Waterproof antibacterial agent for concrete surface and preparation method thereof
By modifying the combination of lignin microspheres and chitosan-Ag@SiO2 powder, superhydrophobic and antibacterial surfaces are formed, which solves the stability of cement-based materials under water and acid erosion, and achieves stable waterproof and antibacterial effects. , extends the service life of concrete.
Patent Information
- Application Number
- CN202410879282.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-02
AI Technical Summary
Existing cement-based materials are prone to cracking or falling off under the erosion of water and acidic attachments, and the existing waterproof and antibacterial properties are unstable and not long-lasting.
Modified lignin microspheres and chitosan-Ag@SiO2 powder are used as waterproof and antibacterial agents to form a superhydrophobic structure and a stable antibacterial surface through chemical modification, enhancing the waterproof and antibacterial properties of concrete.
It significantly improves the waterproof performance and antibacterial ability of the concrete surface, forms a stable hydrophobic coating, effectively inhibits bacterial adhesion and moisture invasion, and extends the service life of concrete.
Smart Images

Figure CN118909507A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete antibacterial agent, in particular to a waterproof antibacterial agent for concrete surface and a preparation method thereof. Background Art
[0002] Cement-based materials are one of the most widely used building materials at present. After construction, they are in contact with substances such as moisture and particulate matter in the air for a long time. These substances are easily adhered to the surface of the concrete structure. Combined with the erosion of rainwater, the surface of the concrete structure is eventually damaged, seriously affecting the functionality, durability and aesthetics of the concrete structure, and the cleaning and maintenance costs are high.
[0003] During the hydration process of cement, a large number of tiny pores and defects will be generated, and groups such as hydroxyl groups will be distributed on the surface, which makes cement-based materials highly hydrophilic. Therefore, the water on the surface of cement-based materials can be easily adsorbed into the interior of cement-based materials under capillary action, thus affecting their performance and durability. Especially in special environments, such as cold areas, the volume of water increases after freezing, which can cause the surface of cement-based materials to fall off or crack; in marine environments, a large number of sulfide bacteria in the water can attach to the surface of concrete structures, produce acidic metabolites, and cause premature failure of marine engineering concrete. Therefore, how to improve the waterproof and antibacterial properties of cement-based materials is of great significance to improving the performance and durability of cement-based structures.
[0004] For example, the patent with publication number CN113603427A discloses a microbial erosion resistant protective concrete and its preparation method, the concrete includes cement, coarse aggregate, fine aggregate, powder, water, polycarboxylic acid water reducer, corrosion inhibitor and antibacterial particles, wherein hydroxypropyl chitosan is introduced into the corrosion inhibitor, and the antibacterial particles include silver nitrate, copper nitrate, nano silicon dioxide and polyvinyl alcohol powder. By introducing a variety of substances with different functions for compounding, more functional effects can be given to the concrete.
[0005] However, the existing method of improving concrete by mixing and compounding multiple components as mentioned above has limited waterproof and antibacterial effects in actual use, and the waterproof and antibacterial properties are unstable and not lasting. Summary of the invention
[0006] The technical problems to be solved by the present invention are:
[0007] In order to solve the problem that the surface of cement-based structures is easily cracked or peeled off due to the erosion of water and acidic attachments, the current method is to introduce substances with strong waterproof or antibacterial effects into concrete and its additives for mixing and compounding, so that the cement-based structures can maintain certain waterproof and antibacterial properties during use. However, this treatment method has the problem that the waterproof and antibacterial properties are unstable and not durable.
[0008] The technical solution adopted by the present invention is:
[0009] The invention provides a waterproof and antibacterial agent for concrete surface, comprising modified lignin microspheres, chitosan-Ag@SiO2 powder and a resin base material; the modified lignin microspheres are microspheres containing super hydrophobic structures formed by covalent bonding of alkyl trichlorosilane and lignin.
[0010] Preferably, the method for preparing the modified lignin microspheres comprises the following steps:
[0011] A1 preparation of lignin microspheres;
[0012] A2: placing lignin microspheres in a solvent, adding water, stirring and dispersing; then adding alkyl trichlorosilane, reacting, washing and drying, to obtain the modified lignin microspheres.
[0013] Preferably, the preparation method of step A1 comprises the following steps:
[0014] The lignin is placed in a valerolactone aqueous solution, deionized water is injected to produce lignin nanospheres, and the lignin microspheres are obtained by dialyzing, centrifuging, and freeze-drying.
[0015] Preferably, the particle size of the lignin nanospheres is 45-60 nm.
[0016] Preferably, the chitosan-Ag@SiO2 powder is a powder particle with SiO2 as a core material and chitosan as a shell material, and silver ions are deposited on the surface of chitosan by chelation.
[0017] Preferably, the method for preparing the chitosan-Ag@SiO2 powder comprises the following steps:
[0018] B1 prepares alkaline precursor solution and reaction base solution containing chitosan respectively;
[0019] B2 introduces the reaction base liquid into the alkaline precursor solution, stirs to produce a precipitate; after washing the precipitate, disperses it in distilled water, adds silver nitrate and sodium borohydride, stirs to react, washes and dries, and powders to obtain the chitosan-Ag@SiO2 powder.
[0020] Preferably, the alkaline precursor solution comprises aqueous ammonia, anhydrous ethanol and water.
[0021] Preferably, the reaction base liquid comprises chitosan, tetraethyl orthosilicate and ethanol.
[0022] Preferably, the amount ratio of the modified lignin microspheres to the chitosan-Ag@SiO2 powder is 0.8-2.5:1 by mass.
[0023] A method for preparing the waterproof antibacterial agent for concrete surface comprises the following steps:
[0024] The modified lignin microspheres and chitosan-Ag@SiO2 powder are added to an organic solvent and dispersed evenly, and then a resin base material and a curing agent are added under stirring, and stirred and mixed to obtain the waterproof and antibacterial agent.
[0025] The beneficial effects of the present invention are as follows:
[0026] The present invention can provide protection through a coating without changing the technology of existing cement-based materials. It is direct, convenient and applicable to existing concrete structures. The waterproof and antibacterial agent provided by the present invention can be applied to concrete and its surface coating, effectively enhancing the ability of concrete to resist water intrusion and improving the service performance of the structure. Specifically, alkyl trichlorosilane is used to modify lignin to form a super-hydrophobic structure through chemical modification, and micro-needle-shaped nipples and surface wax crystal modifications are constructed on the rough surface to achieve a waterproof effect of the super-hydrophobic surface; chitosan-Ag@SiO2 powder can inhibit the adhesion of bacteria on the surface of cement-based materials on the basis of long-term stability of the structure, thereby exerting good antibacterial properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The bacterial morphology of the culture medium treated with the waterproof antibacterial agent in Example 2;
[0028] Figure 2 The bacterial morphology of the culture medium treated with the waterproof antibacterial agent in Example 3;
[0029] Figure 3 The bacterial morphology of the culture medium treated with the waterproof antibacterial agent in Example 5;
[0030] Figure 4 The bacterial morphology of the culture medium treated with the waterproof antibacterial agent in Example 6;
[0031] Figure 5 This is a bacterial morphology diagram of a culture medium that has not been treated with the waterproof antibacterial agent of the present invention;
[0032] Figure 6 This is a bacterial morphology diagram of a cement-based material block treated with the waterproof antibacterial agent in Example 2;
[0033] Figure 7 This is a bacterial morphology diagram of a cement-based material block treated with the waterproof antibacterial agent in Example 3;
[0034] Figure 8 This is a bacterial morphology diagram of a cement-based material block treated with the waterproof antibacterial agent in Example 5;
[0035] Fig. 9 This is a bacterial morphology diagram of a cement-based material block treated with the waterproof antibacterial agent in Example 6;
[0036] Fig.10 This is a bacterial morphology diagram of a cement-based material block that has not been treated with the waterproof and antibacterial agent of the present invention. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0038] The invention provides a waterproof antibacterial agent for concrete surface. The raw materials for preparing the waterproof antibacterial agent include epoxy resin, curing agent, modified lignin microspheres and chitosan-Ag@SiO2 powder. The epoxy resin is used as a matrix material and the curing agent can be selected from diethylenetriamine and the like.
[0039] In the present invention, the preparation method of modified lignin microspheres comprises the following steps:
[0040] (1) dissolving lignin in a valerolactone aqueous solution, and then rapidly injecting deionized water to produce lignin nanospheres with an average diameter of 45-60 nm; placing the lignin nanospheres into a dialysis bag, dialyzing for 5-8 days, centrifuging, and freeze-drying for 10-15 hours to obtain lignin microspheres;
[0041] (2) placing the lignin microspheres in anhydrous ethanol, dispersing them, adding deionized water, stirring at high speed for 20-45 minutes, and then adding alkyltrichlorosilane to react for about 1-3 hours. The product obtained by the reaction was washed three times with anhydrous ethanol to remove the residual alkyltrichlorosilane and other modified impurities, and placed in a vacuum dryer at 50-80° C. for 10-15 hours to obtain hydrophobically modified lignin microspheres;
[0042] The alkyltrichlorosilane may be methyltrichlorosilane and / or hexyltrichlorosilane.
[0043] In the present invention, alkyl trichlorosilane is used to modify lignin so that it forms a super hydrophobic structure through chemical modification. The chemical modification process is shown in the following reaction formula (1):
[0044] Chemical formula (1).
[0045] In the present invention, the preparation method of chitosan-Ag@SiO2 powder comprises the following steps:
[0046] (1) Concentrated ammonia water, anhydrous ethanol and pure water are mixed and mechanically stirred for 3-15 minutes to obtain an alkaline precursor solution; a mixed solution of tetraethyl orthosilicate and ethanol is prepared, and chitosan is added and ultrasonically dispersed for 5-20 minutes to ensure that the chitosan is evenly dispersed in the mixed solution to obtain a reaction base solution;
[0047] (2) The reaction base liquid is quickly poured into the alkaline precursor solution, and stirred at a speed of 600-800 r / min for 2-5 hours to form a chitosan@SiO2 precipitate; the chitosan@SiO2 precipitate is dispersed in distilled water, and washed alternately with anhydrous ethanol and distilled water, and then the chitosan@SiO2 precipitate is dispersed in distilled water, silver nitrate is added, and stirred evenly, and a trace amount of sodium borohydride solution is added, stirred, washed, dried, and powdered to obtain chitosan-Ag@SiO2 powder.
[0048] In the present invention, chitosan in the chitosan-Ag@SiO2 powder serves as an intermediate, which can well wrap silicon dioxide on the one hand, and chelate with silver ions on the other hand to make its structural connection more stable, thereby making the effect of the waterproof and antibacterial agent more stable.
[0049] The present invention also provides a method for preparing a waterproof and antibacterial agent for concrete surface, comprising the following steps:
[0050] The modified lignin microspheres and chitosan-Ag@SiO2 powder are added to anhydrous ethanol at a mass ratio of 0.8-2.5:1, ultrasonically dispersed, stirred, and epoxy resin and curing agent are added under stirring, and stirring is continued until the mixture is uniform to obtain a waterproof and antibacterial agent.
[0051] Example 1
[0052] Step 1: Add 18 mL of 28% concentrated ammonia water, 32 mL of anhydrous ethanol and 50 mL of pure water to a three-necked flask, mix and stir for 5 minutes to obtain an alkaline precursor solution; prepare 100 mL of a mixture of tetraethyl orthosilicate and ethanol in a volume ratio of 9:91, add 0.5 g of chitosan thereto, ultrasonically treat for 10 minutes, and then quickly pour it into the three-necked flask with the alkaline precursor solution, stir continuously at a speed of 600 r / min for 3 hours, and then wash it alternately with anhydrous ethanol and distilled water three times; disperse the obtained precipitate in distilled water, add 0.2 g of silver nitrate, stir evenly, add a trace amount of sodium borohydride solution, wash and dry, make it into powder, and obtain chitosan-Ag@SiO2 powder.
[0053] Step 2: Take 40 mg of lignin, dissolve it in 2 mL of 90% valerolactone aqueous solution, and then quickly inject deionized water to produce lignin nanospheres with an average diameter of about 55 nm; place the lignin nanospheres in a dialysis bag, dialyze for 7 days, centrifuge, and freeze-dry for 12 hours to obtain lignin microspheres; disperse the lignin microspheres in 100 mL of anhydrous ethanol, add 0.5 mL of deionized water, stir rapidly for 30 minutes, and then add 0.15 g of methyltrichlorosilane and react for 2 hours; the reaction product is washed three times with anhydrous ethanol, and then placed at 60°C for vacuum drying for 12 hours to obtain modified lignin microspheres.
[0054] Step 3: Mix chitosan-Ag@SiO2 powder and modified lignin microspheres in a mass ratio of 1:1 in anhydrous ethanol, ultrasonically disperse for 30 minutes, and stir for 50 minutes, then add 7g epoxy resin and 0.07g diethylenetriamine, continue stirring, and mix evenly to obtain a waterproof and antibacterial agent.
[0055] Example 2
[0056] Step 1: Add 18 mL of 28% concentrated ammonia water, 32 mL of anhydrous ethanol and 50 mL of pure water to a three-necked flask, mix and stir for 5 minutes to obtain an alkaline precursor solution; prepare 100 mL of a mixture of tetraethyl orthosilicate and ethanol in a volume ratio of 9:91, add 0.5 g of chitosan thereto, ultrasonically treat for 10 minutes, and then quickly pour it into the three-necked flask with the alkaline precursor solution, stir continuously at a speed of 600 r / min for 3 hours, and then wash it alternately with anhydrous ethanol and distilled water three times; disperse the obtained precipitate in distilled water, add 0.3 g of silver nitrate, stir evenly, add a trace amount of sodium borohydride solution, wash and dry, make it into powder, and obtain chitosan-Ag@SiO2 powder.
[0057] Step 2: Take 40 mg of lignin, dissolve it in 2 mL of 90% valerolactone aqueous solution, and then quickly inject deionized water to produce lignin nanospheres with an average diameter of about 55 nm; place the lignin nanospheres in a dialysis bag, dialyze for 7 days, centrifuge, and freeze-dry for 12 hours to obtain lignin microspheres; disperse the lignin microspheres in 100 mL of anhydrous ethanol, add 0.5 mL of deionized water, stir rapidly for 30 minutes, and then add 0.30 g of methyltrichlorosilane and react for 2 hours; the reaction product is washed three times with anhydrous ethanol, and then placed at 60°C for vacuum drying for 12 hours to obtain modified lignin microspheres.
[0058] Step 3: Mix chitosan-Ag@SiO2 powder and modified lignin microspheres in a mass ratio of 1:1 in anhydrous ethanol, ultrasonically disperse for 30 minutes, and stir for 50 minutes, then add 7g epoxy resin and 0.07g diethylenetriamine, continue stirring, and mix evenly to obtain a waterproof and antibacterial agent.
[0059] Example 3
[0060] Step 1: Add 18 mL of 28% concentrated ammonia water, 32 mL of anhydrous ethanol and 50 mL of pure water to a three-necked flask, mix and stir for 5 minutes to obtain an alkaline precursor solution; prepare 100 mL of a mixture of tetraethyl orthosilicate and ethanol in a volume ratio of 9:91, add 0.5 g of chitosan thereto, ultrasonically treat for 10 minutes, and then quickly pour it into the three-necked flask with the alkaline precursor solution, stir continuously at a speed of 600 r / min for 3 hours, and then wash it alternately with anhydrous ethanol and distilled water three times; disperse the obtained precipitate in distilled water, add 0.3 g of silver nitrate, stir evenly, add a trace amount of sodium borohydride solution, wash and dry, make it into powder, and obtain chitosan-Ag@SiO2 powder.
[0061] Step 2: Take 40 mg of lignin, dissolve it in 2 mL of 90% valerolactone aqueous solution, and then quickly inject deionized water to produce lignin nanospheres with an average diameter of about 55 nm; place the lignin nanospheres in a dialysis bag, dialyze for 7 days, centrifuge, and freeze-dry for 12 hours to obtain lignin microspheres; disperse the lignin microspheres in 100 mL of anhydrous ethanol, add 0.5 mL of deionized water, stir rapidly for 30 minutes, and then add 0.30 g of methyltrichlorosilane and react for 2 hours; the reaction product is washed three times with anhydrous ethanol, and then placed at 60°C for vacuum drying for 12 hours to obtain modified lignin microspheres.
[0062] Step 3: Mix chitosan-Ag@SiO2 powder and modified lignin microspheres in a mass ratio of 2:1 in anhydrous ethanol, ultrasonically disperse for 30 minutes, and stir for 50 minutes, then add 7g epoxy resin and 0.07g diethylenetriamine, continue stirring, and mix evenly to obtain a waterproof and antibacterial agent.
[0063] Example 4
[0064] Step 1: Add 18 mL of 28% concentrated ammonia water, 32 mL of anhydrous ethanol and 50 mL of pure water to a three-necked flask, mix and stir for 5 minutes to obtain an alkaline precursor solution; prepare 100 mL of a mixture of tetraethyl orthosilicate and ethanol in a volume ratio of 9:91, add 0.5 g of chitosan thereto, ultrasonically treat for 10 minutes, and then quickly pour it into the three-necked flask with the alkaline precursor solution, stir continuously at a speed of 600 r / min for 3 hours, and then wash it alternately with anhydrous ethanol and distilled water three times; disperse the obtained precipitate in distilled water, add 0.2 g of silver nitrate, stir evenly, add a trace amount of sodium borohydride solution, wash and dry, make it into powder, and obtain chitosan-Ag@SiO2 powder.
[0065] Step 2: Take 40 mg of lignin, dissolve it in 2 mL of 90% valerolactone aqueous solution, and then quickly inject deionized water to produce lignin nanospheres with an average diameter of about 55 nm; place the lignin nanospheres in a dialysis bag, dialyze for 7 days, centrifuge, and freeze-dry for 12 hours to obtain lignin microspheres; disperse the lignin microspheres in 100 mL of anhydrous ethanol, add 0.5 mL of deionized water, stir rapidly for 30 minutes, and then add 0.15 g of hexyltrichlorosilane and react for 2 hours; the reaction product is washed three times with anhydrous ethanol, and then placed at 60°C for vacuum drying for 12 hours to obtain modified lignin microspheres.
[0066] Step 3: Mix chitosan-Ag@SiO2 powder and modified lignin microspheres in a mass ratio of 1:1 in anhydrous ethanol, ultrasonically disperse for 30 minutes, and stir for 50 minutes, then add 7g epoxy resin and 0.07g diethylenetriamine, continue stirring, and mix evenly to obtain a waterproof and antibacterial agent.
[0067] Example 5
[0068] Step 1: Add 18 mL of 28% concentrated ammonia water, 32 mL of anhydrous ethanol and 50 mL of pure water to a three-necked flask, mix and stir for 5 minutes to obtain an alkaline precursor solution; prepare 100 mL of a mixture of tetraethyl orthosilicate and ethanol in a volume ratio of 9:91, add 0.3 g of chitosan thereto, ultrasonically treat for 10 minutes, and then quickly pour it into the three-necked flask with the alkaline precursor solution, stir continuously at a speed of 600 r / min for 3 hours, and then wash it alternately with anhydrous ethanol and distilled water three times; disperse the obtained precipitate in distilled water, add 0.2 g of silver nitrate, stir evenly, add a trace amount of sodium borohydride solution, wash and dry, make it into powder, and obtain chitosan-Ag@SiO2 powder.
[0069] Step 2: Take 40 mg of lignin, dissolve it in 2 mL of 90% valerolactone aqueous solution, and then quickly inject deionized water to produce lignin nanospheres with an average diameter of about 55 nm; place the lignin nanospheres in a dialysis bag, dialyze for 7 days, centrifuge, and freeze-dry for 12 hours to obtain lignin microspheres; disperse the lignin microspheres in 100 mL of anhydrous ethanol, add 0.5 mL of deionized water, stir rapidly for 30 minutes, and then add 0.15 g of hexyltrichlorosilane and react for 2 hours; the reaction product is washed three times with anhydrous ethanol, and then placed at 60°C for vacuum drying for 12 hours to obtain modified lignin microspheres.
[0070] Step 3: Mix chitosan-Ag@SiO2 powder and modified lignin microspheres in a mass ratio of 1:1 in anhydrous ethanol, ultrasonically disperse for 30 minutes, and stir for 50 minutes, then add 7g epoxy resin and 0.07g diethylenetriamine, continue stirring, and mix evenly to obtain a waterproof and antibacterial agent.
[0071] Example 6
[0072] Step 1: Add 18 mL of 28% concentrated ammonia water, 32 mL of anhydrous ethanol and 50 mL of pure water to a three-necked flask, mix and stir for 5 minutes to obtain an alkaline precursor solution; prepare 100 mL of a mixture of tetraethyl orthosilicate and ethanol in a volume ratio of 9:91, add 0.5 g of chitosan thereto, ultrasonically treat for 10 minutes, and then quickly pour it into the three-necked flask with the alkaline precursor solution, stir continuously at a speed of 600 r / min for 3 hours, and then wash it alternately with anhydrous ethanol and distilled water three times; disperse the obtained precipitate in distilled water, add 0.3 g of silver nitrate, stir evenly, add a trace amount of sodium borohydride solution, wash and dry, make it into powder, and obtain chitosan-Ag@SiO2 powder.
[0073] Step 2: Take 40 mg of lignin, dissolve it in 2 mL of 90% valerolactone aqueous solution, and then quickly inject deionized water to produce lignin nanospheres with an average diameter of about 55 nm; place the lignin nanospheres in a dialysis bag, dialyze for 7 days, centrifuge, and freeze-dry for 12 hours to obtain lignin microspheres; disperse the lignin microspheres in 100 mL of anhydrous ethanol, add 0.5 mL of deionized water, stir rapidly for 30 minutes, and then add 0.30 g of methyltrichlorosilane and react for 2 hours; the reaction product is washed three times with anhydrous ethanol, and then placed at 60°C for vacuum drying for 12 hours to obtain modified lignin microspheres.
[0074] Step 3: Mix chitosan-Ag@SiO2 powder and modified lignin microspheres in a mass ratio of 2:1 in anhydrous ethanol, ultrasonically disperse for 30 minutes, and stir for 50 minutes, then add 7g epoxy resin and 0.07g diethylenetriamine, continue stirring, and mix evenly to obtain a waterproof and antibacterial agent.
[0075] Comparative Example 1
[0076] Step 2: Take 40 mg of lignin, dissolve it in 2 mL of 90% valerolactone aqueous solution, and then quickly inject deionized water to produce lignin nanospheres with an average diameter of about 55 nm; place the lignin nanospheres in a dialysis bag, dialyze for 7 days, centrifuge, and freeze-dry for 12 hours to obtain lignin microspheres; disperse the lignin microspheres in 100 mL of anhydrous ethanol, add 0.5 mL of deionized water, stir rapidly for 30 minutes, and then add 0.15 g of methyltrichlorosilane and react for 2 hours; the reaction product is washed three times with anhydrous ethanol, and then placed at 60°C for vacuum drying for 12 hours to obtain modified lignin microspheres.
[0077] Step 2: Mix 0.5g chitosan, 0.15g silver nitrate, and 2.6g silica, and take an equal mass of modified lignin microspheres, place them together in anhydrous ethanol, ultrasonically disperse for 30 minutes, and stir for 50 minutes, then add 7g epoxy resin and 0.07g diethylenetriamine, continue stirring, and mix evenly to obtain a waterproof antibacterial agent.
[0078] Comparative Example 2
[0079] Step 2: Take 40 mg of lignin, dissolve it in 2 mL of 90% valerolactone aqueous solution, and then quickly inject deionized water to produce lignin nanospheres with an average diameter of about 55 nm; place the lignin nanospheres in a dialysis bag, dialyze for 7 days, centrifuge, and freeze-dry for 12 hours to obtain lignin microspheres; disperse the lignin microspheres in 100 mL of anhydrous ethanol, add 0.5 mL of deionized water, stir rapidly for 30 minutes, and then add 0.15 g of methyltrichlorosilane and react for 2 hours; the reaction product is washed three times with anhydrous ethanol, and then placed at 60°C for vacuum drying for 12 hours to obtain modified lignin microspheres.
[0080] Step 2: Place about 3.4 g of modified lignin microspheres in anhydrous ethanol, ultrasonically disperse for 30 min, and stir for 50 min, then add 7 g of epoxy resin and 0.07 g of diethylenetriamine, continue stirring, and mix evenly to obtain a waterproof and antibacterial agent.
[0081] Comparative Example 3
[0082] Step 1: Add 18 mL of 28% concentrated ammonia water, 32 mL of anhydrous ethanol and 50 mL of pure water to a three-necked flask, mix and stir for 5 minutes to obtain an alkaline precursor solution; prepare 100 mL of a mixture of tetraethyl orthosilicate and ethanol in a volume ratio of 9:91, add 0.5 g of chitosan thereto, ultrasonically treat for 10 minutes, and then quickly pour it into the three-necked flask with the alkaline precursor solution, stir continuously at a speed of 600 r / min for 3 hours, and then wash it alternately with anhydrous ethanol and distilled water three times; disperse the obtained precipitate in distilled water, add 0.2 g of silver nitrate, stir evenly, add a trace amount of sodium borohydride solution, wash and dry, make it into powder, and obtain chitosan-Ag@SiO2 powder.
[0083] Step 2: Take 40 mg of lignin, dissolve it in 2 mL of 90% valerolactone aqueous solution, and then quickly inject deionized water to produce lignin nanospheres with an average diameter of about 55 nm; place the lignin nanospheres in a dialysis bag, dialyze for 7 days, centrifuge, and freeze-dry for 12 hours to obtain lignin microspheres.
[0084] Step 3: Mix chitosan-Ag@SiO2 powder and lignin microspheres in a mass ratio of 1:1 in anhydrous ethanol, ultrasonically disperse for 30 minutes, and stir for 50 minutes, then add 7g epoxy resin and 0.07g diethylenetriamine, continue stirring, and mix evenly to obtain a waterproof and antibacterial agent.
[0085] Comparative Example 4
[0086] Step 1: Add 18 mL of 28% concentrated ammonia water, 32 mL of anhydrous ethanol and 50 mL of pure water to a three-necked flask, mix and stir for 5 minutes to obtain an alkaline precursor solution; prepare 100 mL of a mixture of tetraethyl orthosilicate and ethanol in a volume ratio of 9:91, add 0.5 g of chitosan thereto, ultrasonically treat for 10 minutes, and then quickly pour it into the three-necked flask with the alkaline precursor solution, stir continuously at a speed of 600 r / min for 3 hours, and then wash it alternately with anhydrous ethanol and distilled water three times; disperse the obtained precipitate in distilled water, add 0.2 g of silver nitrate, stir evenly, add a trace amount of sodium borohydride solution, wash and dry, make it into powder, and obtain chitosan-Ag@SiO2 powder.
[0087] Step 2: Place the chitosan-Ag@SiO2 powder in anhydrous ethanol, ultrasonically disperse for 30 minutes, and stir for 50 minutes, then add 7g of epoxy resin and 0.07g of diethylenetriamine, continue stirring, and mix evenly to obtain a waterproof and antibacterial agent.
[0088] <Test example>
[0089] Samples: Examples 1-6, Comparative Examples 1-4
[0090] Take a plurality of cement-based material blocks, and coat the surfaces of the blocks with the waterproof and antibacterial agents of Examples 1-6 and Comparative Examples 1-4 twice, with each coating amount of 600 g / m 2 The interval between the two coatings is 3 hours. The next coating is carried out after the waterproof antibacterial agent is completely absorbed and dried. After the coating is completed, the surface is cleaned with a soft brush. The cement-based material block coated with the waterproof antibacterial agent is subjected to the following test:
[0091] (1) Waterproof performance test
[0092] The contact angles at different positions on the surface of the treated cement-based material block were measured using a static contact angle meter. The static contact angle was measured using the hanging drop method. Five areas were measured and the average value was taken as the test result. The test results are shown in Table 1 below:
[0093] Table 1 Contact angle test results of different samples
[0094] Static contact angle (°) Example 1 158.58 Example 2 163.83 Example 3 163.61 Example 4 156.16 Example 5 158.77 Example 6 158.68 Comparative Example 1 153.12 Comparative Example 2 150.74 Comparative Example 3 147.96 Comparative Example 4 148.50
[0095] It can be seen from Table 1 that after the surface of the cement-based material block is coated with the waterproof and antibacterial agent in Example 1 to Example 6 to form a coating, the contact angle of the surface is significantly greater than the contact angle of the cement-based material block treated with the waterproof and antibacterial agent in Comparative Examples 1 to Comparative Examples 4, indicating that the waterproof and antibacterial agent of the present invention can give the cement-based material surface a good waterproof effect.
[0096] (2) Antibacterial performance and antibacterial adhesion performance test
[0097] Take 200 μL of undiluted composite bacterial suspension with Bacillus as the dominant bacteria, inoculate them in multiple culture media respectively, and then drop 0 and 100 μL of the waterproof antibacterial agent of Example 2, 100 μL of the waterproof antibacterial agent of Example 3, 100 μL of the waterproof antibacterial agent of Example 5, and 100 μL of the waterproof antibacterial agent of Example 6 in sequence, and the culture medium without addition is used as a blank control; the above culture medium is placed in a constant temperature incubator and cultured for 48 hours, and the growth of bacteria is observed after taking it out; and a blank cement-based material block and a cement-based material block treated with a waterproof antibacterial agent are placed in a composite bacterial solution with Bacillus as the dominant bacteria and cultured for 15 days, taken out after 15 days, and the bacteria not attached to the surface are washed with sterile saline, and the bacteria on the surface of the material are observed.
[0098] like Figures 1 to 4 The bacterial morphology of the culture dishes after being treated by Example 2, Example 3, Example 5, and Example 6 are shown respectively. Figure 5 This is a bacterial morphology diagram of a culture dish that has not been treated with the waterproof antibacterial agent of the present invention; Figures 6 to 9 The bacterial morphology of the cement-based material block surface after being treated by Example 2, Example 3, Example 5, and Example 6, respectively. Fig.10 This is a bacterial morphology diagram on the surface of a cement-based material block that has not been treated with the waterproof and antibacterial agent of the present invention.
[0099] By comparison, it can be found that the bacteria in the culture medium after treatment with the waterproof antibacterial agent are significantly lower, and there is obvious biofilm adhesion on the surface of the cement-based material block that has not been treated with the waterproof antibacterial agent, while there is no obvious sign of bacterial growth on the surface of the cement-based material block coated with the waterproof antibacterial agent, indicating that the waterproof antibacterial agent of the present invention can effectively inhibit the growth of bacteria in cement-based materials, and has good antibacterial properties and antibacterial adhesion properties, among which the antibacterial effects of Examples 3 and 6 with high chitosan and Ag content are more significant.
[0100] In summary, the waterproof antibacterial agent prepared in Examples 1 to 6 not only has outstanding advantages in waterproof performance, but also forms a super-hydrophobic structure on the surface of the cement-based material block to achieve a significant hydrophobic and waterproof effect, and also shows an effective effect of inactivating bacteria in terms of antibacterial performance and antibacterial adhesion performance. This shows that the waterproof antibacterial agent provided by the present invention can indeed exert a good waterproof and antibacterial effect, and the effect is significant and stable.
[0101] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A waterproof and antibacterial agent for concrete surface, characterized in that: It includes modified lignin microspheres, chitosan-Ag@SiO2 powder and resin base; The modified lignin microspheres are microspheres containing super hydrophobic structures formed by covalent bonding of alkyl trichlorosilane and lignin.
2. The waterproof and antibacterial agent for concrete surface according to claim 1, characterized in that: The preparation method of the modified lignin microspheres comprises the following steps: A1 preparation of lignin microspheres; A2: placing lignin microspheres in a solvent, adding water, stirring and dispersing; then adding alkyl trichlorosilane, reacting, washing and drying, to obtain the modified lignin microspheres.
3. The waterproof and antibacterial agent for concrete surface according to claim 2, characterized in that: The preparation method of step A1 comprises the following steps: The lignin is placed in a valerolactone aqueous solution, deionized water is injected to generate lignin nanospheres, and the lignin microspheres are obtained by dialyzing, centrifuging, and freeze-drying.
4. The waterproof and antibacterial agent for concrete surface according to claim 3, characterized in that: The particle size of the lignin nanospheres is 45-60 nm.
5. The waterproof and antibacterial agent for concrete surface according to any one of claims 1 to 4, characterized in that: The chitosan-Ag@SiO2 powder is a powder particle with SiO2 as a core material and chitosan as a shell material, and silver ions are deposited on the surface of chitosan through chelation.
6. The waterproof and antibacterial agent for concrete surface according to claim 5, characterized in that: The preparation method of the chitosan-Ag@SiO2 powder comprises the following steps: B1 prepares alkaline precursor solution and reaction base solution containing chitosan respectively; B2 introduces the reaction base liquid into the alkaline precursor solution, stirs to produce a precipitate; after washing the precipitate, disperses it in distilled water, adds silver nitrate and sodium borohydride, stirs to react, washes and dries, and powders to obtain the chitosan-Ag@SiO2 powder.
7. The waterproof and antibacterial agent for concrete surface according to claim 5, characterized in that: The alkaline precursor solution includes ammonia water, anhydrous ethanol and water.
8. The waterproof and antibacterial agent for concrete surface according to claim 5, characterized in that: The reaction base liquid includes chitosan, tetraethyl orthosilicate and ethanol.
9. The waterproof and antibacterial agent for concrete surface according to claim 1, characterized in that: The amount ratio of the modified lignin microspheres to the chitosan-Ag@SiO2 powder is 0.8-2.5:1 by mass.
10. A method for preparing the waterproof and antibacterial agent for concrete surface according to any one of claims 1 to 9, characterized in that: The steps include: The modified lignin microspheres and chitosan-Ag@SiO2 powder are added to an organic solvent and dispersed evenly, and then a resin base material and a curing agent are added under stirring, and stirred and mixed to obtain the waterproof and antibacterial agent.
Citation Information
Patent Citations
Preparation of silver-loaded silica-chitosan compound anti-bacteria agent
CN101297654A
Lignin / silver composite antibacterial agent, and preparation method and application thereof
CN107312315A
Preparation method of lignin grafted polymer microspheres
CN112979928A
SiO2 hydrosol-based antibacterial agent as well as preparation method and application thereof
CN113907090A
Preparation method of lignin micro-nanospheres with adjustable size
CN116731350A