Curing type heat-conducting silicone grease stored at normal temperature and preparation method of curing type heat-conducting silicone grease
By using a combination of vinyl silicone oil, hydrogen-containing silicone oil and pretreated thermal filler in thermal grease, combined with inhibitors and low-temperature wax-coated catalyst system, the curing of room temperature storage and high-performance thermal grease is achieved, and the silicone oil is solved The problems of ooze, cracking and difficult to reduce interface thickness meet the thermal management needs of high-density electronic components.
Patent Information
- Application Number
- CN202411069278.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-08
AI Technical Summary
The existing thermally conductive silicone grease is prone to leakage and cracking of silicone oil during use, and it needs to be refrigerated and stored, which increases the difficulty of storage and transportation, and the interface thickness is difficult to reduce, which cannot meet the thermal management needs of high-density electronic components.
Using cured thermally conductive grease stored at room temperature, the combination of vinyl silicone oil, hydrogen-containing silicone oil, pretreated thermally conductive filler and additive mixed solution is used to prevent cross-linking reactions and achieve curing. Formation, easy to store and use at room temperature.
It realizes that silicone oil leaks and cracks are not prone to occur at room temperature, has good aging resistance, and reduces the interface thickness and thermal resistance of thermal grease, meeting the thermal management needs of high-density electronic components.
Smart Images

Figure CN118909448A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of thermal grease, and in particular to a curing thermal grease stored at room temperature and a preparation method thereof. Background Art
[0002] With the advancement and development of science and technology, electronic components are moving towards high integration and high assembly density, which also brings about the heating problem of high-density equipment. Overheating will greatly affect the performance and service life of electronic components. Thermal grease, as a paste-like thermal interface material, can well fill the gaps between interfaces to achieve rapid heat transfer to the radiator.
[0003] Dense electronic components require thermal grease to have lower thermal resistance and lower interface thickness (Bond Line Thickness, BLT). However, the interface thickness of existing thermal grease is difficult to reduce and cannot meet application requirements. In addition, there are two types of traditional thermal grease matrices, one is non-reactive dimethyl silicone oil, which has a two-dimensional linear structure, and the other uses vinyl silicone oil and hydrogen-containing silicone oil for a small amount of cross-linking to form a weak pre-cross-linked structure. However, these two materials are prone to silicone oil leakage and cracking during use. In recent years, some people have proposed curing thermal grease. Compared with traditional thermal grease, curing thermal grease can effectively solve the problems of silicone oil leakage and cracking. However, curing thermal grease needs to be stored in a refrigerator, which increases the difficulty of storage and transportation. Summary of the invention
[0004] In view of the above-mentioned problems, the present application is proposed to provide a curable thermal conductive silicone grease stored at room temperature and a preparation method thereof, which overcomes the problems or at least partially solves the problems, comprising:
[0005] A curing thermally conductive silicone grease stored at room temperature comprises, by weight: 4-6 parts of vinyl silicone oil, 0.3-2 parts of hydrogenated silicone oil, 87-95 parts of pretreated thermally conductive filler and 0.5-5 parts of an auxiliary agent mixed solution; wherein the auxiliary agent mixed solution comprises, by weight: 50-95 parts of vinyl silicone oil, 1-5 parts of an inhibitor and 2-20 parts of a pretreated catalyst; the pretreated catalyst is a catalyst coated with low-temperature wax.
[0006] Preferably, the vinyl silicone oil comprises at least one of a vinyl silicone oil having a viscosity of 450-550 mPa·s and a vinyl content of 0.38-0.48 wt %, a vinyl silicone oil having a viscosity of 270-300 mPa·s and a vinyl content of 0.52-0.58 wt %, and a vinyl silicone oil having a viscosity of 90-110 mPa·s and a vinyl content of 1.0-1.06 wt %.
[0007] Preferably, the active hydrogen content of the hydrogen-containing silicone oil is 1.5-2.5 mmoles / gm and the viscosity is 40-300 cSt.
[0008] Preferably, the pretreated thermally conductive filler is a thermally conductive filler obtained by surface modification with a coupling agent.
[0009] Preferably, the thermally conductive filler includes at least one of aluminum oxide, aluminum nitride, aluminum hydroxide, zinc oxide, aluminum powder, copper powder, silver powder and diamond.
[0010] Preferably, the coupling agent is at least one of dodecyltrimethoxysilane, dodecyltriethoxysilane, hexadecyltrimethoxysilane, hexadecyltriethoxysilane, single-end trimethyl / ethoxysilane-terminated polydimethylsiloxane and polyether-modified polydimethylsiloxane.
[0011] Preferably, the particle size of the thermally conductive filler is no greater than 20 μm.
[0012] Preferably, the catalyst is a chloroplatinic acid isopropanol solution with a platinum content of 0.2-1 wt%.
[0013] Preferably, the inhibitor is acetylene cyclohexanol.
[0014] A method for preparing the curable thermally conductive silicone grease as described in any one of the above items, comprising:
[0015] Stirring and mixing the coupling agent and the thermally conductive filler to obtain a pretreated thermally conductive filler;
[0016] The catalyst and low-temperature wax are stirred and mixed at 100-120° C., and the pretreated catalyst is obtained after cooling;
[0017] The pretreatment catalyst, the inhibitor and the vinyl silicone oil are stirred and mixed to obtain an additive mixed solution;
[0018] The pretreated thermally conductive filler, the auxiliary agent mixed solution, vinyl silicone oil and hydrogen-containing silicone oil are stirred and mixed to obtain a curing thermally conductive silicone grease.
[0019] This application has the following advantages:
[0020] In the embodiments of the present application, in contrast to the problem that existing thermal greases need to be stored in a refrigerator, the present application provides a solution using an auxiliary agent system that does not react at room temperature, specifically: "A curable thermal grease stored at room temperature, comprising, by mass: 4-6 parts of vinyl silicone oil, 0.3-2 parts of hydrogenated silicone oil, 87-95 parts of pretreated thermal conductive filler and 0.5-5 parts of an auxiliary agent mixed solution; wherein, the auxiliary agent mixed solution comprises, by mass: 50-95 parts of vinyl silicone oil, 1-5 parts of an inhibitor and 2-20 parts of a pretreated catalyst; the pretreated catalyst is a catalyst coated with low-temperature wax". By using a curable thermal grease, it has good aging resistance and is not prone to silicone oil leakage and cracking during use; by using an inhibitor and a catalyst coated with low-temperature wax as an auxiliary agent system, it can effectively prevent the cross-linking reaction of vinyl silicone oil and hydrogenated silicone oil at room temperature from curing and forming, making it easy to store at room temperature. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solution of the present application, the drawings required for use in the description of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0022] Figure 1 It is a flow chart of the steps of a method for preparing a curable thermal grease provided in one embodiment of the present application. DETAILED DESCRIPTION
[0023] In order to make the objects, features and advantages of the present application more obvious and understandable, the present application is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.
[0024] The inventors have found through analysis of the prior art that curable thermal grease contains catalysts and crosslinking agents, which are easy to react at room temperature, causing the grease to cure prematurely. However, the existing curable thermal grease lacks a system that can prevent these additives from reacting at room temperature. Therefore, the product can only be stored at low temperatures to delay the occurrence of crosslinking reactions. In addition, the existing thermal grease contains thermally conductive fillers with large particle sizes, which makes it impossible to fully compress the thermal grease when pressure is applied, making it difficult to reduce the interface thickness of the thermal grease and unable to meet application requirements.
[0025] In one embodiment of the present application, a curable thermal grease for storage at room temperature is provided, which includes, by mass, 4-6 parts of vinyl silicone oil, 0.3-2 parts of hydrogenated silicone oil, 87-95 parts of pretreated thermal conductive filler and 0.5-5 parts of an auxiliary agent mixed solution; wherein the auxiliary agent mixed solution includes, by mass, 50-95 parts of vinyl silicone oil, 1-5 parts of an inhibitor and 2-20 parts of a pretreated catalyst; the pretreated catalyst is a catalyst coated with low-temperature wax.
[0026] By using curing thermal grease, it has good aging resistance and is not prone to silicone oil leakage and cracking during use; by using inhibitors and low-temperature wax-coated catalysts as auxiliary agent systems, it can effectively prevent vinyl silicone oil and hydrogen silicone oil from undergoing cross-linking reactions at room temperature and thus curing and forming, making it easy to store at room temperature.
[0027] Next, a curing thermal grease stored at room temperature in this exemplary embodiment will be further described.
[0028] In this embodiment, the vinyl silicone oil includes at least one of a vinyl silicone oil having a viscosity of 450-550 mPa·s and a vinyl content of 0.38-0.48 wt%, a viscosity of 270-300 mPa·s and a vinyl content of 0.52-0.58 wt%, and a viscosity of 90-110 mPa·s and a vinyl content of 1.0-1.06 wt%. The vinyl silicone oil having a viscosity of 450-550 mPa·s and a vinyl content of 0.38-0.48 wt% can provide appropriate fluidity and can provide an appropriate crosslinking density under the action of a catalyst. The vinyl silicone oil having a viscosity of 270-300 mPa·s and a vinyl content of 0.52-0.58 wt% has higher fluidity and can provide higher crosslinking density under the action of a catalyst. The vinyl silicone oil having a viscosity of 90-110 mPa·s and a vinyl content of 1.0-1.06 wt% provides higher fluidity and can provide higher crosslinking density under the action of a catalyst. In specific applications, vinyl silicone oils with different viscosities and vinyl contents can be selected according to the performance requirements of the thermal grease, or several different types of vinyl silicone oils can be mixed to achieve the best effect.
[0029] In the present embodiment, the active hydrogen content of the hydrogen-containing silicone oil is 1.5-2.5mmoles / gm, and the viscosity is 40-300cSt. The active hydrogen content reflects the number of Si-H bonds in the hydrogen-containing silicone oil. The increase in active hydrogen content can make the cross-linking reaction more sufficient, and the cured thermal grease has a higher cross-linking density, thereby improving its mechanical strength and thermal conductivity. The viscosity range of the hydrogen-containing silicone oil affects the fluidity and coating performance of the thermal grease. A lower viscosity helps to improve the fluidity of the thermal grease, making it easier to fill small gaps when pressure is applied, while a higher viscosity can improve the mechanical strength of the thermal grease and the stability after curing to a certain extent. In specific applications, hydrogen-containing silicone oils with specific active hydrogen content and viscosity can be selected according to the performance requirements of the required thermal grease to achieve the best results.
[0030] In this embodiment, the pretreated thermally conductive filler is a thermally conductive filler surface-modified by a coupling agent. The coupling agent can form a chemically bonded organic layer on the surface of the thermally conductive filler, changing the surface of the thermally conductive filler from hydrophilic to lipophilic, thereby enhancing the compatibility of the thermally conductive filler with the silicone grease matrix.
[0031] In this embodiment, the type of the thermal conductive filler includes at least one of aluminum oxide, aluminum nitride, aluminum hydroxide, zinc oxide, aluminum powder, copper powder, silver powder and diamond.
[0032] In this embodiment, the shape of the thermal conductive filler includes at least one of spherical, quasi-spherical, fibrous and flake.
[0033] In this embodiment, the coupling agent is at least one of dodecyltrimethoxysilane, dodecyltriethoxysilane, hexadecyltrimethoxysilane, hexadecyltriethoxysilane, single-ended trimethyl / ethoxysilane-terminated polydimethylsiloxane and polyether-modified polydimethylsiloxane.
[0034] In this embodiment, the particle size of the thermally conductive filler is no greater than 20 μm. The thermally conductive filler is obtained by sieving powder, so that powder with a particle size greater than 20 μm is sieved out. By using a thermally conductive filler with a particle size no greater than 20 μm, the thermally conductive silicone grease can be fully compressed when pressure is applied, thereby helping to reduce the interface thickness of the thermally conductive silicone grease, thereby obtaining a lower thermal resistance.
[0035] In this embodiment, the pretreatment catalyst includes, by weight, 1-10 parts of catalyst and 1-10 parts of low-temperature wax. As an example, the mass ratio of the catalyst to the low-temperature wax is 1:1.
[0036] In this embodiment, the catalyst is a chloroplatinic acid isopropanol solution with a platinum content of 0.2-1 wt %. The catalyst can accelerate the cross-linking reaction and improve production efficiency.
[0037] In this embodiment, the low temperature wax includes at least one of polyolefin wax, microcrystalline wax, protective wax and resin. The low temperature wax can be coated on the surface of the catalyst to prevent it from being released at room temperature.
[0038] In this embodiment, the softening point of the low temperature wax is 40-100° C. When the temperature exceeds the softening point of the low temperature wax, the catalyst is released, and the vinyl silicone oil and the hydrogen-containing silicone oil undergo a cross-linking reaction under the action of the catalyst, so that the thermal conductive silicone grease is cured and formed.
[0039] In this embodiment, the inhibitor is acetylene cyclohexanol. The inhibitor can prevent the reaction from being too fast, ensure uniformity, prevent side reactions from occurring, and improve durability.
[0040] Reference Figure 1 In one embodiment of the present application, a method for preparing the curable thermal conductive silicone grease as described in any of the above embodiments is provided, comprising:
[0041] S110, stirring and mixing the coupling agent and the thermally conductive filler to obtain a pretreated thermally conductive filler;
[0042] S120, stirring and mixing the catalyst and low-temperature wax at 100-120° C., and cooling to obtain a pretreated catalyst;
[0043] S130, stirring and mixing the pre-treated catalyst, inhibitor and vinyl silicone oil to obtain an additive mixed solution;
[0044] S140, stirring and mixing the pretreated thermally conductive filler, the auxiliary agent mixed solution, the vinyl silicone oil and the hydrogen-containing silicone oil to obtain a curable thermally conductive silicone grease.
[0045] As described in step S110, the coupling agent and the thermally conductive filler are stirred and mixed to obtain a pretreated thermally conductive filler.
[0046] The thermally conductive filler with a large particle size is screened out through a sieve, and the coupling agent and the thermally conductive filler are placed in a high-speed mixer for treatment for 5 minutes to obtain a pretreated thermally conductive filler.
[0047] As described in step S120, the catalyst and low-temperature wax are stirred and mixed at 100-120°C, and then cooled to obtain a pretreated catalyst.
[0048] The catalyst and the low-temperature wax are stirred and mixed at 100-120° C. so that the low-temperature wax is coated on the surface of the catalyst, and a solid pre-treated catalyst is obtained after cooling.
[0049] As described in step S130, the pretreatment catalyst, inhibitor and vinyl silicone oil are stirred and mixed to obtain an additive mixed solution.
[0050] The inhibitor and vinyl silicone oil are stirred and mixed to obtain an inhibitor solution; the pretreated catalyst and the inhibitor solution are stirred and mixed to obtain an additive mixed solution.
[0051] As described in step S140, the pretreated thermally conductive filler, the auxiliary agent mixed solution, the vinyl silicone oil and the hydrogen-containing silicone oil are stirred and mixed to obtain a curable thermally conductive silicone grease.
[0052] The auxiliary agent mixed solution, vinyl silicone oil and hydrogen-containing silicone oil are stirred and mixed to obtain a mixed base material; the pretreated thermal conductive filler and the mixed base material are placed in a homogenizer, and stirred at high speed for 10 minutes under a vacuum condition of -90 kPa to obtain a single-component curable thermal conductive silicone grease.
[0053] Embodiment 1:
[0054] A curable thermal conductive silicone grease stored at room temperature, comprising, by mass: 4.5 parts of vinyl silicone oil with a viscosity of 90-110 mPa·s, 1 part of vinyl silicone oil with a viscosity of 270-300 mPa·s, 1 part of hydrogen-containing silicone oil with a hydrogen content of 0.18%, 92.5 parts of pretreated thermal conductive filler and 1 part of auxiliary agent mixed solution; wherein the pretreated thermal conductive filler comprises, by mass: 80 parts of spherical aluminum powder, 10 parts of zinc oxide, 10 parts of aluminum oxide and hexadecyl trimethylolpropane 0.5 parts of oxysilane; the particle size of the spherical aluminum powder, the zinc oxide and the aluminum oxide is not more than 20 μm; the auxiliary agent mixed solution comprises, by mass: 93 parts of vinyl silicone oil with a viscosity of 90-110 mPa·s, 1 part of acetylene cyclohexanol and 6 parts of a pre-treated catalyst, wherein the pre-treated catalyst is a catalyst coated with low-temperature wax, and comprises, by mass: 3 parts of chloroplatinic acid isopropanol solution with a platinum content of 0.25% and 3 parts of a resin with a softening point of 80°C.
[0055] The preparation method of the curing thermally conductive silicone grease comprises: removing the thermally conductive filler with a particle size greater than 20 μm through a sieve, placing the coupling agent and the thermally conductive filler in a high-speed stirrer for 5 minutes, and obtaining a pretreated thermally conductive filler. The catalyst and the low-temperature wax are stirred and mixed at 110° C. so that the low-temperature wax is coated on the surface of the catalyst, and a solid pretreated catalyst is obtained after cooling. The inhibitor and the vinyl silicone oil are stirred and mixed to obtain an inhibitor solution; the pretreated catalyst and the inhibitor solution are stirred and mixed to obtain an auxiliary agent mixed solution. The auxiliary agent mixed solution, vinyl silicone oil and hydrogen-containing silicone oil are stirred and mixed to obtain a mixed base material; the pretreated thermally conductive filler and the mixed base material are placed in a homogenizer, and stirred at high speed for 10 minutes under a vacuum condition of -90 kPa to obtain a curing thermally conductive silicone grease.
[0056] Embodiment 2:
[0057] A curing thermal conductive silicone grease stored at room temperature, comprising, by weight: 4.5 parts of vinyl silicone oil with a viscosity of 90-110 mPa·s, 0.5 parts of hydrogenated silicone oil with a hydrogen content of 0.36%, 94.5 parts of pretreated thermal conductive filler and 0.5 parts of an auxiliary agent mixed solution; wherein the pretreated thermal conductive filler comprises, by weight: 75 parts of spherical aluminum powder, 10 parts of zinc oxide, 15 parts of aluminum oxide, 0.1 parts of hexadecyltrimethoxysilane and 0.5 parts of single-ended trimethoxysilane with a molecular weight of 1000 Da. 0.4 parts of alkyl-terminated polydimethylsilicone oil; the particle sizes of the spherical aluminum powder, the zinc oxide and the aluminum oxide are not greater than 20 μm; the auxiliary agent mixed solution comprises, by mass, 93 parts of vinyl silicone oil with a viscosity of 90-110 mPa·s, 1 part of acetylene cyclohexanol and 6 parts of a pre-treated catalyst, wherein the pre-treated catalyst is obtained by coating the catalyst with low-temperature wax, and comprises, by mass, 3 parts of chloroplatinic acid isopropanol solution with a platinum content of 0.25% and 3 parts of polyethylene grease with a softening point of 75°C.
[0058] The preparation method of the curable thermally conductive silicone grease is the same as that of Example 1.
[0059] Embodiment 3:
[0060] A curing thermal conductive silicone grease stored at room temperature, comprising, by weight: 4.75 parts of vinyl silicone oil with a viscosity of 90-110 mPa·s, 0.5 parts of hydrogenated silicone oil with a hydrogen content of 0.18%, 0.25 parts of hydrogenated silicone oil with a hydrogen content of 0.36%, 94 parts of pretreated thermal conductive filler and 0.5 parts of an auxiliary agent mixed solution; wherein the pretreated thermal conductive filler comprises, by weight: 80 parts of spherical aluminum powder, 10 parts of zinc oxide, 5 parts of aluminum oxide, 5 parts of aluminum nitride and a single-ended trimethylolpropane with a molecular weight of 1000 Da. 1 part of oxysilane-terminated polydimethylsilicone oil; the particle size of the spherical aluminum powder, the zinc oxide, the aluminum oxide and the aluminum nitride is not more than 20 μm; the auxiliary agent mixed solution comprises, by mass, 90 parts of vinyl silicone oil with a viscosity of 90-110 mPa·s, 2 parts of acetylene cyclohexanol and 8 parts of a pre-treated catalyst, wherein the pre-treated catalyst is obtained by coating the catalyst with low-temperature wax, and comprises, by mass, 4 parts of chloroplatinic acid isopropanol solution with a platinum content of 0.25% and 4 parts of polyethylene wax with a softening point of 80°C.
[0061] The preparation method of the curable thermally conductive silicone grease is the same as that of Example 1.
[0062] Comparative Example 1:
[0063] A non-reactive thermally conductive silicone grease using dimethyl silicone oil as a silicone oil matrix, specifically comprising, by mass, 6.5 parts of dimethyl silicone oil and 92.5 parts of a thermally conductive filler; wherein, by mass, the thermally conductive filler comprises: 80 parts of spherical aluminum powder, 10 parts of zinc oxide and 10 parts of aluminum oxide; the particle sizes of the spherical aluminum powder, the zinc oxide and the aluminum oxide are 10-50 μm, including powders with a particle size greater than 20 μm.
[0064] Comparative Example 2:
[0065] A curing thermally conductive silicone grease using a conventional auxiliary agent system, specifically comprising, by weight: 4.5 parts of vinyl silicone oil with a viscosity of 90-110 mPa·s, 1 part of vinyl silicone oil with a viscosity of 270-300 mPa·s, 1 part of hydrogen-containing silicone oil with a hydrogen content of 0.18%, 92.5 parts of thermally conductive fillers and 1 part of an auxiliary agent mixed solution; wherein the thermally conductive fillers, by weight, comprise: 80 parts of spherical aluminum powder, 10 parts of zinc oxide and 10 parts of aluminum oxide; the particle sizes of the spherical aluminum powder, the zinc oxide and the aluminum oxide are 10-50 μm, including powders with a particle size greater than 20 μm; the auxiliary agent mixed solution, by weight, comprises: 93 parts of vinyl silicone oil with a viscosity of 90-110 mPa·s, 1 part of acetylene cyclohexanol and 3 parts of chloroplatinic acid isopropanol solution with a platinum content of 0.25%.
[0066] The performance of the thermal grease of Examples 1-3 and Comparative Examples 1-2 was tested according to the following method: (1) Thermal conductivity: A HotDisk thermal conductivity meter was used, the test standard was ISO22007-2, and the test temperature was 25°C. (2) Thermal resistance: An interface material thermal resistance and thermal conductivity coefficient meter was used, the test standard was ASTMD5470, and the test conditions were 80°C and 40psi. (3) Viscosity: A Brookfield rotational viscometer was used, the test standard was ASTMD2196, and the test conditions were 25°C and 10rpm. (4) BLT: A micrometer was used for testing. (5) Fixture thermal resistance: The grease was applied to the middle of the fixture with a thickness of 1mm, and the thermal resistance was tested with a fixture tooling. An interface material thermal resistance and thermal conductivity coefficient meter was used, the test standard was ASTMD5470, and the test conditions were 80°C and 40psi. (6) Fixture thermal resistance after high temperature aging: The fixture was placed at 150°C and baked for 1000h, and then the fixture thermal resistance was tested. The results are shown in the following table:
[0067]
[0068] Table 1 Performance test results of Examples 1-3 and Comparative Examples 1-2
[0069] As can be seen from Table 1, when testing BLT and thermal resistance under the same conditions, Experimental Examples 1-3 have lower BLT and therefore lower thermal resistance. In addition, compared with Comparative Example 1 (non-reactive thermal grease), Experimental Examples 1-3 have lower aging thermal resistance change rates, so they have good reliability. At the same time, compared with Comparative Example 2 (conventional curing thermal grease), the room temperature storage viscosity of Experimental Examples 1-3 does not fluctuate much, so the storage conditions are not harsh. In summary, the curing thermal grease of the present application has lower BLT and thermal resistance, good aging resistance, and is easy to store at room temperature.
[0070] Although the preferred embodiments of the present application have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present application.
[0071] Finally, it should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or terminal device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or terminal device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or terminal device including the elements.
[0072] The above is a detailed introduction to a curable thermal grease stored at room temperature and a preparation method thereof provided by the present application. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for general technicians in this field, according to the ideas of the present application, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A curable thermally conductive silicone grease stored at room temperature, characterized in that: The invention comprises, by weight: 4-6 parts of vinyl silicone oil, 0.3-2 parts of hydrogenated silicone oil, 87-95 parts of pretreated thermal conductive filler and 0.5-5 parts of auxiliary agent mixed solution; wherein, the auxiliary agent mixed solution comprises, by weight: 50-95 parts of vinyl silicone oil, 1-5 parts of inhibitor and 2-20 parts of pretreated catalyst; the pretreated catalyst is a catalyst coated with low-temperature wax.
2. The curable thermally conductive silicone grease according to claim 1, characterized in that: The vinyl silicone oil comprises at least one of a vinyl silicone oil having a viscosity of 450-550 mPa·s and a vinyl content of 0.38-0.48 wt %, a vinyl silicone oil having a viscosity of 270-300 mPa·s and a vinyl content of 0.52-0.58 wt %, and a vinyl silicone oil having a viscosity of 90-110 mPa·s and a vinyl content of 1.0-1.06 wt %.
3. The curable thermally conductive silicone grease according to claim 1, characterized in that: The active hydrogen content of the hydrogen-containing silicone oil is 1.5-2.5 mmoles / gm and the viscosity is 40-300 cSt.
4. The curable thermally conductive silicone grease according to claim 1, characterized in that: The pretreated thermally conductive filler is obtained by surface modification of the thermally conductive filler with a coupling agent.
5. The curable thermally conductive silicone grease according to claim 4, characterized in that: The thermal conductive filler includes at least one of aluminum oxide, aluminum nitride, aluminum hydroxide, zinc oxide, aluminum powder, copper powder, silver powder and diamond.
6. The curable thermally conductive silicone grease according to claim 4, characterized in that: The coupling agent is at least one of dodecyltrimethoxysilane, dodecyltriethoxysilane, hexadecyltrimethoxysilane, hexadecyltriethoxysilane, single-end trimethyl / ethoxysilane-terminated polydimethylsiloxane and polyether-modified polydimethylsiloxane.
7. The curable thermally conductive silicone grease according to claim 1, characterized in that: The particle size of the thermal conductive filler is not greater than 20 μm.
8. The curable thermally conductive silicone grease according to claim 1, characterized in that: The catalyst is a chloroplatinic acid isopropanol solution with a platinum content of 0.2-1wt%.
9. The curable thermally conductive silicone grease according to claim 1, characterized in that: The inhibitor is acetylene cyclohexanol.
10. A method for preparing the curable thermally conductive silicone grease according to any one of claims 1 to 9, characterized in that: include: Stirring and mixing the coupling agent and the thermally conductive filler to obtain a pretreated thermally conductive filler; The catalyst and low-temperature wax are stirred and mixed at 100-120° C., and the pretreated catalyst is obtained after cooling; The pretreatment catalyst, the inhibitor and the vinyl silicone oil are stirred and mixed to obtain an additive mixed solution; The pretreated thermally conductive filler, the auxiliary agent mixed solution, vinyl silicone oil and hydrogen-containing silicone oil are stirred and mixed to obtain a curing thermally conductive silicone grease.
Citation Information
Cited By
Heat-conducting silicone grease as well as preparation method and application thereof
CN119799001A
Thermally conductive silicone grease, and preparation method and application thereof
CN119799001B
Organic silicon heat-conducting coating as well as preparation method and application thereof
CN120098545A
An organosilicon heat-conducting coating, its preparation method and application
CN120098545B