifier is: R 1 -COOH and R 2 -(OH) m or (NH2) n -R 2 -(OH) m The ester or amide product produced by esterification or amidation reaction, wherein R 1 is a C15~C19 alkyl group, R 2 is a C1-C6 alkyl group, m is an integer of 1 to 3, and n is an integer of 0 to 3.
2. The composite material according to claim 1, characterized in that By weight, it includes the following components: PA 30-50 parts PP 2-15 parts Thermally conductive filler 10-45 parts Reinforced filler 10-40 parts Compatibilizer 0-10 parts Other additives 0-5 parts Flow modifier 0.5-2 parts, The sum of the weight parts of the thermal conductive filler and the reinforcing filler is 20 to 65 parts.
3. The composite material according to claim 1 or 2, characterized in that: The flow improver, R 1 It is a C17 alkyl group.
4. The composite material according to claim 1 or 2, characterized in that: The flow modifier includes one or more of N-hydroxymethyl stearamide, stearamide MEA, stearamide DEA, ethylene glycol stearate, diethylene glycol monostearate, and glyceryl monostearate.
5. The composite material according to claim 1 or 2, characterized in that: The thermal conductive filler includes one or more of magnesium hydroxide, calcium carbonate, magnesium oxide, aluminum oxide, aluminum nitride, boron nitride, silicon carbide, molybdenum disulfide, zinc sulfide, wollastonite, and talc.
6. The composite material according to claim 1 or 2, characterized in that: The reinforcing filler includes one or more of glass fiber, carbon fiber and mineral powder.
7. The composite material according to claim 1 or 2, characterized in that: The other auxiliary agents include one or more of antioxidants, lubricants and toners.
8. The composite material according to claim 2, characterized in that The compatibilizer includes one or more of EPDM grafted maleic anhydride copolymer, polypropylene grafted maleic anhydride copolymer, and POE grafted maleic anhydride copolymer.
9. Use of the composite material according to any one of claims 1 to 8, characterized in that: Applied to thin-walled lamp housings with a wall thickness of less than 1.0 mm.
10. A flow modifier for improving the processing flow properties of PA / PP composite materials, characterized in that: The flow improver is R 1 -COOH and R 2 -(OH) m or (NH2) n -R 2 -(OH) m The ester or amide product produced by esterification or amidation reaction, wherein R 1 is a C15~C19 alkyl group, R 2 is a C1-C6 alkyl group, m is an integer of 1 to 3, and n is an integer of 0 to 3.
11. The use according to claim 10, characterized in that: The flow modifier includes one or more of N-hydroxymethyl stearamide, stearamide MEA, stearamide DEA, ethylene glycol stearate, diethylene glycol monostearate, and glyceryl monostearate.
Citation Information
Patent Citations
High-filling heat-conducting PA6 / PP composite material with good glue adhesion and application thereof
CN112708266A
High-fluidity high-impact halogen-free flame-retardant polypropylene material and preparation method and application thereof
CN112724580A
Polyamide composition as well as preparation method and application thereof
CN113683883A
High-fluidity halogen-free flame-retardant heat-conducting nylon composite material as well as preparation method and application thereof
CN117820849A
Polyamide composite resin composition for fuel filler pipe
US20160362553A1