BTO-PVDF-b-PTFE thermal insulation coating, preparation method thereof and application of BTO-PVDF-b-PTFE thermal insulation coating in automobile ceiling

Through the preparation of BTO-PVDF-b-PTFE thermal insulation coating, combined with nano barium titanate wet slurry and PVDF-b-PTFE, the problem of insufficient UV and infrared barrier in the prior art is solved, and high-efficiency heat insulation and UV resistance are achieved , infrared rays and reduce costs.

CN118909505APending Publication Date: 2024-11-08ZHEJIANG ROUHE NEW ENERGY MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410889668.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When existing thermal insulation coatings face extreme climatic conditions, it is difficult to effectively block ultraviolet and infrared rays, resulting in temperature instability and material aging, and are costly.

Method used

Using BTO-PVDF-b-PTFE thermal insulation coating, the nano-barium titanate wet slurry and polyvinylidene fluoride-polytetrafluoroethylene block copolymer (PVDF-b-PTFE) was used to prepare excellent thermal insulation and A coating with ultraviolet and infrared properties is made through ultrasonic oscillation and vacuum oven defoaming processes.

Benefits of technology

It realizes the functions of long-term heat insulation, radiation cooling and anti-ultraviolet and infrared, which significantly extends the service life of the coating and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004928349790000071
    Figure BDA0004928349790000071
Patent Text Reader

Abstract

The invention relates to the technical field of thermal insulation coatings, in particular to a BTO-PVDF-b-PTFE thermal insulation coating and a preparation method and application thereof in automobile roofs, and the BTO-PVDF-b-PTFE thermal insulation coating comprises the following components in percentage by mass: 10-25% of nano barium titanate wet slurry, 25-55% of PVDF-b-PTFE, 1-5% of a coating additive and 15-50% of a diluent. According to the BTO-PVDF-b-PTFE heat insulation coating, the preparation method thereof and the application of the BTO-PVDF-b-PTFE heat insulation coating in the automobile ceiling, the obtained heat insulation coating can effectively block ultraviolet rays and infrared rays borne by objects exposed in the atmospheric environment, and the functions of long-time heat insulation, radiation cooling and ultraviolet ray and infrared ray resistance are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermal insulation coatings, in particular to a BTO-PVDF-b-PTFE thermal insulation coating and a preparation method thereof and application in automobile ceilings. Background Art

[0002] Against the backdrop of intensified climate change and growing awareness of environmental protection, the technical standards and performance requirements for thermal insulation coatings are showing a significant upward trend. Especially under extreme climate conditions, such as hot summers and cold winters, the thermal insulation performance of thermal insulation coatings for buildings and new energy vehicles has become a key factor in ensuring stable indoor temperature and improving energy efficiency. At present, thermal insulation coatings are classified in detail into barrier thermal insulation coatings, radiant thermal insulation coatings and reflective thermal insulation coatings, among which reflective thermal insulation coatings have attracted much attention due to their unique properties.

[0003] Solar radiation energy is mainly concentrated in two bands: the visible light band (wavelength range of 400-760nm), accounting for about 45% of the total solar energy; the infrared band (wavelength greater than 760nm), its heat energy accounts for about 50% of the total solar energy, and the remaining 5% of energy is distributed in other bands. In addition, the damage of ultraviolet radiation to the exterior walls of buildings or new energy vehicles exposed to the air cannot be ignored. Long-term exposure to ultraviolet rays can easily cause the coating to fade and age, which not only affects the aesthetics, but also significantly reduces its durability.

[0004] Patent CN117986951A provides an anti-ultraviolet acrylic resin thermal insulation coating for building exterior walls and a preparation method thereof. Acrylic emulsion, uniformly dispersed solid filler, titanium dioxide microspheres coated with ultraviolet absorption additive filler, color enhancer, film former, defoamer, leveling agent, and preservative are added to a high-speed mixer and fully stirred. The obtained thermal insulation coating has excellent thermal insulation and anti-ultraviolet properties; but it ignores the main component of solar radiation, infrared, and the absorption of infrared will cause the temperature to rise rapidly. Patent CN202311304966.X discloses a composite material with high-efficiency infrared shielding performance and its preparation method and application. Composite cesium tungsten bronze nanopowder, potassium tungsten bronze-based composite nanopowder, dispersant, and acrylic acid-hydroxypropyl acrylate copolymer are used as raw materials. A composite material with high-efficiency infrared shielding performance is obtained by blending and ball milling. However, the limited reserves of cesium tungsten bronze on the earth lead to high raw material costs. Therefore, the present invention provides a low-cost thermal insulation coating with good blocking effects on both ultraviolet and infrared rays. Summary of the invention

[0005] The purpose of the present invention is to provide a BTO-PVDF-b-PTFE thermal insulation coating, a preparation method thereof and an application in a car roof. The obtained thermal insulation coating can effectively block ultraviolet rays and infrared rays received by objects exposed to the atmospheric environment, and achieve the functions of long-term heat insulation, radiation cooling, and resistance to ultraviolet rays and infrared rays.

[0006] To achieve the above-mentioned purpose, the present invention provides a BTO-PVDF-b-PTFE thermal insulation coating, which comprises, by mass fraction, 10-25% of nano-barium titanate wet slurry, 25-55% of PVDF-b-PTFE (polyvinylidene fluoride-polytetrafluoroethylene block copolymer), 1-5% of coating additive and 15-50% of diluent.

[0007] Preferably, the solid content of the nano-barium titanate wet slurry is 10-30%, and the particle size of the barium titanate nanoparticles (BTO) in the nano-barium titanate wet slurry is in the range of 20-200 nm.

[0008] Preferably, the coating additive includes one of a thickener, a film-forming aid, a leveling agent, and a defoaming agent.

[0009] Preferably, the thickener is polyacrylamide, the film-forming aid is a mixture of ethylene glycol monobutyl ether / dipropylene glycol butyl ether, the leveling agent is an acrylic copolymer, the defoamer is a non-silicone mineral oil mixture containing hydrophobic particles, and the diluent is xylene.

[0010] A method for preparing a BTO-PVDF-b-PTFE thermal insulation coating comprises the following steps:

[0011] S1: dispersing barium titanate nanoparticles BTO in N,N-dimethylformamide, and vigorously stirring by ultrasonic vibration to obtain a BTO / DMF dispersion, i.e., nano-barium titanate wet slurry;

[0012] S2: adding PVDF-b-PTFE powder to the BTO / DMF dispersion of S1 under heating and stirring conditions, stirring until the particles are completely dissolved, and then adding a coating additive and a diluent to obtain a BTO-PVDF-b-PTFE mixed solution;

[0013] S3 puts the BTO-PVDF-b-PTFE mixed solution prepared in S2 into a vacuum oven for degassing to prepare a BTO-PVDF-b-PTFE thermal insulation coating.

[0014] Preferably, the heating in S2 is water bath heating, and the heating temperature is 40-80°C.

[0015] Preferably, the degassing time in S3 is 2 to 4 hours.

[0016] The invention discloses an application of a BTO-PVDF-b-PTFE heat-insulating coating, which is applied to the ultraviolet-infrared protective coating of the automobile roof.

[0017] Beneficial effects of the present invention:

[0018] (1) The BTO-PVDF-b-PTFE thermal insulation coating provided by the present invention is a block copolymer in the form of a milky white viscous slurry, has ductility and rheological properties, can be applied to the surface of a variety of materials to easily form a film, and is convenient for construction workers to perform operations such as spraying and brushing.

[0019] (2) In the BTO-PVDF-b-PTFE thermal insulation coating provided by the present invention, BTO has excellent thermal insulation performance and can effectively reflect and scatter infrared radiation to reduce heat transfer. PVDF-b-PTFE has a lower thermal conductivity coefficient, which can further reduce the thermal conductivity efficiency of the coating. The combination of the two makes the coating perform excellently in terms of thermal insulation. In addition, both BTO and PVDF-b-PTFE have a certain anti-ultraviolet ability, which can prevent ultraviolet rays from damaging the surface of objects. This dual protection mechanism can significantly extend the service life of the coated object.

[0020] (3) In the BTO-PVDF-b-PTFE thermal insulation coating provided by the present invention, PVDF-b-PTFE is a high-performance fluoropolymer with excellent chemical corrosion resistance and can maintain its stable performance in a variety of harsh environments, so that the thermal insulation coating has a long service life in outdoor environments; and PVDF-b-PTFE has good film-forming properties and adhesion, and can be tightly combined with the substrate to form a uniform and dense coating.

[0021] (4) The BTO-PVDF-b-PTFE thermal insulation coating provided by the present invention overcomes the shortcoming of traditional coatings that only block ultraviolet or infrared light waves, and can achieve the synergistic improvement of thermal insulation and resistance to ultraviolet and infrared rays, thereby improving the performance and stability of the coating for automobile roofs. It also has thermal insulation and resistance to ultraviolet and infrared rays, and has broad application prospects.

[0022] (5) The present invention provides a BTO-PVDF-b-PTFE thermal insulation coating, in which both BTO and PVDF-b-PTFE are non-toxic, pollution-free and environmentally friendly materials, so that the thermal insulation coating can not only protect objects from erosion by the external environment, but also reduce pollution to the environment.

[0023] The technical solution of the present invention is further described in detail below through embodiments. DETAILED DESCRIPTION

[0024] The present invention is further described below in conjunction with embodiments. Unless otherwise defined, the technical terms or scientific terms used in the present invention should be the common meanings understood by people with ordinary skills in the field to which the present invention belongs. The above-mentioned features or features mentioned in the specific examples mentioned in the present invention can be combined arbitrarily, and these specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0025] Example 1

[0026] The invention provides a BTO-PVDF-b-PTFE heat-insulating coating, which comprises the following components in percentage by mass: 15% of nano-barium titanate wet slurry, 35% of PVDF-b-PTFE, 5% of acrylic copolymer and 45% of xylene.

[0027] The preparation method of BTO-PVDF-b-PTFE thermal insulation coating comprises the following steps:

[0028] S1: BTO is dispersed in N,N-dimethylformamide, and then stirred vigorously by ultrasonic oscillation to obtain a BTO / DMF dispersion, i.e., nano-barium titanate wet slurry; the particle size of BTO is in the range of 20 to 200 nm.

[0029] S2 heats the BTO / DMF dispersion of S1 to 40-80°C in a water bath and stirs, adds PVDF-b-PTFE powder, stirs until the particles are completely dissolved, and then adds acrylic copolymer and xylene to obtain a BTO-PVDF-b-PTFE mixed solution.

[0030] S3 puts the BTO-PVDF-b-PTFE mixed solution prepared in S2 into a vacuum oven for degassing for 2 to 4 hours to prepare a BTO-PVDF-b-PTFE thermal insulation coating.

[0031] Example 2

[0032] The invention provides a BTO-PVDF-b-PTFE heat-insulating coating, which comprises the following components in percentage by mass: 15% of nano-barium titanate wet slurry, 35% of PVDF-b-PTFE, 5% of ethylene glycol monobutyl ether / dipropylene glycol butyl ether mixture and 45% of xylene.

[0033] The preparation method of BTO-PVDF-b-PTFE thermal insulation coating comprises the following steps:

[0034] S1: BTO is dispersed in N,N-dimethylformamide, and then stirred vigorously by ultrasonic oscillation to obtain a BTO / DMF dispersion, i.e., nano-barium titanate wet slurry; the particle size of BTO is in the range of 20 to 200 nm.

[0035] S2 heats the BTO / DMF dispersion of S1 to 40-80°C in a water bath and stirs, adds PVDF-b-PTFE powder, stirs until the particles are completely dissolved, and then adds a mixture of ethylene glycol monobutyl ether / dipropylene glycol butyl ether and xylene to obtain a BTO-PVDF-b-PTFE mixed solution.

[0036] S3 puts the BTO-PVDF-b-PTFE mixed solution prepared in S2 into a vacuum oven for degassing for 2 to 4 hours to prepare a BTO-PVDF-b-PTFE thermal insulation coating.

[0037] Example 3

[0038] The invention provides a BTO-PVDF-b-PTFE heat-insulating coating, which comprises the following components in percentage by mass: 15% of nano-barium titanate wet slurry, 35% of PVDF-b-PTFE, 5% of polyacrylamide and 45% of xylene.

[0039] The preparation method of BTO-PVDF-b-PTFE thermal insulation coating comprises the following steps:

[0040] S1: BTO is dispersed in N,N-dimethylformamide, and then stirred vigorously by ultrasonic oscillation to obtain a BTO / DMF dispersion, i.e., nano-barium titanate wet slurry; the particle size of BTO is in the range of 20 to 200 nm.

[0041] S2 heats the BTO / DMF dispersion of S1 to 40-80°C in a water bath and stirs, adds PVDF-b-PTFE powder, stirs until the particles are completely dissolved, and then adds polyacrylamide and xylene to obtain a BTO-PVDF-b-PTFE mixed solution.

[0042] S3 puts the BTO-PVDF-b-PTFE mixed solution prepared in S2 into a vacuum oven for degassing for 2 to 4 hours to prepare a BTO-PVDF-b-PTFE thermal insulation coating.

[0043] Example 4

[0044] The invention provides a BTO-PVDF-b-PTFE heat-insulating coating, which comprises the following components in percentage by mass: 15% of nano-barium titanate wet slurry, 35% of PVDF-b-PTFE, 4% of a non-silicone hydrophobic particle-containing mineral oil mixture, and 46% of xylene.

[0045] The preparation method of BTO-PVDF-b-PTFE thermal insulation coating comprises the following steps:

[0046] S1: BTO is dispersed in N,N-dimethylformamide, and then stirred vigorously by ultrasonic oscillation to obtain a BTO / DMF dispersion, i.e., nano-barium titanate wet slurry; the particle size of BTO is in the range of 20 to 200 nm.

[0047] S2 heats the BTO / DMF dispersion of S1 in a water bath to 40-80°C and stirs, adds PVDF-b-PTFE powder, stirs until the particles are completely dissolved, and then adds a non-silicone-containing hydrophobic particle mineral oil mixture and xylene to obtain a BTO-PVDF-b-PTFE mixed solution.

[0048] S3 puts the BTO-PVDF-b-PTFE mixed solution prepared in S2 into a vacuum oven for degassing for 2 to 4 hours to prepare a BTO-PVDF-b-PTFE thermal insulation coating.

[0049] Example 5

[0050] The invention provides a BTO-PVDF-b-PTFE heat-insulating coating, which comprises the following components in percentage by mass: 10% of nano-barium titanate wet slurry, 40% of PVDF-b-PTFE, 5% of acrylic copolymer and 45% of xylene.

[0051] The preparation method of BTO-PVDF-b-PTFE thermal insulation coating comprises the following steps:

[0052] S1: BTO is dispersed in N,N-dimethylformamide, and then stirred vigorously by ultrasonic oscillation to obtain a BTO / DMF dispersion, i.e., nano-barium titanate wet slurry; the particle size of BTO is in the range of 20 to 200 nm.

[0053] S2 heats the BTO / DMF dispersion of S1 to 40-80°C in a water bath and stirs, adds PVDF-b-PTFE powder, stirs until the particles are completely dissolved, and then adds acrylic copolymer and xylene to obtain a BTO-PVDF-b-PTFE mixed solution.

[0054] S3 puts the BTO-PVDF-b-PTFE mixed solution prepared in S2 into a vacuum oven for degassing for 2 to 4 hours to prepare a BTO-PVDF-b-PTFE thermal insulation coating.

[0055] Performance Testing

[0056] The ultraviolet and infrared transmittances of BTO-PVDF-b-PTFE thermal insulation coatings were tested by an optical transmittance meter. The thermal insulation performance of thermal insulation coatings was tested with reference to the standard JG / T 235-2014 "Architectural Reflective Thermal Insulation Coatings". The thermal conductivity of the coating was tested using a multifunctional rapid thermal conductivity tester (HotDisk method). The test results are shown in Table 1.

[0057] Table 1 Performance data of BTO-PVDF-b-PTFE thermal insulation coatings prepared in Examples 1-5

[0058]

[0059] It can be seen from Table 1 that the content of nano-barium titanate wet slurry and PVDF-b-PTFE has a great influence on the performance of thermal insulation coatings. Within the appropriate range, the higher the content of PVDF-b-PTFE, the lower the ultraviolet and infrared transmittance of the coating, and the better the thermal insulation performance; coating additives (including film-forming additives, leveling agents, thickeners, and defoaming agents) have a slight effect on coating performance and can be selected according to actual production requirements and economic costs.

[0060] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A BTO-PVDF-b-PTFE thermal insulation coating, characterized in that: The invention comprises, by mass fraction, 10-25% of nano-barium titanate wet slurry, 25-55% of PVDF-b-PTFE, 1-5% of coating additive and 15-50% of diluent.

2. A BTO-PVDF-b-PTFE thermal insulation coating according to claim 1, characterized in that: The solid content of the nano-barium titanate wet slurry is 10-30%, and the particle size range of the barium titanate nanoparticles in the nano-barium titanate wet slurry is 20-200nm.

3. A BTO-PVDF-b-PTFE thermal insulation coating according to claim 1, characterized in that: Coating additives include thickeners, film-forming additives, leveling agents, and defoaming agents.

4. A BTO-PVDF-b-PTFE thermal insulation coating according to claim 3, characterized in that: The thickener is polyacrylamide, the film-forming aid is a mixture of ethylene glycol monobutyl ether / dipropylene glycol butyl ether, the leveling agent is an acrylic copolymer, the defoaming agent is a mixture of non-silicone-containing hydrophobic particles and mineral oil, and the diluent is xylene.

5. A method for preparing the BTO-PVDF-b-PTFE thermal insulation coating according to any one of claims 1 to 4, characterized in that: The following steps are included: S1: dispersing barium titanate nanoparticles BTO in N,N-dimethylformamide, and vigorously stirring by ultrasonic vibration to obtain a BTO / DMF dispersion, i.e., nano-barium titanate wet slurry; S2: adding PVDF-b-PTFE powder to the BTO / DMF dispersion of S1 under heating and stirring conditions, stirring until the particles are completely dissolved, and then adding a coating additive and a diluent to obtain a BTO-PVDF-b-PTFE mixed solution; S3 puts the BTO-PVDF-b-PTFE mixed solution prepared in S2 into a vacuum oven for degassing to prepare a BTO-PVDF-b-PTFE thermal insulation coating.

6. The method for preparing a BTO-PVDF-b-PTFE thermal insulation coating according to claim 5, characterized in that: The heating in S2 is water bath heating, and the heating temperature is 40-80°C.

7. The method for preparing a BTO-PVDF-b-PTFE thermal insulation coating according to claim 5, characterized in that: The degassing time in S3 is 2 to 4 hours.

8. An application of the BTO-PVDF-b-PTFE thermal insulation coating according to any one of claims 1 to 4, characterized in that: Used in UV-IR protective coatings on car roofs.