Joint sealing material for high plateau airport runway and preparation method of joint sealing material

By introducing photoinitiators and ethyl vinyl sulfide into the high plateau airport runway filler, the photopolymerization reaction of polysulfide gel is promoted, and the solidification product containing sulfide bonds is generated, which solves the problem of polysulfide filler in the high cold. The low curing rate and performance attenuation problems in strong ultraviolet environments have achieved better bonding and mechanical properties, meeting the construction requirements under high cold conditions.

CN118909439AActive Publication Date: 2024-11-08SOUTHWEST DESIGN & RES INST OF CIVIL AVIATION AIRPORT CONSTR GRP CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410973421.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

Under the special climatic conditions of high plateau airports, polysulfur caulks are prone to aging and decomposing under strong ultraviolet radiation environments, resulting in a decrease in mechanical properties and insufficient curing, which affects the construction quality and service life.

Method used

A caulking material including base paste and sulfide paste is used. The base paste consists of liquid polysulfide gel, ethyl vinyl sulfide and auxiliary materials. The sulfide paste contains manganese dioxide, photoinitiator and auxiliary materials, and passes through photoinitiator. Initiate the photopolymerization reaction of polysulfide gel and ethyl vinyl sulfide to form a cured product containing sulfide bonds, enhancing adhesion and mechanical properties.

Benefits of technology

In the high day-night temperature difference and strong ultraviolet ray environment at high plateau airports, the curing rate of the caulk material is improved, the bonding and mechanical properties are not easy to attenuate, meeting the requirements of continuous navigation construction, extending service life, and reducing maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909439A_ABST
    Figure CN118909439A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of runway joint sealing materials, and discloses a joint sealing material for high plateau airport runways and a preparation method thereof.The joint sealing material comprises base paste and vulcanization paste, and the base paste comprises liquid polysulfide raw rubber, ethyl vinyl sulfide and an auxiliary material A; the vulcanizing paste comprises manganese dioxide, a photoinitiator and an auxiliary material B; the airfield runway joint sealing material provided by the invention can effectively solve the problems that a polysulfide joint sealing material is low in curing rate and poor in performance after curing caused by large day and night temperature difference of a high plateau airport, the performance is easy to attenuate caused by ultraviolet radiation of the high plateau and the like, the curing rate can meet the requirement of non-stop construction, and the airfield runway joint sealing material has a wide market application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of runway joint filling materials, in particular to a joint filling material for a high-altitude airport runway and a preparation method thereof. Background Art

[0002] Civil airport runways are civil aviation professional projects and are runways dedicated to aircraft takeoff and landing. For the cement concrete pavement in the flight area, the shrinkage joints and the upper joints of the closed expansion joints need to be filled with caulking materials to prevent the infiltration of aviation fuel, moisture, and debris on the runway. Otherwise, hard debris falling into the caulking will cause the corners of the cement concrete slab to break, the infiltrated moisture will reduce the stability of the base layer, and the aviation kerosene leaked from the aircraft will penetrate and cause environmental pollution. Runway caulking materials play an important role, and the special climatic conditions of high-altitude airports also place higher demands on the performance of runway caulking materials. If the selection of caulking materials and the construction process are rigorous during the caulking material construction process, the strength of the pavement can be maintained and the service life of the pavement can be extended, thereby ensuring the safe operation of the airport runway.

[0003] At present, the commonly used materials for airport runway caulking are polysulfide and polyurethane. Among them, polysulfide is also used for the sealing of aircraft fuel tanks. It has excellent resistance to aviation kerosene and can effectively prevent the leakage of aviation kerosene on the airport runway from penetrating and polluting.

[0004] Polysulfide caulking materials are usually two-component for easy construction. They need to be mixed at room temperature and then cured. The curing time is greatly affected by temperature. Within a certain range, the higher the temperature, the faster the curing rate, the better the caulking bonding effect and durability; when the temperature is below 5°C, the curing is insufficient, which can easily cause a significant decrease in bonding and mechanical properties, and caulking is not suitable.

[0005] High plateau airports (airport altitude is above 2,438 meters) have special environments such as high altitude, low air pressure, low oxygen content, low humidity, strong ultraviolet radiation, long sunshine hours, and large temperature difference between day and night. Compared with general airports, they are much more complicated.

[0006] On the one hand, if the polysulfide caulking material used for general airport runways is applied to high-altitude airports, the construction time and construction quality are difficult to control. In the actual construction experience of high-altitude airport runway caulking materials, the curing and maintenance of polysulfide glue is greatly affected by the weather. The temperature difference between day and night in high-altitude areas is large, and the bonding effect after curing is unstable during the curing time. It is even easy to have insufficient curing, resulting in poor caulking effect, shortened service life, high replacement frequency, etc., which increases maintenance costs, which will have a great impact on the construction process and project quality assurance.

[0007] On the other hand, due to the presence of disulfide bonds in the molecular structure of ordinary polysulfide adhesive (R-SS-R'), it is prone to aging and decomposition under the strong ultraviolet radiation environment of high-altitude airports, causing the adhesion to decay and debond, and the mechanical properties to decrease.

[0008] In summary, the special climatic conditions of high-altitude airports are not suitable for the use of polysulfide fillers for general airport runways. The polysulfide fillers need to be modified and optimized according to the characteristics of the service environment. Summary of the invention

[0009] Technical problems solved by the present invention:

[0010] It is used to solve the problem that the polysulfide filler currently used in general airport runways is easily aged and decomposed in a strong ultraviolet radiation environment, resulting in a decrease in mechanical properties.

[0011] The technical solution adopted by the present invention is:

[0012] In view of the above technical problems, the purpose of the present invention is to provide a high-altitude airport runway filler and a preparation method thereof. The specific contents are as follows:

[0013] A seam filler for a high-altitude airport runway comprises a base paste and a vulcanizing paste. The base paste comprises liquid polysulfide rubber, ethyl vinyl sulfide and auxiliary material A; the vulcanizing paste comprises manganese dioxide, a photoinitiator and auxiliary material B.

[0014] According to some optional embodiments, auxiliary material A includes active nano calcium carbonate, light calcium carbonate, fumed silica, magnesium stearate, dioctyl terephthalate, and vinyl triethoxysilane.

[0015] According to some optional embodiments, the components of the base paste, measured by weight, include 98-100 parts of liquid polysulfide rubber, 8-9 parts of ethyl vinyl sulfide, 28-30 parts of active nano calcium carbonate, 4-5 parts of light calcium carbonate, 1-2 parts of fumed silica, 0.5-1 part of magnesium stearate, 8-9 parts of dioctyl terephthalate, and 0.1-0.5 parts of vinyl triethoxy silane.

[0016] According to some optional embodiments, the components of the base paste, measured by weight, include 100 parts of liquid polysulfide rubber, 8 parts of ethyl vinyl sulfide, 30 parts of active nano calcium carbonate, 5 parts of light calcium carbonate, 1 part of fumed silica, 1 part of magnesium stearate, 8.5 parts of dioctyl terephthalate, and 0.45 parts of vinyl triethoxysilane.

[0017] According to some optional embodiments, the photoinitiator is Irgacure 2959.

[0018] According to some optional embodiments, auxiliary material B includes dioctyl terephthalate, 1,3-biphenylguanidine, carbon black, epoxy resin, and sulfur.

[0019] According to some optional embodiments, the components of the vulcanizing paste include, by weight, 90 parts of manganese dioxide, 0.1-0.2 parts of photoinitiator, 8-10 parts of dioctyl terephthalate, 5-7 parts of 1,3-biphenylguanidine, 8-10 parts of carbon black, 8-10 parts of epoxy resin, and 0.1-0.3 parts of sulfur.

[0020] According to some optional embodiments, the components of the vulcanizing paste are, by weight, 90 parts of manganese dioxide, 0.2 parts of photoinitiator, 9 parts of dioctyl terephthalate, 7 parts of 1,3-biphenylguanidine, 9 parts of carbon black, 9 parts of epoxy resin, and 0.25 parts of sulfur.

[0021] According to some optional embodiments, the liquid polysulfide rubber is obtained by mixing liquid polysulfide rubbers with weight average molecular weights of 2000 and 4500 in a mass ratio of 3-5:5-7. A further preferred ratio is 4:6.

[0022] According to some optional embodiments, the mass ratio of the base paste to the vulcanizing paste is 100:8-10, more preferably 100:8.5-9, and even more preferably 100:9.

[0023] Second, the present invention provides a method for preparing the aforementioned high plateau airport runway filler, comprising the following steps:

[0024] Weigh each component of the base paste, and blend them (a planetary mixer may be selected as the blending equipment) to obtain the base paste;

[0025] Weigh each component of the vulcanized paste, grind it (a three-roll grinder can be selected as the grinding equipment) to obtain the vulcanized paste;

[0026] The base paste and the vulcanized paste are mixed to obtain a joint filler for high-altitude airport runways.

[0027] The technical mechanism adopted by the present invention and the beneficial effects achieved are:

[0028] The high plateau airport runway caulking material provided by the present invention utilizes polysulfide raw rubber to generate a cured product containing a disulfide bond (R-SS-R') under the action of a manganese dioxide oxidant, and at the same time, polysulfide raw rubber and ethyl vinyl sulfide are photopolymerized and cured under a high plateau strong ultraviolet environment and a photoinitiator to generate a cured product containing a thioether bond (-CS-), as a supplement to the oxidative curing of the polysulfide caulking material; after the thioether bond (-CS-) is introduced into the cured product, the bonding performance and mechanical properties are more excellent, and the bonding performance and mechanical properties are not easy to decay under a strong ultraviolet service environment. The airport runway caulking material provided by the present invention can effectively solve the problems of low curing rate of polysulfide caulking material caused by large temperature difference between day and night at high plateau airports, poor performance after curing, and easy attenuation of performance due to ultraviolet radiation from high plateaus, and the curing rate can meet the requirements of non-stop construction, and has broad market application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a physical picture of the adhesion test results of the caulking material prepared in Example 1;

[0030] Figure 2 This is a physical picture of the adhesion test results of the caulking material prepared in Comparative Example 3. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0032] <Example>

[0033] Example 1

[0034] This embodiment provides a method for preparing a seam filler for a high-altitude airport runway, comprising the following steps:

[0035] Take 100g of liquid polysulfide rubber (liquid polysulfide rubbers with weight-average molecular weights of 2000 and 4500 are mixed in a mass ratio of 4:6), 8g of ethyl vinyl sulfide, 30g of active nano-calcium carbonate, 5g of light calcium carbonate, 1g of fumed silica, 1g of magnesium stearate, 8.5g of dioctyl terephthalate, and 0.45g of vinyl triethoxysilane, grind them on a three-roll grinder for 10 minutes to prepare a base paste; take 90g of manganese dioxide, 0.2g of Irgacure 2959, 9g of dioctyl terephthalate, 7g of 1,3-biphenylguanidine, 9g of carbon black, 9g of epoxy resin, and 0.25g of sulfur, grind them on a three-roll grinder for 10 minutes to prepare a vulcanizing paste to obtain a two-component material. When used, mix and stir the two components to obtain a sealant 1.

[0036] <Comparative Example>

[0037] Comparative Example 1

[0038] This comparative example provides a method for preparing a seam filler for a high-altitude airport runway, comprising the following steps:

[0039] Take 100g of liquid polysulfide rubber (liquid polysulfide rubbers with weight-average molecular weights of 2000 and 4500 are mixed in a mass ratio of 4:6), 6g of ethyl vinyl sulfide, 30g of active nano-calcium carbonate, 5g of light calcium carbonate, 1g of fumed silica, 1g of magnesium stearate, 8.5g of dioctyl terephthalate, and 0.45g of vinyl triethoxysilane, grind them on a three-roll grinder for 10 minutes to prepare a base paste; take 90g of manganese dioxide, 0.15g of Irgacure 2959, 9g of dioctyl terephthalate, 7g of 1,3-biphenylguanidine, 9g of carbon black, 9g of epoxy resin, and 0.25g of sulfur, grind them on a three-roll grinder for 10 minutes to prepare a vulcanizing paste to obtain a two-component material. When used, the two components are mixed and stirred evenly to obtain a sealant 2.

[0040] Comparative Example 2

[0041] This comparative example provides a method for preparing a seam filler for a high-altitude airport runway, comprising the following steps:

[0042] Take 100g of liquid polysulfide rubber (liquid polysulfide rubbers with weight-average molecular weights of 2000 and 4500 are mixed in a mass ratio of 4:6), 10g of ethyl vinyl sulfide, 30g of active nano-calcium carbonate, 5g of light calcium carbonate, 1g of fumed silica, 1g of magnesium stearate, 8.5g of dioctyl terephthalate, and 0.45g of vinyl triethoxysilane, grind them on a three-roll grinder for 10 minutes to prepare a base paste; take 90g of manganese dioxide, 0.25g of Irgacure 2959, 9g of dioctyl terephthalate, 7g of 1,3-biphenylguanidine, 9g of carbon black, 9g of epoxy resin, and 0.25g of sulfur, grind them on a three-roll grinder for 5 minutes to prepare a vulcanizing paste to obtain a two-component joint filler. When used, mix and stir the two components to obtain joint filler 3.

[0043] Comparative Example 3

[0044] This comparative example provides a method for preparing a seam filler for a high-altitude airport runway, comprising the following steps:

[0045] Take 100g of liquid polysulfide rubber (liquid polysulfide rubbers with weight-average molecular weights of 2000 and 4500 are mixed in a mass ratio of 4:6), 30g of active nano-calcium carbonate, 5g of light calcium carbonate, 1g of fumed silica, 1g of magnesium stearate, 8.5g of dioctyl terephthalate, and 0.45g of vinyl triethoxysilane, and grind them on a three-roll grinder for 10 minutes to prepare a base paste; take 100g of manganese dioxide, 10g of dioctyl terephthalate, 8g of 1,3-biphenylguanidine, 10g of carbon black, 10g of epoxy resin, and 0.3g of sulfur, and grind them on a three-roll grinder for 5 minutes to prepare a vulcanizing paste to obtain a two-component sealant. When using, mix and stir the two components to obtain sealant 4.

[0046] <Test example>

[0047] Curing performance test

[0048] According to the requirements of civil aviation standard MH 5006 "Technical Specification for Construction of Cement Concrete Surface Layers for Civil Airports", in accordance with standards GB / T 13477.17 "Test Methods for Building Sealing Materials Part 17: Determination of Elastic Recovery Rate", GB / T 13477.13 "Test Methods for Building Sealing Materials Part 13: Determination of Adhesion after Cold Drawing-Hot Pressing" (cold area: elongation +40% at -30±2°C; compression -12.5% ​​at 40±2°C), GB / T 13477.5 "Test Methods for Building Sealing Materials Part 5: Determination of Surface Dry Time", ASTM D2240 "Standard Test Methods for Rubber Properties - Durometer Hardness", the concrete standard specimens prepared in Example 1 and Comparative Examples 1-3 were tested respectively under a low-temperature ultraviolet radiation environment (taking the average daily ultraviolet light intensity of a high plateau airport as 55 W·m -2 , using a radiation intensity of 0.034 W·m -2 The UVA340 ultraviolet lamp was used to irradiate the surface of the test specimen, and the ultraviolet intensity was adjusted to 55W·m -2 , placed in a low-temperature chamber at 3°C ​​to simulate the high-altitude airport's high-cold and strong ultraviolet construction environment) surface drying time, hardness after 7 days of curing, and hardness, elastic recovery rate, tensile modulus, and elongation at break after 28 days of curing. The test results are shown in Table 1.

[0049] Table 1 Test results of curing performance of joint filler

[0050]

[0051] Anti-ultraviolet aging performance test

[0052] Take 350MJ·m -2 The annual total ultraviolet radiation intensity of the high plateau airport is 0.034Mw·m -2 The UVA340 ultraviolet lamp is 50mm away from the sample for artificial accelerated ultraviolet aging, and the distance between the lamps is 70mm. According to the principle of equivalent indoor and outdoor ultraviolet radiation intensity, the two-year outdoor ultraviolet radiation time is converted into 576 hours (24 days) of radiation time in the indoor ultraviolet aging box by calculation.

[0053] According to the requirements of the civil aviation standard MH 5006 Technical Specifications for Construction of Cement Concrete Surface Layers at Civil Airports, and in accordance with the standards GB / T 13477.17, GB / T 13477.13, ASTM D2377, and ASTM D2240, the hardness, elastic recovery rate, tensile modulus, elongation at break, and adhesion of the concrete specimens of the present invention and the comparative example were tested before and after accelerated aging for 576 hours in the above-mentioned UV aging box (placed in a low-temperature chamber at 3°C). The test results are shown in Table 1. The actual picture of the adhesion test is shown in Figure 1 (Example 1) and Figure 2 (Comparative Example 3).

[0054] Table 2 Anti-ultraviolet aging performance of joint fillers

[0055]

[0056] From the formula point of view, Example 1, Comparative Example 1 and Comparative Example 2 introduce ethyl vinyl sulfide and photoinitiator Irgacure 2959 compared with Comparative Example 3. Ethyl vinyl sulfide and polysulfide rubber undergo photopolymerization reaction under the action of the photoinitiator and ultraviolet radiation to generate a cured product containing a thioether bond (-CS-). Not only is the degree of curing of Example 1, Comparative Example 1 and Comparative Example 1 improved under a low-temperature ultraviolet environment, the product also has a higher bond energy of the disulfide bond (RSS-R') than that of Comparative Example 2, and has better mechanical properties and resistance to high-cold and strong ultraviolet radiation aging. However, due to different formula ratios, the content of the cured product containing thioether bonds (-CS-) in the product is different. Therefore, the mechanical properties and high-cold strong ultraviolet radiation aging resistance of Example 1, Comparative Example 1, and Comparative Example 2 are quite different: the mechanical properties and high-cold strong ultraviolet radiation aging resistance of Example 1 are the best, indicating that the content of thioether bonds (-CS-) in the cured product is the highest, and its formula is optimal under the construction conditions of high-cold strong ultraviolet radiation; the comprehensive performance of Comparative Example 2 is better than that of Comparative Example 1, indicating that the content of thioether bonds (-CS-) in the cured product is higher than that of Comparative Example 1, but it still does not meet the standard requirements, so the formulas of Comparative Example 1 and Comparative Example 2 are not suitable for airport construction conditions with high cold and strong ultraviolet radiation.

[0057] From the perspective of curing performance, the surface drying time of Example 1, Comparative Example 1, and Comparative Example 2 under low-temperature ultraviolet radiation environment is less than 16 hours, which meets the requirements of the civil aviation MH 5006 standard, while Comparative Example 3 does not meet the construction standard requirements, indicating that the introduction of ethyl vinyl sulfide and photoinitiator improves the curing speed of the sealant in a high-cold and strong ultraviolet environment.

[0058] From the perspective of curing performance, the surface drying time of Example 1 is only 6 hours, which is of great significance for non-stop construction under high-altitude and cold conditions at high-altitude airports (MH 5006 requires that the surface drying time should not exceed 6 hours when non-stop construction is carried out). In terms of mechanical properties after 28 days of curing, the civil aviation MH 5006 standard requires an elastic recovery rate of ≥80 / %, a tensile modulus of ≤0.4MPa at 23°C, and a tensile modulus of ≤0.6MPa at -20°C. Only Example 1 fully meets the standard requirements, indicating that the caulking material provided by the present invention can still achieve a high degree of curing in a relatively short curing time under a strong ultraviolet environment with a large temperature difference between day and night, and the adhesive properties and mechanical properties after curing meet the requirements of civil aviation construction.

[0059] From the perspective of curing performance, the tensile modulus of Comparative Example 2 meets the requirements, but the elastic recovery rate is slightly lower than the requirements.

[0060] From the perspective of curing performance, the tensile modulus and elastic recovery rate of Comparative Examples 1 and 3 do not meet the requirements.

[0061] From the perspective of high-cold and strong ultraviolet radiation resistance, after two years of artificially simulating the actual service environment of high-cold and strong ultraviolet radiation at a high-altitude airport, the mechanical properties and bonding properties of Comparative Example 3 are the worst. The bonding failure form after ultraviolet aging is no longer cohesive failure, but interfacial failure is formed at the bonding interface between the joint glue and the concrete, indicating that its internal molecular chain scission fails and loses its adhesion to the concrete. Only Example 1 still meets the requirements of the civil aviation MH 5006 standard after ultraviolet aging (elastic recovery rate ≥ 80 / %, 23°C tensile modulus ≤ 0.4MPa, -20°C tensile modulus ≤ 0.6MPa); the performance of Comparative Example 2 barely meets the standard requirements before ultraviolet aging, but after artificial accelerated aging, the mechanical properties and bonding properties are significantly reduced.

[0062] The performance of Example 1 is higher than that of Comparative Example 1 and Comparative Example 2, indicating that 0.2 g of Irgacure 2959 photoinitiator in Example 1 is the best ratio to initiate the photopolymerization reaction of 8 g of ethyl vinyl sulfide and liquid polysulfide rubber. At the same time, a redox reaction of liquid polysulfide rubber and manganese dioxide is also taking place in Example 1. Liquid polysulfide rubber is a consumable monomer of the two reactions. Only the formula of Example 1 can cure the two components into a caulking adhesive with performance that meets the civil aviation construction standards under a high-cold and strong ultraviolet environment.

[0063] In summary, the surface drying time, hardness after 7 days of curing, elastic recovery rate, tensile modulus, elongation at break after 28 days of curing, and elastic recovery rate, tensile modulus, elongation at break, and hardness after two years of artificial UV aging of Example 1 are far superior to those of Comparative Example 3, indicating that with the introduction of ethyl vinyl sulfide and photoinitiator Irgacure 2959, the polysulfide raw rubber undergoes a photopolymerization reaction under ultraviolet radiation to generate a cured product containing a thioether bond (-CS-) with more stable bond energy.

[0064] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A high-altitude airport runway filler, comprising a base paste and a vulcanized paste, characterized in that: The base paste includes liquid polysulfide rubber, ethyl vinyl sulfide and auxiliary material A; the vulcanizing paste includes manganese dioxide, photoinitiator and auxiliary material B.

2. The high plateau airport runway filler according to claim 1, characterized in that: The auxiliary material A comprises active nano calcium carbonate, light calcium carbonate, fumed silicon dioxide, magnesium stearate, dioctyl terephthalate and vinyl triethoxysilane.

3. The high plateau airport runway filler according to claim 2, characterized in that: The components of the base paste are calculated by weight and include 98-100 parts of liquid polysulfide rubber, 8-9 parts of ethyl vinyl sulfide, 28-30 parts of active nano calcium carbonate, 4-5 parts of light calcium carbonate, 1-2 parts of fumed silica, 0.5-1 part of magnesium stearate, 8-9 parts of dioctyl terephthalate, and 0.1-0.5 parts of vinyl triethoxy silane.

4. The high plateau airport runway filler according to claim 3, characterized in that: The components of the base paste are calculated by weight and include 100 parts of liquid polysulfide rubber, 8 parts of ethyl vinyl sulfide, 30 parts of active nano calcium carbonate, 5 parts of light calcium carbonate, 1 part of fumed silica, 1 part of magnesium stearate, 8.5 parts of dioctyl terephthalate, and 0.45 parts of vinyl triethoxysilane.

5. The high plateau airport runway filler according to claim 1, characterized in that: Auxiliary material B includes dioctyl terephthalate, 1,3-biphenylguanidine, carbon black, epoxy resin and sulfur.

6. The high plateau airport runway filler according to claim 5, characterized in that: The components of the vulcanizing paste are calculated by weight and include 90 parts of manganese dioxide, 0.1-0.2 parts of photoinitiator, 8-10 parts of dioctyl terephthalate, 5-7 parts of 1,3-biphenylguanidine, 8-10 parts of carbon black, 8-10 parts of epoxy resin and 0.1-0.3 parts of sulfur.

7. The high plateau airport runway filler according to claim 6, characterized in that: The components of the vulcanizing paste are calculated by weight: 90 parts of manganese dioxide, 0.2 parts of photoinitiator, 9 parts of dioctyl terephthalate, 7 parts of 1,3-biphenylguanidine, 9 parts of carbon black, 9 parts of epoxy resin, and 0.25 parts of sulfur.

8. The high plateau airport runway filler according to claim 1, characterized in that: The liquid polysulfide rubber is obtained by mixing liquid polysulfide rubbers with weight average molecular weights of 2000 and 4500 in a mass ratio of 3-5:5-7.

9. The high plateau airport runway filler according to claim 1, characterized in that: The mass ratio of base paste to vulcanizing paste is 100:8-10.

10. A method for preparing a high-altitude airport runway filler as claimed in any one of claims 1 to 9, characterized in that: The steps include: Weigh each component of the base paste and blend them to obtain the base paste; Weigh each component of the vulcanizing paste, grind it, and obtain the vulcanizing paste; The base paste and the vulcanized paste are mixed to obtain a joint filler for high-altitude airport runways.

Citation Information

Patent Citations

  • Silane-terminiated polysulfide rubber sealant and preparation method thereof

    CN103059800A

  • Room-temperature-curing three-component polysulfide waterproof sealant and preparation method thereof

    CN103450839A

  • High peeling strength polysulfide sealant and sealing method

    CN103555264A

  • Polythioether sealant

    CN105295375A

  • Aircraft environmental-protection sealant and preparation method thereof

    CN109021912A