Anti-corrosion aluminum shell and preparation method and application thereof
By installing insulating coatings of photosensitive resin, photoinitiator and modified silica inside the aluminum shell of the lithium-ion battery, the safety accident caused by the failure of the insulation design of the outer layer of the aluminum shell is solved, and the safety and resistance of the battery are improved Corrosive.
Patent Information
- Application Number
- CN202411009890.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
AI Technical Summary
Prior Art In lithium-ion batteries, the failure of the outer insulation design of the aluminum shell causes the negative electrode column of the battery cell to come into contact with the aluminum shell, causing safety accidents.
An insulating coating is provided inside the aluminum shell, and a photosensitive resin, a photoinitiator and modified silica are used to form an insulating layer through electrostatic spraying and photocuring to prevent the aluminum shell from being charged.
It improves the safety and corrosion resistance of lithium-ion batteries, prevents the short circuit between the negative electrode column and the aluminum shell, and enhances the safety during use.
Smart Images

Figure BDA0004964766700000061 
Figure BDA0004964766700000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery materials and relates to an anti-corrosion aluminum shell and a preparation method and application thereof. Background Art
[0002] The safety of square lithium-ion batteries has always been a concern for all users, but corrosion often occurs during use. In order to prevent corrosion inside the aluminum shell, the plastic between the positive pole and the cover usually has a weak resistance, so that the positive pole and the aluminum shell are connected and the aluminum shell is positively charged, but this usually leads to short circuits when the negative pole contacts other cells during use, or short circuits when the negative pole ear inside the battery contacts the aluminum shell, causing safety risks.
[0003] CN112934641A discloses a method for spraying an insulating layer and its use in a battery shell, the method comprising the following steps: spraying an insulating powder coating on the outer surface of the battery shell by an electrostatic powder spraying method, curing, and forming an insulating layer. The method adopts an electrostatic powder spraying method to spray the insulating powder coating on the outer surface of the battery shell to form an insulating layer.
[0004] CN114672223A discloses a light-curing insulating lithium battery shell coating and its preparation method. A light-curing insulating lithium battery shell coating comprises the following components in parts by weight: 30-60 parts of modified epoxy acrylate; 80-120 parts of reactive diluent; 1-5 parts of photoinitiator; 40-60 parts of filler; and its preparation method is: adding modified epoxy acrylate, photoinitiator and filler to the reactive diluent, mixing and stirring, and obtaining the light-curing insulating lithium battery shell coating.
[0005] The above solution provides an insulating coating on the outer layer of the aluminum shell, but the inner layer may fail in the later stage of use due to the insulation design failure of the outer layer of the aluminum shell, resulting in a safety accident caused by the contact between the negative electrode of the battery cell and the aluminum shell. Summary of the invention
[0006] The purpose of the present invention is to provide an anti-corrosion aluminum shell and a preparation method and application thereof. The present invention sprays a light-curing insulating material on the inside of the aluminum shell, and the aluminum shell is not charged, thereby improving safety during use.
[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides an anti-corrosion aluminum shell, wherein an insulating coating is provided on the inner surface of the anti-corrosion aluminum shell, and the insulating coating comprises a cured photosensitive resin, a photoinitiator and modified silica.
[0009] The present invention arranges an insulating coating inside the anti-corrosion aluminum shell, and the aluminum shell is not charged, thereby avoiding safety accidents caused by contact between the negative pole of the battery cell and the aluminum shell due to failure of the insulation design of the outer layer of the aluminum shell in the later stage of lithium-ion battery use. The insulating coating includes a photosensitive resin, a photoinitiator and modified silicon dioxide. The photoinitiator triggers the curing of the photosensitive resin, and modified silicon dioxide particles are added in the middle to form an insulating layer, which further improves the corrosion resistance and safety of the aluminum shell.
[0010] Preferably, the photosensitive resin includes polyurethane oligomer and / or acrylate oligomer.
[0011] Preferably, the photoinitiator includes any one of an acetone photoinitiator, a ketone photoinitiator or a phosphorus oxide photoinitiator, or a combination of at least two thereof.
[0012] Preferably, the acetone-based photoinitiator includes 2-hydroxy-2-methyl-1-phenyl-1-propanone.
[0013] Preferably, the ketone photoinitiator includes 4-chlorobenzophenone.
[0014] Preferably, the phosphorus oxide photoinitiator includes diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide.
[0015] Preferably, the modified silica includes any one of crystalline silica, glassy silica or gel-like silica, or a combination of at least two of them. Typical but non-limiting combinations include a combination of crystalline silica and glassy silica, a combination of glassy silica and gel-like silica, or a combination of crystalline silica and gel-like silica, etc.
[0016] Preferably, taking the mass of the insulating coating as 100%, the mass of the photosensitive resin is 70-90%, for example 70%, 75%, 80%, 85% or 90%, etc., and is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0017] Preferably, the mass of the photoinitiator is 3-5%, for example, 3%, 3.5%, 4%, 4.5% or 5%, etc., and is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0018] Preferably, the mass of the modified silicon dioxide is 10-25%, for example, 10%, 12%, 15%, 20% or 25%, etc., not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0019] Preferably, the thickness of the insulating coating is 10 to 100 μm, for example, 10 μm, 20 μm, 50 μm, 80 μm or 100 μm, etc., but is not limited to the listed values. Other unlisted values within the numerical range are also applicable, preferably 20 to 80 μm.
[0020] In a second aspect, the present invention provides a method for preparing the anti-corrosion aluminum shell as described in the first aspect, the preparation method comprising the following steps:
[0021] Mixing a photosensitive resin, a photoinitiator, modified silicon dioxide and a solvent to obtain an insulating mixed material;
[0022] The insulating mixed material is sprayed on the inner surface of the aluminum shell and subjected to light curing treatment to obtain the anti-corrosion aluminum shell.
[0023] Preferably, the solvent includes any one of methanol, ethanol or acetone, or a combination of at least two of them.
[0024] Preferably, the spraying method includes electrostatic spraying and / or air spraying.
[0025] Preferably, the light intensity of the photocuring treatment is 1000-2000 mW / cm 2 , for example: 1000mW / cm 2 , 1200mW / cm 2 , 1500mW / cm 2 、1800mW / cm 2 or 2000mW / cm 2 The present invention is not limited to the numerical values listed, and other numerical values not listed within the numerical range are also applicable.
[0026] Preferably, the photocuring treatment time is 5 to 15 seconds, for example, 5 seconds, 8 seconds, 10 seconds, 12 seconds or 15 seconds, etc., and is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0027] In a third aspect, the present invention provides a lithium-ion battery, wherein the lithium-ion battery comprises the anti-corrosion aluminum shell as described in the first aspect.
[0028] Preferably, the lithium-ion battery comprises plastic under the positive electrode.
[0029] Preferably, the positive electrode lower plastic is a fully insulated positive electrode lower plastic.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) The present invention performs insulation spraying inside the aluminum shell. When the plastic under the positive electrode is fully insulated, the aluminum shell will not be charged, thereby preventing the negative electrode pole from contacting the positive electrode aluminum shell during use of the lithium-ion battery and causing a safety accident.
[0032] (2) The insulating material of the present invention uses photosensitive resin, photoinitiator and modified silica, and is directly sprayed on the inside of the aluminum shell by spraying. The manufacturing method is simple and the feasibility is high. DETAILED DESCRIPTION
[0033] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0034] The polymers described in the examples and comparative examples of the present invention were purchased from BASF, and the silicon dioxide was purchased from Grace.
[0035] Example 1
[0036] This embodiment provides an anti-corrosion aluminum shell, and the preparation method of the anti-corrosion aluminum shell is as follows:
[0037] (1) mixing a polyurethane oligomer, 2-hydroxy-2-methyl-1-phenyl-1-propanone and crystalline silica in a mass ratio of 80:5:15 to obtain an insulating mixed material;
[0038] (2) After the inner surface of the aluminum shell is dusted, the insulating mixed material is electrostatically sprayed on the inner surface of the aluminum shell at 1200 mW / cm 2 The coating was photocured for 15 seconds under light to obtain an anti-corrosion aluminum shell with an insulating coating thickness of 20 μm.
[0039] Example 2
[0040] This embodiment provides an anti-corrosion aluminum shell, and the preparation method of the anti-corrosion aluminum shell is as follows:
[0041] (1) mixing acrylate oligomer, 4-chlorobenzophenone and glassy silica in a mass ratio of 77:3:20 to obtain an insulating mixed material;
[0042] (2) After the inner surface of the aluminum shell is dusted, the insulating mixed material is electrostatically sprayed on the inner surface of the aluminum shell at 1500 mW / cm 2 The coating was photocured for 10 seconds under light to obtain an anti-corrosion aluminum shell with an insulating coating thickness of 80 μm.
[0043] Example 3
[0044] This embodiment provides an anti-corrosion aluminum shell, and the preparation method of the anti-corrosion aluminum shell is as follows:
[0045] (1) mixing a polyurethane oligomer, diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide and gel-like silica in a mass ratio of 86:4:10 to obtain an insulating mixed material;
[0046] (2) After the inner surface of the aluminum shell is dusted, the insulating mixed material is electrostatically sprayed on the inner surface of the aluminum shell at 2000 mW / cm 2 The coating was photocured for 8 seconds under light to obtain an anti-corrosion aluminum shell with an insulating coating thickness of 50 μm.
[0047] Example 4
[0048] The only difference between this embodiment and embodiment 1 is that the mass proportion of modified silica in the insulating coating is 5% (the proportion of photoinitiator remains unchanged, and the rest is replaced by photosensitive resin), and other conditions and parameters are exactly the same as those in embodiment 1.
[0049] Example 5
[0050] The only difference between this embodiment and embodiment 1 is that the mass proportion of modified silica in the insulating coating is 25% (the proportion of photoinitiator remains unchanged, and the content of photosensitive resin is reduced), and other conditions and parameters are exactly the same as those in embodiment 1.
[0051] Example 6
[0052] The only difference between this embodiment and the first embodiment is that the thickness of the insulating coating is 100 μm, and the other conditions and parameters are exactly the same as those of the first embodiment.
[0053] Example 7
[0054] The only difference between this embodiment and the first embodiment is that the thickness of the insulating coating is 10 μm, and the other conditions and parameters are exactly the same as those of the first embodiment.
[0055] Comparative Example 1
[0056] The only difference between this comparative example and Example 1 is that the crystalline silica is replaced with conventional commercially available silica, and the other conditions and parameters are exactly the same as those in Example 1.
[0057] Comparative Example 2
[0058] The only difference between this comparative example and Example 1 is that the photosensitive resin is replaced by epoxy resin and no photoinitiator is added. Other conditions and parameters are exactly the same as those in Example 1.
[0059] Comparative Example 3
[0060] The only difference between this comparative example and Example 1 is that commercially available conventional silicon dioxide is used as the insulating coating and no photoinitiator is added. Other conditions and parameters are exactly the same as those in Example 1.
[0061] Performance Test:
[0062] The aluminum shells obtained in the embodiments and comparative examples were made into batteries, and voltage was applied between the positive electrode column and the aluminum shell, with a voltage range of 0 to 100 mV. The voltage between the negative electrode column and the aluminum shell was tested, and the test results are shown in Table 1:
[0063] Table 1
[0064]
[0065]
[0066] As can be seen from Table 1, from Examples 1-3, the voltage between the anti-corrosion aluminum shell and the negative electrode column prepared by the method of the present invention can reach below 1.7-1.8V, the insulation effect is good, and the safety during use is improved.
[0067] By comparing Example 1 with Examples 4-5, it can be seen that the proportion of modified silica in the insulating coating of the anti-corrosion aluminum shell of the present invention will affect its performance. When the mass proportion of modified silica in the insulating coating is controlled at 10-20%, the performance of the obtained anti-corrosion aluminum shell is better. If the mass proportion of modified silica in the insulating coating is too high, the cost increases but the effect is not significantly improved. If the mass proportion of modified silica in the insulating coating is too low, the insulating effect is significantly deteriorated.
[0068] By comparing Example 1 with Examples 6-7, it can be seen that the thickness of the insulating coating of the anti-corrosion aluminum shell of the present invention will affect its performance. When the thickness of the insulating coating is controlled at 20 to 80 μm, the performance of the obtained anti-corrosion aluminum shell is better. If the thickness of the insulating coating is too large, the cost increases but the effect is not significantly improved. If the thickness of the insulating coating is too small, it cannot play an insulating role.
[0069] From the comparison between Example 1 and Comparative Example 1, it can be seen that the use of unmodified silica in the insulating layer of the present invention does not have an obvious insulating effect. This may be because the bonding strength between conventional silica and photosensitive resin is low, the coating uniformity is poor, and the outer surface of the aluminum shell cannot be completely covered.
[0070] By comparing Example 1 and Comparative Example 2, it can be seen that the present invention uses a photosensitive resin in combination with a photoinitiator to prepare an insulating coating. Compared with conventional resins, the coating obtained after photochemical treatment of the photosensitive resin has better insulation effect, greater bonding strength with silicon dioxide, and significantly improved stability.
[0071] From the comparison between Example 1 and Comparative Example 3, it can be seen that the insulating coating is prepared by combining the photosensitive resin of the present invention with the photoinitiator, the photocuring operation is simple, and the mechanical strength of the modified silica can be significantly increased.
[0072] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. An anti-corrosion aluminum shell, characterized in that: An insulating coating is arranged on the inner surface of the anti-corrosion aluminum shell, and the insulating coating comprises a cured photosensitive resin, a photoinitiator and modified silicon dioxide.
2. The anti-corrosion aluminum shell according to claim 1, characterized in that: The photosensitive resin includes polyurethane oligomer and / or acrylate oligomer.
3. The anticorrosive aluminum shell according to claim 1 or 2, characterized in that: The photoinitiator includes any one of an acetone photoinitiator, a ketone photoinitiator or a phosphorus oxide photoinitiator, or a combination of at least two thereof; Preferably, the acetone-based photoinitiator includes 2-hydroxy-2-methyl-1-phenyl-1-propanone; Preferably, the ketone photoinitiator includes 4-chlorobenzophenone; Preferably, the phosphorus oxide photoinitiator includes diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide.
4. The anti-corrosion aluminum shell according to any one of claims 1 to 3, characterized in that: The modified silica includes any one of crystalline silica, glassy silica or gel-like silica, or a combination of at least two of them.
5. The anti-corrosion aluminum shell according to any one of claims 1 to 4, characterized in that: Taking the mass of the insulating coating as 100%, the mass of the photosensitive resin is 70-90%; Preferably, the mass of the photoinitiator is 3-5%; Preferably, the mass of the modified silicon dioxide is 10-25%.
6. The anti-corrosion aluminum shell according to any one of claims 1 to 5, characterized in that: The thickness of the insulating coating is 10-100 μm, preferably 20-80 μm.
7. A method for preparing the anticorrosive aluminum shell according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: Mixing a photosensitive resin, a photoinitiator, modified silicon dioxide and a solvent to obtain an insulating mixed material; The insulating mixed material is sprayed on the inner surface of the aluminum shell and subjected to light curing treatment to obtain the anti-corrosion aluminum shell.
8. The preparation method according to claim 7, characterized in that: The solvent includes any one of methanol, ethanol or acetone or a combination of at least two thereof; Preferably, the spraying method includes electrostatic spraying and / or air spraying; Preferably, the light intensity of the photocuring treatment is 1000-2000 mW / cm 2 ; Preferably, the light curing treatment time is 5 to 15 seconds.
9. A lithium ion battery, characterized in that: The lithium-ion battery comprises the anti-corrosion aluminum shell as described in any one of claims 1-6.
10. The lithium ion battery according to claim 9, characterized in that The lithium-ion battery includes a plastic under the positive electrode; Preferably, the positive electrode lower plastic is a fully insulated positive electrode lower plastic.
Citation Information
Patent Citations
(Methyl) acrylic modified polyurethane resin, and ultraviolet curable insulating coating containing same and nano-material
CN103408716A
Photocured insulating paint composition
CN108329786A
Photocuring insulating lithium battery shell coating and preparation method thereof
CN114672223A
Light-cured lithium battery shell heat-resistant insulating coating as well as preparation method and application thereof
CN118064018A
Zinc oxide varistor, a method of preparing the same, and a crystallized glass composition for coating
US5294908A