Spraying liquid vehicle cover film composition, spraying vehicle cover film and preparation method of spraying liquid vehicle cover film
Through the combination of isocyanate prepolymer, imine resin and polyaspartic acid ester resin, combined with alicyclic structure and topcoat layer, the problems of slow drying speed and low mechanical properties of sprayed car coat film coating are solved, and the problem of The coating with high adhesion, good peeling and mechanical strength improves the convenience of changing the car coat film and decorative effect.
Patent Information
- Application Number
- CN202410960301.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-17
AI Technical Summary
The water-based polyurethane in existing sprayed car coated film coatings has problems such as slow drying speed, low strength and poor water resistance. The cross-linking and curing speed of aromatic sprayed polyurea leads to poor surface effect. The sterically hindered secondary amine aspartate polyurea The coating has low mechanical properties and is difficult to peel off the whole sheet.
The composition of isocyanate prepolymer, imine resin and polyaspartic acid ester resin is adopted to introduce alicyclic structure through hydrolysis and curing reaction, adjust the reaction speed and mechanical properties, and form a high-strength and high-elongation coating. And add a topcoat layer to the coating to improve gloss and hardness.
The coating is achieved with high adhesion, good peeling and mechanical strength, simplifying the process of changing the car coating film, and improving the coating's weather resistance and gloss.
Smart Images

Figure BDA0004950065700000191 
Figure BDA0004950065700000201 
Figure BDA0004950065700000202
Abstract
Description
Technical Field
[0001] The present application relates to the field of spray-coated car cover films, and more specifically, to a spray-coated liquid car cover film composition, a spray-coated car cover film and a preparation method thereof. Background Art
[0002] Car film is a polymer film used to protect the car body. It is usually made of polyurethane, polyethylene, polyvinyl chloride and other materials. It has the characteristics of wear resistance, scratch resistance, UV resistance and pollution resistance. Car film can be attached to the surface of the car body to form a protective layer, effectively preventing the paint from being damaged by external factors while maintaining the gloss of the car body. In addition, car film can also be customized with different colors and patterns according to needs to add personalized elements to the car body.
[0003] Traditional car film generally needs to be prefabricated in the factory. The general process is: masterbatch melting → cast film → adhesive backing process → coating process. Not only is the process complicated and costly, but the car film needs to be sold in the form of a whole roll, which is pasted on the car body and then cut, which is relatively wasteful. In addition, the process of pasting car film is long, and it also requires high skills from the workers. It is very easy to cause bulging, delamination, etc. due to operational problems. Therefore, more and more people are beginning to use spray car film instead of traditional factory prefabricated film.
[0004] At present, the coatings used for spray-on car film mostly use water-based polyurethane as the main component, but they usually have problems such as slow drying speed, low strength, and poor water resistance. Polyurea is a type of polymer compound generated by the reaction of isocyanate components and amino compound components. It has gradually attracted people's attention because of its good anti-corrosion, waterproof, wear-resistant, and aging-resistant properties. People have found that using polyurea instead of water-based polyurethane can make the performance of spray-on car film better in all aspects.
[0005] Commonly used polyureas include aromatic spray polyurea and hindered secondary amine aspartic acid ester polyurea. However, these two types of polyurea have the following problems: Spray polyurea uses aromatic amino components and isocyanate to crosslink and cure after spraying. Due to the extremely fast reaction speed, the coating is cured before it has time to wet the inside of the substrate. The resulting coating has poor surface effect, low adhesion, and poor weather resistance, and cannot be directly used on civilian car cover films; and although hindered secondary amine aspartic acid ester polyurea has a moderate curing speed and good adhesion, the resulting coating has low mechanical properties such as tensile strength and tear strength, making it difficult to peel off the coating as a whole, and the peelability is poor, affecting the convenience of replacing the car cover film. Summary of the invention
[0006] In order to solve the above technical problems, the present application provides a sprayable liquid car cover film composition, a sprayable car cover film and a preparation method thereof.
[0007] In the first aspect, the present application provides a sprayable liquid car cover film composition, which adopts the following technical solution: A sprayable liquid car cover film composition comprises a component A and a component B. In parts by weight, the raw materials used in component A comprise 10-40 parts of isocyanate prepolymer; the raw materials used in component B comprise 5-20 parts of imide resin and 0-20 parts of polyaspartic acid ester resin; the isocyanate prepolymer is selected from aliphatic isocyanate prepolymer and / or alicyclic isocyanate elastic prepolymer; the imide resin is selected from aliphatic imide resin and / or alicyclic imide resin; the polyaspartic acid ester resin is selected from aliphatic polyaspartic acid ester resin and / or alicyclic polyaspartic acid ester resin; and, when component A and component B are mixed for use, at least one of the isocyanate prepolymer, imide resin and polyaspartic acid ester resin contains an alicyclic structure.
[0008] Optionally, the aliphatic isocyanate elastic prepolymer is obtained by polymerizing an aliphatic isocyanate monomer with at least one of a polyol and a polyaspartic acid ester resin.
[0009] Optionally, the aliphatic isocyanate monomer is at least one selected from hexamethylene diisocyanate, hexamethylene diisocyanate trimer, 1,5-pentamethylene diisocyanate, 1,5-pentamethylene diisocyanate trimer and trimethylhexamethylene diisocyanate.
[0010] Optionally, the polyol includes a diol, and the average molecular weight of the diol is 62-3000.
[0011] More specifically, the diol is selected from at least one of polyester diol, polycaprolactone diol, polycarbonate diol, polytetrahydrofuran diol, and a chain aliphatic diol having 1 to 18 carbon atoms. To further optimize certain properties of the isocyanate prepolymer, other alcohols other than the diol may be added to the polyol as a molecular weight regulator, a functionality regulator, or a chain extender.
[0012] The aliphatic isocyanate elastic prepolymer is prepared by the following method: the reaction raw materials are kept at a temperature of 60-90° C. for 5-9 hours to obtain an aliphatic isocyanate elastic prepolymer with an NCO content of 2-10%. The polymerization reaction may also selectively add a solvent, and the selectively added solvent is referred to as the first solvent in this application. The polymerization reaction may also selectively add a catalyst to assist the polymerization reaction, and the selectively added catalyst is referred to as the first catalyst in this application.
[0013] Optionally, the first solvent is selected from one of an alkane organic solvent, an aromatic hydrocarbon organic solvent, an aromatic alkane organic solvent, an ester organic solvent, an ether organic solvent, and a ketone organic solvent.
[0014] More specifically, the first solvent is selected from at least one of toluene, xylene, acetone, butanone, ethyl acetate, butyl acetate, ethylene glycol diacetate, propylene glycol diacetate, propylene glycol methyl ether acetate, methyl 3-methoxypropionate and ethyl 3-ethoxypropionate.
[0015] Optionally, the first catalyst is an organic bismuth catalyst.
[0016] Optionally, the alicyclic isocyanate elastic prepolymer is obtained by polymerizing an alicyclic isocyanate monomer with at least one of a polyol and a polyaspartic acid ester resin.
[0017] Optionally, the alicyclic isocyanate monomer is selected from at least one of isophorone diisocyanate, isophorone diisocyanate trimer, dicyclohexylmethane diisocyanate, and cyclohexane dimethylene diisocyanate.
[0018] The alicyclic isocyanate elastic prepolymer is prepared by the same method as that of the aliphatic isocyanate elastic prepolymer.
[0019] Optionally, the aliphatic imine resin is obtained by reacting an aliphatic diamine with at least one of a ketone compound and an aldehyde compound.
[0020] Optionally, the aliphatic diamine is selected from at least one of pentamethylenediamine, 2-methyl-1,5-pentamethylenediamine, hexamethylenediamine and trimethylhexamethylenediamine.
[0021] Optionally, the ketone compound is selected from at least one of acetone, butanone, methyl isobutyl ketone, methyl isoamyl ketone and methyl isopropyl ketone.
[0022] Optionally, the aldehyde compound is selected from at least one of benzaldehyde, phenylacetaldehyde, n-butyraldehyde, isobutyraldehyde, isovaleraldehyde, and 2,2-dimethyl-3-lauroyloxy-propionaldehyde.
[0023] The aliphatic imine resin is prepared by the following method: dehydrating and condensing the reaction raw materials at a temperature of 90-120° C. for 12-24 hours.
[0024] Optionally, the alicyclic imine resin is obtained by reacting an alicyclic diamine with at least one of a ketone compound and an aldehyde compound.
[0025] Optionally, the alicyclic diamine is selected from at least one of 4,4'-diaminodicyclohexylmethane, 3,3'-dimethyl-4,4-diaminodicyclohexylmethane, isophoronediamine, methylcyclohexanediamine, cyclohexanediamine, and 1,3-cyclohexanedimethylamine.
[0026] The alicyclic imine resin is prepared by the same method as the aliphatic imine resin.
[0027] The preparation method of the aliphatic polyaspartic acid ester resin comprises the following steps: adding reaction of aliphatic diamine with one of maleate and fumarate at a temperature of 70-10° C. for 12-48 hours.
[0028] The preparation method of the aliphatic polyaspartic acid ester resin also includes the following steps: dehydrating and condensing the product obtained after the addition reaction with at least one of a ketone compound and an aldehyde compound at a temperature of 90-120° C. for 12-24 hours.
[0029] Optionally, the maleate is selected from at least one of dimethyl maleate, diethyl maleate, di-n-butyl maleate, and diisooctyl maleate.
[0030] Optionally, the fumarate ester is selected from at least one of dimethyl fumarate, diethyl fumarate, dipropyl fumarate and dibutyl fumarate.
[0031] The alicyclic polyaspartic acid ester resin is prepared by the same method as the aliphatic polyaspartic acid ester resin, except that the aliphatic diamine is replaced by the alicyclic diamine.
[0032] Through the above technical scheme, the present application utilizes the hydrolysis of imide resin and the curing of isocyanate prepolymer to obtain a coating with high strength, high elongation and strong weather resistance, and the introduction of the rigid alicyclic structure further improves the strength of the coating, so that the coating has good tearability and high tear strength. When the car cover film needs to be replaced, the coating can be peeled off in one piece, and the peelability is strong, which greatly improves the convenience of replacing the car cover film. At the same time, the present application also utilizes the combination of imide resin with isocyanate prepolymer and polyaspartic acid ester resin, which significantly reduces the reaction rate between the amino compound component and the isocyanate component, adjusts the drying speed, and allows the coating to fully wet the inside of the substrate, thereby improving the adhesion between the cured coating and the car paint. After testing, the pull-out adhesion between the spray liquid car cover film composition of the present application and the smooth car paint surface after curing to form a coating can reach 3-5MPa.
[0033] Preferably, when component A and component B are used in combination, at least two of the isocyanate prepolymer, imide resin and polyaspartic acid ester resin contain an alicyclic structure.
[0034] Preferably, when component A and component B are mixed for use, the isocyanate prepolymer, imide resin and polyaspartic acid ester resin all contain alicyclic structures.
[0035] Through the above technical solution, the present application optimizes the minimum introduction amount of the alicyclic structure, further enhances the mechanical strength of the coating, and thus further improves the strippability of the coating.
[0036] Preferably, the component A further comprises 1-10 parts by weight of an isocyanate monomer, and the isocyanate monomer is an alicyclic isocyanate monomer.
[0037] Through the above technical scheme, the present application uses isocyanate monomers and isocyanate prepolymers with rigid alicyclic structures to be cured together with components such as the imide resin in component B, thereby further improving the mechanical strength of the coating and thus improving the strippability of the coating.
[0038] Preferably, the sprayable liquid car cover film composition further comprises at least one of a defoaming agent, a leveling agent, an anti-sagging agent, an ultraviolet absorber, a second catalyst, a second solvent, and a color paste.
[0039] Optionally, in parts by weight, the defoamer is 0-1 part, the leveling agent is 0-1 part, the anti-sagging agent is 0-1 part, the ultraviolet absorber is 0-3 parts, the second catalyst is 0-3 parts, the second solvent is 0-60 parts, and the color paste is 0-20 parts.
[0040] Through the above technical solution, when it is necessary to add the above substances, as known to those skilled in the art, these substances can be added to component A or component B in any combination or separately form component C and mix with component A and component B. In the specific implementation of the present application, the addition of the above substances to component A and component B is used as an example for explanation.
[0041] Optionally, the defoamer is selected from one of a polyether defoamer, a silicone defoamer, and a polyether-modified silicone defoamer. Preferably, the defoamer is a polyether defoamer. More specifically, the polyether defoamer is one of BYK1790, BYK054, and BYK052.
[0042] By adopting the above technical solution, polyether defoamers, silicone defoamers, and polyether-modified silicone defoamers can achieve good defoaming effects. Among them, polyether defoamers have a moderate lipophilic and hydrophilic ratio, a high defoaming rate, and good compatibility in polyaspartic acid resin systems and polyurea systems, and the resulting coating has a better appearance.
[0043] Optionally, the leveling agent is a polyacrylate leveling agent or a fluorocarbon modified polyacrylate leveling agent.
[0044] Preferably, the leveling agent is one of BYK354, BYK399 and EFKA3600.
[0045] By adopting the above technical solution, the three leveling agents BYK354, BYK399 and EFKA3600 have better compatibility with the polyaspartic acid ester resin, so that the leveling property of the coating is better and the obtained coating has higher gloss.
[0046] Optionally, the anti-sagging agent is BYK410.
[0047] Optionally, the ultraviolet absorber is UV1130 or UV292.
[0048] Optionally, the second catalyst is selected from one of an organic bismuth catalyst and an acid catalyst. The acid catalyst is selected from at least one of an inorganic acid catalyst, an organic acid catalyst and a Lewis acid catalyst.
[0049] More specifically, the second catalyst is selected from one of phosphoric acid, lactic acid, glacial acetic acid, citric acid, lauric acid, oxalic acid and dodecylbenzenesulfonic acid.
[0050] Optionally, the second solvent is selected from one of an alkane organic solvent, an aromatic hydrocarbon organic solvent, an aromatic alkane organic solvent, an ester organic solvent, an ether organic solvent, and a ketone organic solvent.
[0051] More specifically, the second solvent is selected from one of toluene, xylene, acetone, butanone, ethyl acetate, butyl acetate, ethylene glycol diacetate, propylene glycol diacetate, propylene glycol methyl ether acetate, methyl 3-methoxypropionate and ethyl 3-ethoxypropionate.
[0052] Preferably, the color paste is prepared from at least one of polyaspartic acid ester resin and imide resin, an anti-settling agent, a dispersant, a pigment, and a third solvent.
[0053] Optionally, in parts by weight, the polyaspartic acid ester resin is 0-60 parts, the imide resin is 0-60 parts, the anti-settling agent is 0.1-1 parts, the dispersant is 1-10 parts, the pigment is 10-70 parts, and the third solvent is 0-20 parts.
[0054] The preparation method of the color paste is: all components are mixed, and dispersed at a high speed of 1000-1500 r / min for 30-40 minutes, and then ground to a fineness of less than 20 μm.
[0055] Optionally, the anti-settling agent is BYK163.
[0056] Optionally, the dispersant is fumed silica R972 or polyamide wax 6900-20X.
[0057] Optionally, the pigment is selected from inorganic pigments, pearlescent pigments, and organic pigments, wherein the inorganic pigments include but are not limited to diamond titanium dioxide, carbon black, red iron oxide, and iron yellow.
[0058] Optionally, the third solvent is selected from one of an alkane organic solvent, an aromatic hydrocarbon organic solvent, an aromatic alkane organic solvent, an ester organic solvent, an ether organic solvent, and a ketone organic solvent.
[0059] More specifically, the third solvent is selected from at least one of toluene, xylene, acetone, butanone, ethyl acetate, butyl acetate, ethylene glycol diacetate, propylene glycol diacetate, propylene glycol methyl ether acetate, methyl 3-methoxypropionate and ethyl 3-ethoxypropionate.
[0060] Through the above technical scheme, the color paste prepared by mixing polyaspartic acid ester resin or imide resin with pigment and other components has excellent weather resistance, good compatibility with the polyurea coating of the present application, and is easy to be evenly dispersed in the polyurea coating of the present application.
[0061] In a second aspect, the present application provides a spray-coated car cover film, comprising a protective layer, wherein the protective layer is formed by spraying a liquid car cover film composition and curing it on a car paint surface.
[0062] Through the above technical scheme, the spray-coated car cover film of the present application not only has good adhesion with the smooth car paint, but also has excellent mechanical strength and weather resistance, can be peeled off in one piece, and is easy to replace.
[0063] Preferably, a topcoat layer is further provided on the outer surface of the protective layer, and the topcoat layer is an acrylic resin layer or a polyaspartic acid ester polyurea layer.
[0064] Through the above technical solution, the present application further sets a topcoat layer on the outer surface of the protective layer, which can further enhance the gloss, hardness, scratch resistance and other properties of the sprayed car cover film. Among them, the acrylic resin layer is formed by curing acrylic resin coating. The polyaspartic acid ester polyurea layer is formed by curing polyaspartic acid ester polyurea coating. The topcoat layers formed by the above two coatings have excellent fullness, gloss, weather resistance, and light and color retention. In the specific implementation of the present application, polyaspartic acid ester polyurea coating is used as an example for explanation.
[0065] Preferably, a color-adjusting layer is further provided between the protective layer and the topcoat layer, and the color-adjusting layer is selected from at least one of a solid color paint layer, a metallic paint layer or a pearlescent paint layer.
[0066] Optionally, the solid color paint layer is formed by curing one of polyaspartic acid ester solid color paint, polyurethane solid color paint, and acrylate solid color paint. The color of the solid color paint layer can be adjusted according to actual needs.
[0067] Optionally, the metal paint layer is formed by curing one of polyaspartic acid ester metal paint, polyurethane metal paint and acrylate metal paint. The color of the metal paint layer can be adjusted according to actual needs.
[0068] Optionally, the pearlescent paint layer is formed by curing one of polyaspartic acid ester pearlescent paint, polyurethane pearlescent paint, and acrylate pearlescent paint. The color of the pearlescent paint layer can be adjusted according to actual needs.
[0069] Through the above technical scheme, the present application further sets a color adjustment layer between the protective layer and the topcoat layer, which can provide different colors for the spray-coated car cover film to meet the decorative requirements. And according to actual needs, a solid color paint layer or a more decorative metallic paint layer or pearlescent paint layer can be selected. In the specific implementation of the present application, a solid color paint layer is used as an example for illustration. In the solid color paint layer, the above three solid color coatings all have good weather resistance and light and color retention. In the specific implementation of the present application, a polyaspartic acid ester type solid color coating is used as an example for illustration. The polyaspartic acid ester type solid color coating has the same raw material selection and preparation method as the color paste in the spray liquid car cover film composition.
[0070] In a third aspect, the present application provides a method for preparing a spray-coated car cover film, which adopts the following technical solution: A method for preparing a spray-coated car cover film comprises the following steps: S1. The raw materials used for component A of the sprayable liquid car cover film composition are dispersed at a speed of 1000-1500r / min for 30-40 minutes to obtain component A; the raw materials used for component B of the sprayable liquid car cover film composition are dispersed at a speed of 1000-1500r / min for 30-40 minutes to obtain component B; S2. Mix component A and component B in a weight ratio of (1-10):1, spray them on the outer surface of the car paint, and form a protective layer after curing to obtain a spray car cover film.
[0071] In summary, the present application has the following beneficial technical effects: the present application adopts imide resin, isocyanate prepolymer and polyaspartic acid ester resin to prepare a coating with high strength, high elongation and strong weather resistance. The coating not only has good adhesion with smooth car paint, but also has extremely high tensile strength, weather resistance and tear strength. It can be peeled off in one piece, has strong peelability and is easy to replace. DETAILED DESCRIPTION
[0072] <Specific Embodiments of Aliphatic Polyaspartic Acid Ester Resin and Alicyclic Polyaspartic Acid Ester Resin> In some embodiments of the aliphatic polyaspartic acid ester resin, the aliphatic diamine is selected from at least one of pentamethylenediamine, 2-methyl-1,5-pentamethylenediamine, hexamethylenediamine, and trimethylhexamethylenediamine; In some embodiments of the aliphatic polyaspartic acid ester resin, the maleate is selected from at least one of dimethyl maleate, diethyl maleate, di-n-butyl maleate, and diisooctyl maleate; In some embodiments of the aliphatic polyaspartic acid ester resin, the fumarate is selected from at least one of dimethyl fumarate, diethyl fumarate, dipropyl fumarate, and dibutyl fumarate; In some embodiments of the aliphatic polyaspartic acid ester resin, the ketone compound is selected from at least one of acetone, butanone, methyl isobutyl ketone, methyl isoamyl ketone and methyl isopropyl ketone; In some embodiments of the aliphatic polyaspartic acid ester resin, the aldehyde compound is selected from at least one of benzaldehyde, phenylacetaldehyde, n-butyraldehyde, isobutyraldehyde, isovaleraldehyde, and 2,2-dimethyl-3-lauroyloxy-propionaldehyde; In some specific embodiments of the aliphatic polyaspartic acid ester resin, the above raw materials are used to perform an addition reaction of an aliphatic diamine with one of maleate and fumarate at a temperature of 70-100° C. for 12-24 hours to obtain an aliphatic polyaspartic acid ester resin.
[0073] In some specific embodiments of the aliphatic polyaspartic acid ester resin, the above raw materials are used to firstly carry out an addition reaction of an aliphatic diamine with one of maleate and fumarate at a temperature of 70-100° C. for 12-24 hours, and then carry out a dehydration condensation reaction with at least one of a ketone compound and an aldehyde compound at a temperature of 90-120° C. for 12-24 hours to obtain an aliphatic polyaspartic acid ester resin containing an imine group.
[0074] The specific embodiment of the alicyclic polyaspartic acid ester resin is different from the specific embodiment of the aliphatic polyaspartic acid ester resin in that the aliphatic diamine is replaced by the alicyclic diamine, and the rest are the same. The alicyclic diamine is selected from at least one of 4,4'-diaminodicyclohexylmethane, 3,3'-dimethyl-4,4-diaminodicyclohexylmethane, isophoronediamine, methylcyclohexanediamine, cyclohexanediamine, and 1,3-cyclohexanedimethylamine.
[0075] Among the above-mentioned numerous specific embodiments of aliphatic polyaspartic acid ester resin and alicyclic polyaspartic acid ester resin, the applicant uses the following specific embodiments as examples for illustration. Unless otherwise specified, the raw materials used in the specific embodiments of the present application are all commercially available products.
[0076] Preparation Example 1.1.1 Aliphatic polyaspartic acid ester resin 1 was prepared by the following method: 116 kg of 2-methyl-1,5-pentanediamine and 344 kg of diethyl maleate were subjected to addition reaction at 70° C. for 24 hours to obtain aliphatic polyaspartic acid ester resin 1 having an amine equivalent of 230.
[0077] Preparation Example 1.1.2 Alicyclic polyaspartic acid ester resin 1 was prepared by the following method: 238 kg of 3,3'-dimethyl-4,4-diaminodicyclohexylmethane and 344 kg of diethyl maleate were subjected to addition reaction at 100° C. for 48 hours to obtain alicyclic polyaspartic acid ester resin 1 having an amine equivalent of 291.
[0078] Preparation Example 1.2.1 Aliphatic polyaspartic acid ester resin 2 was prepared by the following method: 158 kg of trimethylhexamethylenediamine and 344 kg of diethyl fumarate were subjected to addition reaction at 70° C. for 24 hours to obtain aliphatic polyaspartic acid ester resin 2 having an amine equivalent of 251.
[0079] Preparation Example 1.2.2 Alicyclic polyaspartic acid ester resin 2 was prepared by the following method: 170 kg of isophorone diamine and 344 kg of diethyl fumarate were subjected to addition reaction at 100° C. for 24 hours to obtain alicyclic polyaspartic acid ester resin 2 having an amine equivalent of 257.
[0080] Preparation Example 1.3.1 Aliphatic imine group-containing polyaspartic acid ester resin is prepared by the following method: 158 kg of trimethylhexanediamine and 172 kg of diethyl maleate were subjected to addition reaction at 70°C for 12 hours, and then 114 kg of benzaldehyde was added, and the temperature was raised to 120°C for dehydration condensation for 12 hours to obtain an aliphatic imine group-containing polyaspartic acid ester resin.
[0081] Preparation Example 1.3.2 The alicyclic imine group-containing polyaspartic acid ester resin is prepared by the following method: 210 kg of 4,4'-diaminodicyclohexylmethane and 172 kg of diethyl maleate were subjected to addition reaction at 90°C for 24 hours, and then 114 kg of benzaldehyde was added, and the temperature was raised to 120°C for dehydration condensation for 12 hours to obtain alicyclic imine group-containing polyaspartic acid ester resin.
[0082] <Specific Embodiments of Aliphatic Isocyanate Prepolymer and Alicyclic Isocyanate Prepolymer> In some specific embodiments of the aliphatic isocyanate prepolymer, the aliphatic isocyanate monomer is selected from at least one of hexamethylene diisocyanate, hexamethylene diisocyanate trimer, 1,5-pentamethylene diisocyanate, 1,5-pentamethylene diisocyanate trimer and trimethylhexamethylene diisocyanate; In some specific embodiments of the aliphatic isocyanate prepolymer, the polyol is a diol, and the diol is selected from at least one of polyester diol, polycaprolactone diol, polycarbonate diol, polytetramethylene glycol, and a chain aliphatic diol having 1 to 18 carbon atoms, and the molecular weight of the diol is 62 to 3000; In some specific embodiments of the aliphatic isocyanate prepolymer, the first catalyst is an organic bismuth catalyst, the main component of which is bismuth isooctanoate, the effective component content is 20%, and it is purchased from Xinghai Chemical; In some embodiments of the aliphatic isocyanate prepolymer, the first solvent is selected from at least one of toluene, xylene, acetone, butanone, ethyl acetate, butyl acetate, ethylene glycol diacetate, propylene glycol diacetate, propylene glycol methyl ether acetate, methyl 3-methoxypropionate, and ethyl 3-ethoxypropionate; In some specific embodiments of the aliphatic isocyanate prepolymer, the above raw materials are used to react an aliphatic isocyanate monomer with a polyol or a polyaspartic acid ester resin or a mixture of a polyol and a polyaspartic acid resin at 60-90° C. for 5-9 hours with the addition of a first catalyst or a first solvent to obtain an aliphatic isocyanate prepolymer having an NCO content of 2-10%.
[0083] The specific embodiment of the alicyclic isocyanate prepolymer is different from the specific embodiment of the aliphatic isocyanate prepolymer in that the aliphatic isocyanate monomer is replaced by an alicyclic isocyanate monomer, and the rest are the same. The alicyclic isocyanate monomer is selected from at least one of isophorone diisocyanate, isophorone diisocyanate trimer, dicyclohexylmethane diisocyanate, and cyclohexane dimethylene diisocyanate.
[0084] Among the above-mentioned numerous specific embodiments of aliphatic isocyanate prepolymers and alicyclic isocyanate prepolymers, the applicant uses the following specific embodiments as examples for illustration. Unless otherwise specified, the raw materials used in the specific embodiments of the present application are all commercially available products.
[0085] Preparation Example 2.1.1 Aliphatic isocyanate prepolymer 1 was prepared by the following method: 100 kg of hexamethylene diisocyanate (NCO content of 49.5%) was heated to 70°C, 302 kg of polycaprolactone diol (average molecular weight of 1000) was added, and then the mixture was kept at 70°C for 8 hours to obtain aliphatic isocyanate prepolymer 1 with an NCO content of 6.0%.
[0086] Preparation Example 2.1.2 The alicyclic isocyanate prepolymer 1 was prepared by the following method: 100 kg of isophorone diisocyanate (NCO content: 37.5%) was heated to 70°C, and 219 kg of polycaprolactone diol (average molecular weight: 1000) was added, followed by reaction at 70°C for 8 hours to obtain alicyclic isocyanate prepolymer 1 having an NCO content of 6.0%.
[0087] Preparation Example 2.2.1 Aliphatic isocyanate prepolymer 2 was prepared by the following method: 0.01 kg of organic bismuth catalyst was added to 100 kg of 1,5-pentane diisocyanate (NCO content of 54.5%), and after heating to 60° C., 290 kg of polytetrahydrofuran diol (average molecular weight of 2000) and 100 kg of polycarbonate diol (average molecular weight of 650) were added, and then the mixture was kept warm at 60° C. for 5 hours to obtain aliphatic isocyanate prepolymer 2 with an NCO content of 6.0%.
[0088] Preparation Example 2.2.2 The alicyclic isocyanate prepolymer 2 was prepared by the following method: 0.01 kg of organic bismuth catalyst was added to 100 kg of dicyclohexylmethane diisocyanate (NCO content was 32%), and after heating to 60° C., 290 kg of polytetrahydrofuran diol (average molecular weight was 2000) and 100 kg of polycarbonate diol (average molecular weight was 650) were added, and then the mixture was kept warm at 60° C. for 5 hours to obtain alicyclic isocyanate prepolymer 2 having an NCO content of 6.0%.
[0089] Preparation Example 2.3.1 Aliphatic isocyanate prepolymer 3 was prepared by the following method: To 138 kg of trimethylol hexamethylene diisocyanate (NCO content of 40%), 40 kg of xylene and 30 kg of butyl acetate were added, and after heating to 80°C, 290 kg of polycaprolactone diol (average molecular weight of 2000) was added, followed by keeping the reaction at 80°C for 5 hours, and then 20 kg of propylene glycol (average molecular weight of 92) was added and kept reacting for 1 hour to obtain aliphatic isocyanate prepolymer 3 with an NCO content of 3.0%.
[0090] Preparation Example 2.3.2 The alicyclic isocyanate prepolymer 3 was prepared by the following method: To 193 kg of dicyclohexylmethane diisocyanate (NCO content: 32%), add 68.5 kg of xylene and 51.5 kg of butyl acetate, heat to 80°C and add 290 kg of polycaprolactone diol (average molecular weight: 2000), then keep warm at 80°C for 5 hours, then continue to add 180 kg of alicyclic polyaspartic acid ester resin 1 (average molecular weight: 582) obtained in Preparation Example 1.1.2 and keep warm for 1 hour to obtain alicyclic isocyanate prepolymer 3 with an NCO content of 3.0%.
[0091] Preparation Example 2.4.1 Aliphatic isocyanate prepolymer 4 was prepared by the following method: 0.01 kg of organic bismuth catalyst was added to 100 kg of 1,5-pentane diisocyanate (NCO content of 54.5%), and the temperature was raised to 75°C, and 950 kg of polyester diol (average molecular weight of 3000) was added, followed by keeping the temperature at 75°C for 8 hours, and then 500 kg of 1,5-pentane diisocyanate trimer (NCO content of 25%) was added and kept warm for 1 hour to obtain aliphatic isocyanate prepolymer 4 with an NCO content of 9.86%.
[0092] Preparation Example 2.4.2 The alicyclic isocyanate prepolymer 4 was prepared by the following method: 0.01 kg of organic bismuth catalyst was added to 130 kg of cyclohexane dimethylene diisocyanate (NCO content of 43%), and 950 kg of polyester diol (average molecular weight of 3000) was added after heating to 75°C, and then kept warm at 75°C for 8 hours. After that, 330 kg of dicyclohexylmethane diisocyanate (NCO content of 32%) and 50 kg of isophorone diisocyanate trimer (NCO content of 17.5%) were added and kept warm for 1 hour to obtain alicyclic isocyanate prepolymer 4 with an NCO content of 9.86%.
[0093] <Specific Embodiments of Aliphatic Imine Resins and Alicyclic Imine Resins> In some embodiments of the aliphatic imine resin, the aliphatic diamine is selected from at least one of pentamethylenediamine, 2-methyl-1,5-pentamethylenediamine, hexamethylenediamine, and trimethylhexamethylenediamine; In some specific embodiments of the aliphatic imine resin, the above raw materials are used to dehydrate and condense an aliphatic diamine with at least one of a ketone compound and an aldehyde compound at a temperature of 90-120° C. for 12-24 hours to obtain an aliphatic imine resin.
[0094] The specific embodiment of the alicyclic imine resin is different from the specific embodiment of the aliphatic imine resin in that the aliphatic diamine is replaced by the alicyclic diamine, and the rest are the same. The alicyclic diamine is selected from at least one of 4,4'-diaminodicyclohexylmethane, 3,3'-dimethyl-4,4-diaminodicyclohexylmethane, isophoronediamine, methylcyclohexanediamine, cyclohexanediamine, and 1,3-cyclohexanedimethylamine.
[0095] Among the above-mentioned numerous specific embodiments of aliphatic imine resins and alicyclic imine resins, the applicant uses the following specific embodiments as examples for illustration. Unless otherwise specified, the raw materials used in the specific embodiments of the present application are all commercially available products.
[0096] Preparation Example 3.1.1 Aliphatic imide resin 1 was prepared by the following method: 116 kg of hexamethylenediamine and 144 kg of isobutylaldehyde were mixed, heated to 90° C. and dehydrated and condensed for 12 hours to obtain aliphatic imine resin 1.
[0097] Preparation Example 3.1.2 Alicyclic imide resin 1 was prepared by the following method: 170 kg of isophorone diamine, 128 kg of methylcyclohexane diamine and 577 kg of butanone were mixed, heated to 90° C. for dehydration condensation for 12 hours to obtain alicyclic imine resin 1.
[0098] Preparation Example 3.2.1 The preparation method of aliphatic imine resin 2 is as follows: 102 kg of pentamethylenediamine and 220 kg of benzaldehyde were mixed, heated to 120° C. and dehydrated and condensed for 12 hours to obtain aliphatic imine resin 2.
[0099] Preparation Example 3.2.2 The preparation method of alicyclic imine resin 2 is as follows: 210 kg of 4,4'-diaminodicyclohexylmethane, 53 kg of isobutylaldehyde and 220 kg of methyl isobutyl ketone were mixed, and the mixture was heated to 120° C. for dehydration condensation for 12 hours to obtain alicyclic imine resin 2.
[0100] Preparation Example 3.3.1 The preparation method of aliphatic imide resin 3 is as follows: 116 kg of 2-methyl-1,5-pentanediamine, 108 kg of butanone and 150 kg of methyl isobutyl ketone were mixed, heated to 90° C. and dehydrated and condensed for 24 hours to obtain aliphatic imine resin 3.
[0101] Preparation Example 3.3.2 The preparation method of alicyclic imine resin 3 is as follows: 238 kg of 3,3'-dimethyl-4,4-diaminodicyclohexylmethane, 108 kg of butanone and 150 kg of methyl isobutyl ketone were mixed, and the temperature was raised to 110° C. for dehydration condensation for 24 hours to obtain alicyclic imine resin 3.
[0102] <Specific implementation method of color paste> In some specific embodiments of the color paste, the anti-settling agent is BYK163; In some embodiments of the color paste, the dispersant is fumed silica R972 or polyamide wax 6900-20X; In some specific embodiments of the color paste, the pigment is selected from one of an inorganic pigment, a pearlescent pigment, and an organic pigment; wherein the inorganic pigment includes but is not limited to diamond titanium dioxide, carbon black, red iron oxide, and iron yellow; In some specific embodiments of the color paste, the third solvent is selected from at least one of toluene, xylene, acetone, butanone, ethyl acetate, butyl acetate, ethylene glycol diacetate, propylene glycol diacetate, propylene glycol methyl ether acetate, methyl 3-methoxypropionate, and ethyl 3-ethoxypropionate; In some specific embodiments of the color paste, the above raw materials are used to mix 0-60 parts of polyaspartic acid ester resin, 0-60 parts of imide resin, 0.1-1 parts of anti-settling agent, 1-10 parts of dispersant, 10-70 parts of pigment, and 0-20 parts of the third solvent, and dispersed at a high speed of 1000-1500r / min for 30-40 minutes, and then ground to a fineness of less than 20μm to obtain a color paste.
[0103] Among the above-mentioned numerous specific embodiments of the color paste, the applicant uses the following specific embodiments as examples for illustration. Unless otherwise specified, the raw materials used in the specific embodiments of the present application are all commercially available products.
[0104] Preparation Example 4.1 Color paste 1 was prepared by the following method: 35 kg of the alicyclic polyaspartic acid ester resin 1 prepared in Preparation Example 1.1.2, 15 kg of the alicyclic imine resin 1 prepared in Preparation Example 3.1.2, 0.2 kg of anti-settling agent (BYK163), 1 kg of dispersant (fumed silica R972), 8 kg of red iron oxide, 25 kg of pearl white, 10 kg of butyl acetate, and 5.8 kg of propylene glycol methyl ether acetate were dispersed at a high speed of 1000 r / min for 40 minutes, and then ground to a fineness of less than 20 μm to obtain color paste 1.
[0105] Preparation Example 4.2 Color paste 2 was prepared by the following method: 60 kg of alicyclic polyaspartic acid ester resin 1 prepared in Preparation Example 1.1.2, 0.1 kg of anti-settling agent (BYK163), 5 kg of dispersant (polyamide wax 6900-20X), 8 kg of red iron oxide, 11.1 kg of pearl white, 10 kg of butyl acetate, and 5.8 kg of propylene glycol methyl ether acetate were dispersed at a high speed of 1500 r / min for 30 minutes, and then ground to a fineness of less than 20 μm to obtain color paste 2.
[0106] Preparation Example 4.3 Color paste 3 was prepared by the following method: 25 kg of the alicyclic imide resin 1 prepared in Preparation Example 3.1.2, 1 kg of anti-settling agent (BYK163), 1 kg of dispersant (fumed silica R972), 30 kg of red iron oxide, 40 kg of pearl white, and 3 kg of ethylene glycol diacetate were dispersed at a high speed of 1300 r / min for 35 minutes, and then ground to a fineness of less than 20 μm to obtain color paste 3.
[0107] <Specific implementation method of spraying car cover film> The applicant uses the raw materials prepared in the above preparation examples and other raw materials, and then uses the following embodiments and comparative examples as examples to explain in detail the effects of the raw material adjustment of the present application on the performance of the spray-coated car cover film.
[0108] Example 1.1 A method for preparing a spray-coated car cover film comprises the following steps: S1. 40 kg of the alicyclic isocyanate prepolymer 1 prepared in Preparation Example 2.1.2, 25 kg of the second solvent (10 kg of butyl acetate, 15 kg of propylene glycol methyl ether acetate), 1 kg of a defoamer (BYK1790), 1 kg of a leveling agent (EFKA3600), and 3 kg of an ultraviolet absorber (UV1130) were dispersed at a speed of 1000 r / min for 40 minutes to obtain component A; 20 kg of the aliphatic imine resin 1 prepared in Preparation Example 3.1.1, 20 kg of the aliphatic polyaspartic acid ester resin 1 prepared in Preparation Example 1.1.1, and 35 kg of the second solvent (20 kg of xylene, 15 kg of propylene glycol methyl ether acetate) were dispersed at a speed of 1000 r / min for 40 minutes to obtain component B; S2. After mixing component A and component B in a weight ratio of 4.5:1, spray them on the outer surface of the car paint, and after curing, form a protective layer with a thickness of 100 μm to obtain a spray car cover film.
[0109] Example 1.2 A method for preparing a spray-coated car cover film comprises the following steps: S1. 40 kg of the alicyclic isocyanate prepolymer 2 prepared in Preparation Example 2.2.2, 25 kg of the second solvent (10 kg of butyl acetate, 15 kg of propylene glycol methyl ether acetate), 1 kg of a defoamer (BYK1790), 1 kg of a leveling agent (EFKA3600), and 3 kg of an ultraviolet absorber (UV1130) were dispersed at a speed of 1500 r / min for 30 minutes to obtain component A; 20 kg of the aliphatic imine resin 2 prepared in Preparation Example 3.2.1, 20 kg of the aliphatic polyaspartic acid ester resin 2 prepared in Preparation Example 1.2.1, and 35 kg of the second solvent (20 kg of xylene, 15 kg of propylene glycol methyl ether acetate) were dispersed at a speed of 1500 r / min for 30 minutes to obtain component B; S2. After mixing component A and component B in a weight ratio of 4:1, spray them on the outer surface of the car paint, and after curing, form a protective layer with a thickness of 100 μm to obtain a spray car cover film.
[0110] Example 1.3 A method for preparing a spray-coated car cover film comprises the following steps: S1. 40 kg of the alicyclic isocyanate prepolymer 3 prepared in Preparation Example 2.3.2, 25 kg of the second solvent (10 kg of butyl acetate, 15 kg of propylene glycol methyl ether acetate), 1 kg of a defoamer (BYK1790), 1 kg of a leveling agent (EFKA3600), and 3 kg of an ultraviolet absorber (UV1130) were dispersed at a speed of 1000 r / min for 40 minutes to obtain component A; 20 kg of the aliphatic imine resin 2 prepared in Preparation Example 3.2.1, 20 kg of the aliphatic imine group-containing polyaspartic acid ester resin prepared in Preparation Example 1.3.1, and 35 kg of the second solvent (20 kg of xylene, 15 kg of propylene glycol methyl ether acetate) were dispersed at a speed of 1000 r / min for 40 minutes to obtain component B; S2. After mixing component A and component B in a weight ratio of 10:1, spray them on the outer surface of the car paint, and after curing, form a protective layer with a thickness of 100 μm to obtain a spray car cover film.
[0111] Example 1.4 A method for preparing a spray-coated car cover film comprises the following steps: S1. The alicyclic isocyanate prepolymer 4 prepared in Preparation Example 2.4.2 is used as component A; the aliphatic imide resin 3 prepared in Preparation Example 3.3.1 is used as component B; S2. After mixing component A and component B in a weight ratio of 3.5:1, spray them on the outer surface of the car paint, and after curing, form a protective layer with a thickness of 100 μm to obtain a spray car cover film.
[0112] Example 2.1 A method for preparing a spray-coated car cover film comprises the following steps: S1. 40 kg of the aliphatic isocyanate prepolymer 1 prepared in Preparation Example 2.1.1, 25 kg of the second solvent (10 kg of butyl acetate, 15 kg of propylene glycol methyl ether acetate), 1 kg of a defoamer (BYK1790), 1 kg of a leveling agent (EFKA3600), and 3 kg of an ultraviolet absorber (UV1130) were dispersed at a speed of 1000 r / min for 40 minutes to obtain component A; 20 kg of the alicyclic imine resin 1 prepared in Preparation Example 3.1.2, 20 kg of the aliphatic polyaspartic acid ester resin 1 prepared in Preparation Example 1.1.1, and 35 kg of the second solvent (20 kg of xylene, 15 kg of propylene glycol methyl ether acetate) were dispersed at a speed of 1000 r / min for 40 minutes to obtain component B; S2. After mixing component A and component B in a weight ratio of 4.2:1, spray them on the outer surface of the car paint, and after curing, form a protective layer with a thickness of 100 μm to obtain a spray car cover film.
[0113] Example 2.2 A method for preparing a spray-coated car cover film comprises the following steps: S1. 40 kg of the aliphatic isocyanate prepolymer 2 prepared in Preparation Example 2.2.1, 25 kg of the second solvent (10 kg of butyl acetate, 15 kg of propylene glycol methyl ether acetate), 1 kg of a defoamer (BYK1790), 1 kg of a leveling agent (EFKA3600), and 3 kg of an ultraviolet absorber (UV1130) were dispersed at a speed of 1500 r / min for 30 minutes to obtain component A; 20 kg of the alicyclic imine resin 2 prepared in Preparation Example 3.2.2, 20 kg of the aliphatic polyaspartic acid ester resin 2 prepared in Preparation Example 1.2.1, and 35 kg of the second solvent (20 kg of xylene, 15 kg of propylene glycol methyl ether acetate) were dispersed at a speed of 1500 r / min for 40 minutes to obtain component B; S2. After mixing component A and component B in a weight ratio of 3.2:1, spray them on the outer surface of the car paint, and after curing, form a protective layer with a thickness of 100 μm to obtain a spray car cover film.
[0114] Example 2.3 A method for preparing a spray-coated car cover film comprises the following steps: S1. 40 kg of the aliphatic isocyanate prepolymer 3 prepared in Preparation Example 2.3.1, 25 kg of the second solvent (10 kg of butyl acetate, 15 kg of propylene glycol methyl ether acetate), 1 kg of a defoamer (BYK1790), 1 kg of a leveling agent (EFKA3600), and 3 kg of an ultraviolet absorber (UV1130) were dispersed at a speed of 1000 r / min for 40 minutes to obtain component A; 20 kg of the alicyclic imine resin 2 prepared in Preparation Example 3.2.2, 20 kg of the aliphatic imine group-containing polyaspartic acid ester resin prepared in Preparation Example 1.3.1, and 35 kg of the second solvent (20 kg of xylene, 15 kg of propylene glycol methyl ether acetate) were dispersed at a speed of 1000 r / min for 40 minutes to obtain component B; S2. After mixing component A and component B in a weight ratio of 7:1, spray them on the outer surface of the car paint, and after curing, form a protective layer with a thickness of 100 μm to obtain a spray car cover film.
[0115] Example 2.4 A method for preparing a spray-coated car cover film comprises the following steps: S1. 10 kg of the aliphatic isocyanate prepolymer 4 prepared in Preparation Example 2.4.1, 5 kg of the second solvent (xylene), 0.1 kg of a defoamer (BYK1790), 0.1 kg of a leveling agent (EFKA3600), and 0.5 kg of an ultraviolet absorber (UV1130) were dispersed at a speed of 1000 r / min for 40 minutes to obtain component A; 5 kg of the alicyclic imine resin 3 prepared in Preparation Example 3.3.2, 13 kg of the second solvent (propylene glycol methyl ether acetate), 0.1 kg of a defoamer (BYK1790), 0.1 kg of a leveling agent (EFKA3600), and 0.5 kg of an ultraviolet absorber (UV1130) were dispersed at a speed of 1000 r / min for 40 minutes to obtain component B; S2. After mixing component A and component B in a weight ratio of 1:1, spray them on the outer surface of the car paint, and after curing, form a protective layer with a thickness of 100 μm to obtain a spray car cover film.
[0116] Example 3.1 A method for preparing a spray-coated car cover film comprises the following steps: S1. 40 kg of the aliphatic isocyanate prepolymer 1 prepared in Preparation Example 2.1.1, 25 kg of the second solvent (10 kg of butyl acetate, 15 kg of propylene glycol methyl ether acetate), 1 kg of a defoamer (BYK1790), 1 kg of a leveling agent (EFKA3600), and 3 kg of an ultraviolet absorber (UV1130) were dispersed at a speed of 1000 r / min for 40 minutes to obtain component A; 20 kg of the aliphatic imine resin 1 prepared in Preparation Example 3.1.1, 20 kg of the alicyclic polyaspartic acid ester resin 1 prepared in Preparation Example 1.1.2, and 35 kg of the second solvent (20 kg of xylene, 15 kg of propylene glycol methyl ether acetate) were dispersed at a speed of 1500 r / min for 40 minutes to obtain component B; S2. After mixing component A and component B in a weight ratio of 4.2:1, spray them on the outer surface of the car paint, and after curing, form a protective layer with a thickness of 100 μm to obtain a spray car cover film.
[0117] Example 3.2 A method for preparing a spray-coated car cover film comprises the following steps: S1. 40 kg of the aliphatic isocyanate prepolymer 2 prepared in Preparation Example 2.2.1, 25 kg of the second solvent (10 kg of butyl acetate, 15 kg of propylene glycol methyl ether acetate), 1 kg of defoamer (BYK1790), 1 kg of leveling agent (EFKA3600), and 3 kg of ultraviolet absorber (UV1130) were dispersed at a speed of 1000 r / min for 40 minutes to obtain component A; 20 kg of the aliphatic imine resin 2 prepared in Preparation Example 3.2.1, 20 kg of the alicyclic polyaspartic acid ester resin 2 prepared in Preparation Example 1.2.2, and 35 kg of the second solvent (20 kg of xylene, 15 kg of propylene glycol methyl ether acetate) were dispersed at a speed of 1500 r / min for 40 minutes to obtain component B of the polyurea coating; S2. After mixing component A and component B in a weight ratio of 4:1, spray them on the outer surface of the car paint, and after curing, form a protective layer with a thickness of 100 μm to obtain a spray car cover film.
[0118] Example 3.3 A method for preparing a spray-coated car cover film comprises the following steps: S1. 40 kg of the aliphatic isocyanate prepolymer 3 prepared in Preparation Example 2.3.1, 25 kg of the second solvent (10 kg of butyl acetate, 15 kg of propylene glycol methyl ether acetate), 1 kg of a defoamer (BYK1790), 1 kg of a leveling agent (EFKA3600), and 3 kg of an ultraviolet absorber (UV1130) were dispersed at a speed of 1000 r / min for 40 minutes to obtain component A; 20 kg of the aliphatic imine resin 3 prepared in Preparation Example 3.3.1, 20 kg of the alicyclic imine group-containing polyaspartic acid ester resin prepared in Preparation Example 1.3.2, and 35 kg of the second solvent (20 kg of xylene, 15 kg of propylene glycol methyl ether acetate) were dispersed at a speed of 1500 r / min for 40 minutes to obtain component B; S2. After mixing component A and component B in a weight ratio of 10:1, spray them on the outer surface of the car paint, and after curing, form a protective layer with a thickness of 100 μm to obtain a spray car cover film.
[0119] Example 4 A method for preparing a spray car cover film, which is different from Example 1.1 in that the aliphatic imine resin 1 prepared in Preparation Example 3.1.1 is replaced by the alicyclic imine resin 2 prepared in Preparation Example 3.2.2, the weight ratio of component A to component B is 3.3:1, and the rest are the same.
[0120] Example 5.1 A method for preparing a spray car cover film, which is different from Example 4 in that the aliphatic polyaspartic acid ester resin 1 prepared in Preparation Example 1.1.1 is replaced by the alicyclic polyaspartic acid ester resin 1 prepared in Preparation Example 1.1.2, the weight ratio of component A to component B is 3:1, and the rest are the same.
[0121] Example 5.2 A method for preparing a spray-coated car cover film, which is different from Example 5.1 in that: in step S2, 3 kg of a second catalyst (phosphoric acid) is also added, and the rest is the same.
[0122] Example 6.1 A method for preparing a spray-coated car cover film, which is different from Example 2.1 in that: 1 kg of 1,5-pentanediisocyanate trimer is also added to component A in step S1, the weight ratio of component A to component B is 3.5:1, and the rest is the same.
[0123] Example 6.2 A method for preparing a spray-coated car cover film, which is different from Example 2.1 in that: 10 kg of dicyclohexylmethane diisocyanate is also added to component A in step S1, the weight ratio of component A to component B is 1.5:1, and the rest is the same.
[0124] Examples 7.1-7.4 A method for preparing a spray car cover film, which is different from Example 2.1 in that: 20 kg of color paste is also added to component B in step S1, wherein Example 7.1 uses ordinary color paste purchased from Axalta, model number Spies Hecker; Examples 7.2-7.4 respectively use the color paste prepared in Preparation Examples 4.1-4.3.
[0125] Example 8.1 A method for preparing a spray-coated car cover film, which is different from Example 5.1 in that: a polyaspartic acid ester polyurea coating is also sprayed on the outer surface of the protective layer, and a topcoat layer with a thickness of 40 μm is formed after curing. The polyaspartic acid ester polyurea coating is a homemade product, and the specific raw materials are: Component A uses 40 kg of alicyclic polyaspartic acid ester resin prepared in Preparation Example 1.1.2, 40 kg of a second solvent (20 kg of butyl acetate, 20 kg of propylene glycol methyl ether acetate), 0.1 kg of defoamer (BYK1790), 0.1 kg of leveling agent (EFKA3600) and 0.3 kg of ultraviolet absorber (UV1130); Component B uses 20 kg of HDI trimer and 20 kg of a second solvent (10 kg of xylene, 10 kg of propylene glycol methyl ether acetate).
[0126] Example 8.2 A method for preparing a spray-coated car cover film, which is different from Example 5.1 in that: a polyaspartic acid ester polyurea coating is also sprayed on the outer surface of the protective layer, and a topcoat layer with a thickness of 100 μm is formed after curing. The polyaspartic acid ester polyurea coating is a homemade product, and the specific raw materials are: Component A uses 40 kg of alicyclic polyaspartic acid ester resin prepared in Preparation Example 1.1.2, 40 kg of a second solvent (20 kg of butyl acetate, 20 kg of propylene glycol methyl ether acetate), 0.1 kg of a defoamer (BYK1790), 0.1 kg of a leveling agent (EFKA3600) and 0.3 kg of an ultraviolet absorber (UV1130); Component B uses 20 kg of HDI trimer and 20 kg of a second solvent (10 kg of xylene, 10 kg of propylene glycol methyl ether acetate).
[0127] Example 9 A method for preparing a spray-coated car cover film, which differs from Example 8.1 in that: a polyaspartic acid ester solid color coating is first sprayed on the outer surface of the protective layer, and then a polyaspartic acid ester polyurea coating is sprayed. The polyaspartic acid ester solid color coating adopts the color paste prepared in Preparation Example 4.1, and after curing, a color adjustment layer with a thickness of 20 μm is formed.
[0128] Comparative Example 1 The difference from Example 1.1 is that the alicyclic isocyanate prepolymer 1 prepared in Preparation Example 2.1.2 in component A is replaced by the aliphatic isocyanate prepolymer 1 prepared in Preparation Example 2.1.1, the aliphatic imine resin and the aliphatic polyaspartic acid ester resin in component B are replaced by diphenylmethanediamine (MDA), and the remaining steps are prepared by the same method as Example 1.1 to prepare aromatic spray polyurea, which is sprayed on the outer surface of the vehicle paint to form a protective layer with a thickness of 100 μm after curing.
[0129] Comparative Example 2 The difference from Example 1.1 is that the alicyclic isocyanate prepolymer 1 prepared in Preparation Example 2.1.2 in component A is replaced by the aliphatic isocyanate prepolymer 1 prepared in Preparation Example 2.1.1, the aliphatic imine resin in component B is removed, and the remaining steric secondary amine aspartic acid ester polyurea is prepared by the same method as in Example 1.1, which is sprayed on the outer surface of the car paint and forms a protective layer with a thickness of 100 μm after curing.
[0130] Comparative Example 3 The difference from Example 1.1 is that the alicyclic isocyanate prepolymer 1 prepared in Preparation Example 2.1.2 in step S1 is replaced by the aliphatic isocyanate prepolymer 1 prepared in Preparation Example 2.1.1, and the rest are the same.
[0131] Performance Testing The spray car cover films prepared in the above-mentioned Examples 1-9 and Comparative Examples 1-3 were respectively tested for surface drying time, press drying time, tensile strength, elongation, tear strength, aging resistance, gloss loss and pull-out adhesion, and the hardness of Example 5.1 and Examples 8.1-8.2 was tested. The test results are shown in Table 1.
[0132] Among them, the surface drying time and the pressing drying time are tested with reference to GB / T 1728-1989; The tensile strength, elongation and tear strength refer to GB / T 16777-2008. The coatings in the above embodiments and comparative examples are coated on glass plates respectively. After curing for 168 hours under standard conditions, the coatings are cured to form a coating with a thickness of (0.2-1.0) mm. The coatings are then cut with a slicer to obtain dumbbell I-type specimens that meet the requirements of GB / T 528. The specimens are then stretched to fracture at a tensile speed of 500 mm / min using a tensile testing machine, and the tensile strength, elongation and tear strength are calculated. For aging resistance, refer to GB / T 1766-2008. In a UVA aging box, irradiate the sample with ultraviolet light and calculate the color change rate ΔE of the sample after 1000 hours. For gloss loss rate, refer to GB / T 1766-2008 to measure the gloss before and after aging and calculate the gloss loss rate. The pull-off adhesion is tested with reference to GB / T 5210-2006; the hardness is tested with reference to GB / T2739-2006.
[0133] Table 1 Performance test results Table 1 Data Analysis: As can be seen from Table 1, the spray-coated car cover films prepared in Examples 1-3 of the present application have good strength, elongation, weather resistance, and tear strength, can be peeled off in one piece, have good tearability, and also have good adhesion to the car paint. However, the car cover film prepared by the reaction of aromatic amino components and isocyanate in Comparative Example 1 has too fast drying speed, low pull-out adhesion, and is easy to fall off. It also has poor weather resistance, is easy to yellow, and loses gloss. Comparative Example 2 uses a car cover film prepared by the reaction of a sterically hindered secondary amine aspartic acid ester resin and isocyanate. Although the adhesion is good, the mechanical properties such as tensile strength and tear strength are poor, and it is difficult to peel off in one piece.
[0134] The tensile strength and tear strength of Example 4 are significantly higher than those of Example 1.1, and the weather resistance is better than that of Example 1.1. The tensile strength and tear strength of Example 5 are higher than those of Example 4, and the weather resistance is better than that of Example 4. This indicates that Examples 4-5 enhance the mechanical strength of the coating by optimizing the minimum introduction amount of the alicyclic structure, thereby improving the strippability of the coating.
[0135] The tensile strength and tear strength of Examples 6.1-6.2 are significantly higher than those of Example 2.1, and the weather resistance is stronger than that of Example 2.1, which indicates that Examples 6.1-6.2 use isocyanate monomers and isocyanate prepolymers with rigid alicyclic structures for curing together with components such as the imide resin in component B, which further improves the mechanical strength of the coating, thereby improving the strippability of the coating.
[0136] In Examples 7.1-7.4, the tensile strength and tear strength of Examples 7.2-7.4 are higher than those of Example 7.1, and the weather resistance is stronger than that of Example 7.1, which indicates that the color paste prepared by mixing polyaspartic acid ester resin or imide resin with pigments and other components in Examples 7.2-7.4 has excellent weather resistance, good compatibility with other components in the coating, and is easy to be evenly dispersed in the coating.
[0137] The hardness of Examples 8.1-8.2 is significantly greater than that of Example 5.1, which indicates that providing a topcoat layer on the outer surface of the protective layer can increase the hardness of the car cover film, thereby enhancing the scratch resistance of the car cover film.
[0138] The embodiments of this specific implementation method are all preferred embodiments of the present application, and are not intended to limit the protection scope of the present application. Therefore, all equivalent changes made based on the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A sprayable liquid car cover film composition, comprising component A and component B, characterized in that: In parts by weight, the raw materials used in component A include: 10-40 parts of isocyanate prepolymer; the raw materials used in component B include: 5-20 parts of imide resin and 0-20 parts of polyaspartic acid ester resin; the isocyanate prepolymer is selected from aliphatic isocyanate prepolymer and / or alicyclic isocyanate elastic prepolymer; the imide resin is selected from aliphatic imide resin and / or alicyclic imide resin; the polyaspartic acid ester resin is selected from aliphatic polyaspartic acid ester resin and / or alicyclic polyaspartic acid ester resin; and, when component A and component B are mixed for use, at least one of the isocyanate prepolymer, imide resin and polyaspartic acid ester resin contains an alicyclic structure.
2. A sprayable liquid car cover film composition according to claim 1, characterized in that: When the A component and the B component are used in combination, at least two of the isocyanate prepolymer, the imide resin and the polyaspartic acid ester resin contain an alicyclic structure.
3. A sprayable liquid car cover film composition according to claim 2, characterized in that: When the A component and the B component are mixed for use, the isocyanate prepolymer, the imide resin and the polyaspartic acid ester resin all contain an alicyclic structure.
4. A sprayable liquid car cover film composition according to claim 1, characterized in that: In parts by weight, the component A further comprises 1-10 parts of isocyanate monomers, and the isocyanate monomers are alicyclic isocyanate monomers.
5. The sprayable liquid car cover film composition according to claim 1, characterized in that: The sprayable liquid car cover film composition also includes at least one of a defoamer, a leveling agent, an anti-sagging agent, an ultraviolet absorber, a second catalyst, a second solvent, and a color paste.
6. A sprayable liquid car cover film composition according to claim 5, characterized in that: The color paste is prepared from at least one of polyaspartic acid ester resin and imide resin, an anti-settling agent, a dispersant, a pigment and a third solvent.
7. A spray-coated car cover film, comprising a protective layer, characterized in that: The protective layer is formed by curing the sprayable liquid car cover film composition according to any one of claims 1 to 6 on the outer surface of the car paint.
8. The spray-coated car cover film according to claim 7, characterized in that: The outer surface of the protective layer is also provided with a topcoat layer, and the topcoat layer is an acrylic resin layer or a polyaspartic acid ester polyurea layer.
9. The spray-coated car cover film according to claim 8, characterized in that: A color-adjusting layer is also provided between the protective layer and the topcoat layer, and the color-adjusting layer is selected from at least one of a solid color paint layer, a metallic paint layer, and a pearlescent paint layer.
10. A method for preparing a spray-coated car cover film according to claim 7, characterized in that: The following steps are involved: S1. The raw materials used for component A of the sprayable liquid car cover film composition are dispersed at a speed of 1000-1500r / min for 30-40 minutes to obtain component A; the raw materials used for component B of the sprayable liquid car cover film composition are dispersed at a speed of 1000-1500r / min for 30-40 minutes to obtain component B; S2. Mix component A and component B in a weight ratio of (1-10):1, spray them on the outer surface of the car paint, and form a protective layer after curing to obtain a spray car cover film.
Citation Information
Patent Citations
Imine modified polyaspartate waterproof and anticorrosive coating as well as preparation method and application thereof
CN105949987A
High-weather-resistance high-solid-content polyaspartic acid ester finish paint and preparation method thereof
CN115926595A
Modified asparaginic acid ester resin containing imino group as well as preparation method and application of modified asparaginic acid ester resin
CN116606218A
Reactive oligomers for isocyanate coatings
CN1278276A
method of wet-on-wet application of a multilayer coating
DE102018110594A1
Cited By
Two-component coating composition and application thereof
CN119899580A
Single-component radix asparagi polyurea dispersion liquid and polyurea car cover film water-based paint