Composite coating containing nano microbead material as well as preparation method and application of composite coating

Through the preparation and modification of nanobead materials, the durability and environmental friendliness of solar thermal reflective coatings are improved, the problems of insufficient durability and flame retardancy of existing coatings are solved, and higher antibacterial and photocatalytics are achieved Degradation and thermal insulation properties.

CN118909526APending Publication Date: 2024-11-08SHANDONG WEIDE REMANUFACTURING TECH CO LTD

Patent Information

Application Number
CN202410874896.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing solar thermal reflective coatings have insufficient durability, weather resistance and flame retardancy, resulting in a short service life and need to be improved to environmentally friendly and safe.

Method used

Using nano-bead material, the preparation method of ZnO/TiO2 coated hollow glass beads, combined with tannin modification and carbonization treatment, form a composite coating with high reflectivity, antibacterial and photocatalytic degradation capabilities, and is treated by alkaline treatment. and flame retardant modification improves its flame retardant, thermal insulation and thermal insulation properties.

Benefits of technology

It significantly improves the durability, weather resistance and environmental friendliness of the coating, enhances its antibacterial, photocatalytic degradation, flame retardant, thermal insulation, and thermal insulation properties, ensuring longer service life and higher safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004922715770000161
    Figure BDA0004922715770000161
  • Figure BDA0004922715770000181
    Figure BDA0004922715770000181
  • Figure BDA0004922715770000182
    Figure BDA0004922715770000182
Patent Text Reader

Abstract

The invention provides a composite coating containing a nano microbead material as well as a preparation method and application of the composite coating, and belongs to the technical field of coatings. The coating is prepared from the following raw materials in parts by weight: 15 to 20 parts of a nano microbead material, 150 to 170 parts of waterborne polyurethane, 0.3 to 0.5 part of a silane coupling agent, 0.2 to 0.4 part of a flatting agent, 0.1 to 0.3 part of a de-foaming agent and 150 to 200 parts of water. The prepared composite coating containing the nano microbead material has good reflectivity, water serves as a solvent, the green and environment-friendly performance of the composite coating is improved, meanwhile, the composite coating further has good antibacterial performance, photocatalytic degradation of VOCs, flame retardance, heat preservation, heat insulation, good conductivity and good mechanical performance, and the composite coating has wide application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to a composite coating containing nano-bead materials, a preparation method and application thereof. Background Art

[0002] Due to direct sunlight exposure, some non-metallic materials will gradually lose their original properties and limit the use of large equipment. Sunlight can cause the temperature inside the container to rise sharply, which greatly affects the use and causes great damage to the storage and transportation of products. Buildings and bridges will also be affected by structural expansion due to high temperature. Therefore, it is a simple technical method to apply low solar absorption coating on the surface of objects to reduce the surface temperature increase caused by sunlight.

[0003] Chinese patent document CN101712835B discloses a hollow glass microsphere heat reflective coating, which is composed of a topcoat and a bottomcoat, wherein the topcoat contains at least silicone-acrylic emulsion, rutile titanium dioxide, and nano-composite functional materials, and the bottomcoat contains at least silicone-acrylic emulsion, hollow glass microspheres, hollow inorganic fibers, and engineered cellulose. The synthetic nano-composite functional materials have a strong reflection effect on sunlight, and the reflectivity can reach more than 0.9, giving the coating film excellent reflective and heat-insulating functions. However, as a solar heat reflective coating, its durability, weather resistance, and flame retardancy are poor, which greatly shortens its service life. Summary of the invention

[0004] The purpose of the present invention is to propose a composite coating containing nano-bead material and its preparation method and application, which has good reflectivity and uses water as a solvent to improve its green environmental protection. At the same time, it also has good antibacterial and photocatalytic degradation of VOCs, as well as flame retardancy, heat preservation and heat insulation, good conductivity, excellent mechanical properties, and has broad application prospects.

[0005] The technical solution of the present invention is achieved in this way:

[0006] The invention provides a composite coating containing nano-bead material, which is prepared from the following raw materials by weight: 15-20 parts of nano-bead material, 150-170 parts of waterborne polyurethane, 0.3-0.5 parts of silane coupling agent, 0.2-0.4 parts of leveling agent, 0.1-0.3 parts of defoaming agent and 150-200 parts of water.

[0007] As a further improvement of the present invention, the method for preparing the nano-bead material comprises the following steps:

[0008] S1. Preparation of ZnO / TiO2 coated hollow glass microspheres: dissolving zinc acetate and tetrabutyl titanate in ethanol, adding hollow glass microspheres, dropping ammonia solution, adding polyethylene glycol, heating and stirring to react, centrifuging, washing, drying, and calcining to obtain ZnO / TiO2 coated hollow glass microspheres;

[0009] S2. Tannic acid modification: adding Tris-HCl solution and alkali into water, adjusting the pH value of the aqueous solution, adding ZnO / TiO2 coated hollow glass microspheres and tannic acid, heating and stirring to react, centrifuging, washing, and drying to obtain modified ZnO / TiO2 coated hollow glass microspheres;

[0010] S3. Silver deposition: dissolve silver nitrate in water, add ammonia solution until the precipitate disappears, add modified ZnO / TiO2 coated hollow glass microspheres, stir and mix evenly, add glucose aqueous solution, heat and stir to react, centrifuge, wash, and dry to obtain silver-deposited modified ZnO / TiO2 coated hollow glass microspheres;

[0011] S4. Carbonization: The silver-deposited modified ZnO / TiO2 coated hollow glass microspheres are heated and carbonized to obtain the product.

[0012] As a further improvement of the present invention, the mass ratio of zinc acetate, tetrabutyl titanate, hollow glass microspheres and polyethylene glycol in step S1 is 5-7:10-12:25-30:1-2, the concentration of the ammonia solution is 24-25wt%, the temperature of the heating and stirring reaction is 50-60°C, the time is 2-4h, and the calcination temperature is 450-550°C, and the time is 1-3h.

[0013] As a further improvement of the present invention, the pH value of the aqueous solution is adjusted to 8.5-9.5 in step S2, the mass ratio of the ZnO / TiO2 coated hollow glass microspheres and tannic acid is 15-20:7-10, the temperature of the heating and stirring reaction is 60-70°C, and the time is 1-3h.

[0014] As a further improvement of the present invention, the mass ratio of silver nitrate, modified ZnO / TiO2 coated hollow glass microspheres and glucose in step S3 is 4-7:15-25:7-10, the concentration of the ammonia solution is 24-25wt%, the temperature of the heating and stirring reaction is 90-95°C, and the time is 2-4h.

[0015] As a further improvement of the present invention, the carbonization temperature in step S4 is 1200-1400° C. and the time is 2-4 hours.

[0016] As a further improvement of the present invention, the method for preparing the nano-bead material further comprises the following steps after step S4:

[0017] S5. Alkali treatment: adding the product obtained in step S4 to an alkali solution, stirring the reaction, centrifuging, washing, and drying to obtain an alkali-treated product;

[0018] S6. Flame retardant modification: adding the alkali-treated product to a phytic acid solution, stirring for reaction, centrifuging, washing, drying, and then adding it to an aluminum salt solution, stirring for reaction, centrifuging, washing, drying to obtain a product.

[0019] As a further improvement of the present invention, the alkali solution in step S5 is a 10-12wt% NaOH or KOH solution, the stirring reaction temperature is 40-50°C, and the time is 20-40min; the concentration of the phytic acid solution in step S6 is 12-15wt%, the concentration of the aluminum salt solution is 4-6wt%, and the aluminum salt is selected from at least one of aluminum chloride, aluminum nitrate, and aluminum sulfate.

[0020] The present invention further protects a method for preparing the composite coating containing the nano-bead material, comprising the following steps: adding the nano-bead material into water, adding a silane coupling agent, stirring for reaction, adjusting the pH value of the solution to 8.5-9.5, stirring and dispersing for 1-2 hours, adding waterborne polyurethane, a leveling agent and a defoaming agent, stirring and dispersing for 2-4 hours, and obtaining a composite coating containing the nano-bead material.

[0021] The present invention further protects the use of the composite coating containing the nano-bead material in heat-insulating building materials.

[0022] The present invention has the following beneficial effects:

[0023] The present invention prepares two nanometer microsphere materials, adopts sol-gel reaction to prepare ZnO / TiO2 coated hollow glass microspheres, and coats the surface of the hollow glass microspheres with a layer of ZnO / TiO2 material. The zinc oxide and titanium oxide layers have good ultraviolet light reflection performance, thereby greatly improving the durability and weather resistance of the coating. At the same time, C doping after carbonization in step S4 can improve the catalytic activity of titanium oxide, so that it can use the visible light region, greatly improving the antibacterial and photocatalytic degradation performance of the coating, so that the coating can degrade VOCs such as formaldehyde, ammonia, benzene, etc. in the air, solving the problem that building materials often release VOCs such as formaldehyde and have poor environmental protection, and improving the safety of the coating.

[0024] After the ZnO / TiO2 coated hollow glass microspheres are modified with tannic acid, the surface is rich in carboxyl groups, which can adsorb silver ions (actually silver ammine ions), so that they can react with glucose on the surface of the microspheres to generate silver in situ, further improving the light reflection performance, good antibacterial properties, good conductivity, and can also improve the mechanical properties of the coating. In addition, after the tannic acid forms silver in situ, it can also become a carbon material with a network structure after the subsequent carbonization reaction, and be doped in the titanium oxide layer to improve its photocatalytic activity. At the same time, the carbon material also improves the conductivity of the nanomaterial. At the same time, its loose network structure provides structural convenience for the subsequent adsorption and fixation of phytic acid molecules.

[0025] After carbonization, the surface of the material is treated with alkali to form abundant hydroxyl groups. When added to the phytic acid solution, it can adsorb and fix more phytic acid molecules. Its network structure and large specific surface area provide convenience for the adsorption and fixation of more phytic acid molecules. At the same time, after the phytic acid molecules are fixed, they are further added to the aluminum salt aqueous solution. The phosphoric acid structure on the phytic acid can form a complex bond with the aluminum ions, thereby fixing the aluminum ions. After modification, the flame retardant, thermal insulation and heat insulating properties of the coating are greatly improved.

[0026] The composite coating containing nano-bead material prepared by the present invention has good reflectivity, and water is used as a solvent to improve its green environmental protection. At the same time, it also has good antibacterial and photocatalytic degradation of VOCs, as well as flame retardancy, heat preservation and heat insulation, good electrical conductivity, excellent mechanical properties, and has broad application prospects. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Hollow glass microspheres, industrial grade, 400 mesh, were purchased from Shuolong Mineral Processing Plant in Lingshou County.

[0029] Waterborne polyurethane (solid content 35%), industrial grade, was purchased from Jining Huakai Resin Co., Ltd.

[0030] Preparation Example 1 Preparation method of nano-microsphere material

[0031] The following steps are involved:

[0032] S1. Preparation of ZnO / TiO2 coated hollow glass microspheres: 5 g zinc acetate and 10 g tetrabutyl titanate were dissolved in 500 mL ethanol, 25 g hollow glass microspheres were added, 20 mL 25 wt% ammonia solution was added dropwise, 1 g polyethylene glycol 200 was added, heated to 50°C, stirred for reaction for 2 h, centrifuged, washed, dried, and calcined at 450°C for 1 h to obtain ZnO / TiO2 coated hollow glass microspheres;

[0033] S2. Tannic acid modification: Tris-HCl solution and NaOH were added to water, the pH value of the aqueous solution was adjusted to 8.5, 15 g ZnO / TiO2 coated hollow glass microspheres and 7 g tannic acid were added, heated to 60 ° C, stirred for 1 h, centrifuged, washed, and dried to obtain modified ZnO / TiO2 coated hollow glass microspheres;

[0034] S3. Silver deposition: 4 g of silver nitrate was dissolved in 200 mL of water, 25 wt% ammonia solution was added dropwise until the precipitate disappeared, 15 g of modified ZnO / TiO2 coated hollow glass microspheres were added, stirred and mixed for 15 min, 100 mL of an aqueous solution containing 7 g of glucose was added dropwise, heated to 90 ° C, stirred and reacted for 2 h, centrifuged, washed, and dried to obtain silver-deposited modified ZnO / TiO2 coated hollow glass microspheres;

[0035] S4. Carbonization: The silver-deposited modified ZnO / TiO2 coated hollow glass microspheres were heated to 1200°C and carbonized for 2 hours to obtain the product.

[0036] Preparation Example 2 Preparation method of nano-microsphere material

[0037] The following steps are involved:

[0038] S1. Preparation of ZnO / TiO2 coated hollow glass microspheres: 7 g zinc acetate and 12 g tetrabutyl titanate were dissolved in 500 mL ethanol, 30 g hollow glass microspheres were added, 20 mL 25 wt% ammonia solution was added dropwise, 2 g polyethylene glycol 200 was added, heated to 60°C, stirred for 4 h, centrifuged, washed, dried, and calcined at 550°C for 3 h to obtain ZnO / TiO2 coated hollow glass microspheres;

[0039] S2. Tannic acid modification: Tris-HCl solution and NaOH were added to water, the pH value of the aqueous solution was adjusted to 9.5, 20 g ZnO / TiO2 coated hollow glass microspheres and 10 g tannic acid were added, heated to 70 ° C, stirred for 3 h, centrifuged, washed, and dried to obtain modified ZnO / TiO2 coated hollow glass microspheres;

[0040] S3. Silver deposition: 7 g of silver nitrate was dissolved in 200 mL of water, 25 wt% ammonia solution was added dropwise until the precipitate disappeared, 25 g of modified ZnO / TiO2 coated hollow glass microspheres were added, stirred and mixed for 15 min, 100 mL of an aqueous solution containing 10 g of glucose was added dropwise, heated to 95 ° C, stirred and reacted for 4 h, centrifuged, washed, and dried to obtain silver-deposited modified ZnO / TiO2 coated hollow glass microspheres;

[0041] S4. Carbonization: The silver-deposited modified ZnO / TiO2 coated hollow glass microspheres were heated to 1400°C and carbonized for 4 hours to obtain the product.

[0042] Preparation Example 3 Preparation method of nano-microsphere material

[0043] The following steps are involved:

[0044] S1. Preparation of ZnO / TiO2 coated hollow glass microspheres: 6 g zinc acetate and 11 g tetrabutyl titanate were dissolved in 500 mL ethanol, 27 g hollow glass microspheres were added, 20 mL 25 wt% ammonia solution was added dropwise, 1.5 g polyethylene glycol 200 was added, heated to 55°C, stirred for reaction for 3 h, centrifuged, washed, dried, and calcined at 500°C for 2 h to obtain ZnO / TiO2 coated hollow glass microspheres;

[0045] S2. Tannic acid modification: Tris-HCl solution and NaOH were added to water, the pH value of the aqueous solution was adjusted to 9, 17 g ZnO / TiO2 coated hollow glass microspheres and 8 g tannic acid were added, heated to 65 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain modified ZnO / TiO2 coated hollow glass microspheres;

[0046] S3. Silver deposition: 5.5 g of silver nitrate was dissolved in 200 mL of water, 25 wt% ammonia solution was added dropwise until the precipitate disappeared, 20 g of modified ZnO / TiO2 coated hollow glass microspheres were added, stirred and mixed for 15 min, 100 mL of an aqueous solution containing 8.5 g of glucose was added dropwise, heated to 92 ° C, stirred for 3 h, centrifuged, washed, and dried to obtain silver-deposited modified ZnO / TiO2 coated hollow glass microspheres;

[0047] S4. Carbonization: The silver-deposited modified ZnO / TiO2 coated hollow glass microspheres were heated to 1300°C and carbonized for 3 hours to obtain the product.

[0048] Comparative Preparation Example 1

[0049] Compared with Preparation Example 3, the difference is that zinc acetate is not added in step S1.

[0050] The details are as follows:

[0051] S1. Preparation of TiO2-coated hollow glass microspheres: Dissolve 17 g of tetrabutyl titanate in 500 mL of ethanol, add 27 g of hollow glass microspheres, drop 20 mL of 25 wt% ammonia solution, add 1.5 g of polyethylene glycol 200, heat to 55 ° C, stir to react for 3 h, centrifuge, wash, dry, and calcine at 500 ° C for 2 h to obtain TiO2-coated hollow glass microspheres.

[0052] Comparative Preparation Example 2

[0053] Compared with Preparation Example 3, the difference is that tetrabutyl titanate is not added in step S1.

[0054] The details are as follows:

[0055] S1. Preparation of ZnO-coated hollow glass microspheres: Dissolve 17 g zinc acetate in 500 mL ethanol, add 27 g hollow glass microspheres, drop 20 mL 25 wt% ammonia solution, add 1.5 g polyethylene glycol 200, heat to 55 ° C, stir to react for 3 h, centrifuge, wash, dry, and calcine at 500 ° C for 2 h to obtain ZnO-coated hollow glass microspheres.

[0056] Comparative Preparation Example 3

[0057] Compared with Preparation Example 3, the difference is that steps S2 and S4 are not performed.

[0058] The details are as follows:

[0059] S1. Preparation of ZnO / TiO2 coated hollow glass microspheres: 6 g zinc acetate and 11 g tetrabutyl titanate were dissolved in 500 mL ethanol, 27 g hollow glass microspheres were added, 20 mL 25 wt% ammonia solution was added dropwise, 1.5 g polyethylene glycol 200 was added, heated to 55°C, stirred for reaction for 3 h, centrifuged, washed, dried, and calcined at 500°C for 2 h to obtain ZnO / TiO2 coated hollow glass microspheres;

[0060] S2. Silver deposition: 5.5 g of silver nitrate was dissolved in 200 mL of water, and a 25 wt% ammonia solution was added dropwise until the precipitate disappeared. 20 g of modified ZnO / TiO2-coated hollow glass microspheres were added, and the mixture was stirred for 15 min. 100 mL of an aqueous solution containing 8.5 g of glucose was added dropwise, and the mixture was heated to 92°C and stirred for 3 h. The mixture was centrifuged, washed, and dried to obtain silver-deposited modified ZnO / TiO2-coated hollow glass microspheres, which were the product.

[0061] Comparative Preparation Example 4

[0062] Compared with Preparation Example 3, the difference is that step S3 is not performed.

[0063] The details are as follows:

[0064] S1. Preparation of ZnO / TiO2 coated hollow glass microspheres: 6 g zinc acetate and 11 g tetrabutyl titanate were dissolved in 500 mL ethanol, 27 g hollow glass microspheres were added, 20 mL 25 wt% ammonia solution was added dropwise, 1.5 g polyethylene glycol 200 was added, heated to 55°C, stirred for reaction for 3 h, centrifuged, washed, dried, and calcined at 500°C for 2 h to obtain ZnO / TiO2 coated hollow glass microspheres;

[0065] S2. Tannic acid modification: Tris-HCl solution and NaOH were added to water, the pH value of the aqueous solution was adjusted to 9, 17 g ZnO / TiO2 coated hollow glass microspheres and 8 g tannic acid were added, heated to 65 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain modified ZnO / TiO2 coated hollow glass microspheres;

[0066] S3. Carbonization: The modified ZnO / TiO2 coated hollow glass microspheres were heated to 1300°C and carbonized for 3 hours to obtain the product.

[0067] Comparative Preparation Example 5

[0068] Compared with Preparation Example 3, the difference is that step S4 is not performed.

[0069] The details are as follows:

[0070] S1. Preparation of ZnO / TiO2 coated hollow glass microspheres: 6 g zinc acetate and 11 g tetrabutyl titanate were dissolved in 500 mL ethanol, 27 g hollow glass microspheres were added, 20 mL 25 wt% ammonia solution was added dropwise, 1.5 g polyethylene glycol 200 was added, heated to 55°C, stirred for reaction for 3 h, centrifuged, washed, dried, and calcined at 500°C for 2 h to obtain ZnO / TiO2 coated hollow glass microspheres;

[0071] S2. Tannic acid modification: Tris-HCl solution and NaOH were added to water, the pH value of the aqueous solution was adjusted to 9, 17 g ZnO / TiO2 coated hollow glass microspheres and 8 g tannic acid were added, heated to 65 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain modified ZnO / TiO2 coated hollow glass microspheres;

[0072] S3. Silver deposition: 5.5 g of silver nitrate was dissolved in 200 mL of water, and a 25 wt% ammonia solution was added dropwise until the precipitate disappeared. 20 g of modified ZnO / TiO2-coated hollow glass microspheres were added, and the mixture was stirred for 15 min. 100 mL of an aqueous solution containing 8.5 g of glucose was added dropwise, and the mixture was heated to 92°C and stirred for 3 h. The mixture was centrifuged, washed, and dried to obtain silver-deposited modified ZnO / TiO2-coated hollow glass microspheres, which were the product.

[0073] Preparation Example 4 Preparation method of nano-microsphere material

[0074] The following steps are involved:

[0075] S1. Preparation of ZnO / TiO2 coated hollow glass microspheres: 6 g zinc acetate and 11 g tetrabutyl titanate were dissolved in 500 mL ethanol, 27 g hollow glass microspheres were added, 20 mL 25 wt% ammonia solution was added dropwise, 1.5 g polyethylene glycol 200 was added, heated to 55°C, stirred for reaction for 3 h, centrifuged, washed, dried, and calcined at 500°C for 2 h to obtain ZnO / TiO2 coated hollow glass microspheres;

[0076] S2. Tannic acid modification: Tris-HCl solution and NaOH were added to water, the pH value of the aqueous solution was adjusted to 9, 17 g ZnO / TiO2 coated hollow glass microspheres and 8 g tannic acid were added, heated to 65 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain modified ZnO / TiO2 coated hollow glass microspheres;

[0077] S3. Silver deposition: 5.5 g of silver nitrate was dissolved in 200 mL of water, 25 wt% ammonia solution was added dropwise until the precipitate disappeared, 20 g of modified ZnO / TiO2 coated hollow glass microspheres were added, stirred and mixed for 15 min, 100 mL of an aqueous solution containing 8.5 g of glucose was added dropwise, heated to 92 ° C, stirred for 3 h, centrifuged, washed, and dried to obtain silver-deposited modified ZnO / TiO2 coated hollow glass microspheres;

[0078] S4. Carbonization: The silver-deposited modified ZnO / TiO2 coated hollow glass microspheres were heated to 1300°C and carbonized for 3 h to obtain the product;

[0079] S5. Alkali treatment: 10 g of the product obtained in step S4 was added to 100 mL of a 10 wt% NaOH solution, stirred at 40 ° C for 20 min, centrifuged, washed, and dried to obtain an alkali-treated product;

[0080] S6. Flame retardant modification: The alkali-treated product was added to a 12 wt% phytic acid solution, stirred for reaction for 20 min, centrifuged, washed, dried, and then added to a 4 wt% aluminum chloride solution, stirred for reaction for 30 min, centrifuged, washed, dried to obtain the product.

[0081] Preparation Example 5 Preparation method of nano-microsphere material

[0082] The following steps are involved:

[0083] S1. Preparation of ZnO / TiO2 coated hollow glass microspheres: 6 g zinc acetate and 11 g tetrabutyl titanate were dissolved in 500 mL ethanol, 27 g hollow glass microspheres were added, 20 mL 25 wt% ammonia solution was added dropwise, 1.5 g polyethylene glycol 200 was added, heated to 55°C, stirred for reaction for 3 h, centrifuged, washed, dried, and calcined at 500°C for 2 h to obtain ZnO / TiO2 coated hollow glass microspheres;

[0084] S2. Tannic acid modification: Tris-HCl solution and NaOH were added to water, the pH value of the aqueous solution was adjusted to 9, 17 g ZnO / TiO2 coated hollow glass microspheres and 8 g tannic acid were added, heated to 65 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain modified ZnO / TiO2 coated hollow glass microspheres;

[0085] S3. Silver deposition: 5.5 g of silver nitrate was dissolved in 200 mL of water, 25 wt% ammonia solution was added dropwise until the precipitate disappeared, 20 g of modified ZnO / TiO2 coated hollow glass microspheres were added, stirred and mixed for 15 min, 100 mL of an aqueous solution containing 8.5 g of glucose was added dropwise, heated to 92 ° C, stirred for 3 h, centrifuged, washed, and dried to obtain silver-deposited modified ZnO / TiO2 coated hollow glass microspheres;

[0086] S4. Carbonization: The silver-deposited modified ZnO / TiO2 coated hollow glass microspheres were heated to 1300°C and carbonized for 3 h to obtain the product;

[0087] S5. Alkali treatment: 10 g of the product obtained in step S4 was added to 100 mL of a 12 wt% KOH solution, stirred at 50 ° C for 40 min, centrifuged, washed, and dried to obtain an alkali-treated product;

[0088] S6. Flame retardant modification: The alkali-treated product was added to a 15 wt% phytic acid solution, stirred for reaction for 20 min, centrifuged, washed, dried, and then added to a 6 wt% aluminum nitrate solution, stirred for reaction for 30 min, centrifuged, washed, dried to obtain the product.

[0089] Preparation Example 6 Preparation method of nano-microsphere material

[0090] The following steps are involved:

[0091] S1. Preparation of ZnO / TiO2 coated hollow glass microspheres: 6 g zinc acetate and 11 g tetrabutyl titanate were dissolved in 500 mL ethanol, 27 g hollow glass microspheres were added, 20 mL 25 wt% ammonia solution was added dropwise, 1.5 g polyethylene glycol 200 was added, heated to 55°C, stirred for reaction for 3 h, centrifuged, washed, dried, and calcined at 500°C for 2 h to obtain ZnO / TiO2 coated hollow glass microspheres;

[0092] S2. Tannic acid modification: Tris-HCl solution and NaOH were added to water, the pH value of the aqueous solution was adjusted to 9, 17 g ZnO / TiO2 coated hollow glass microspheres and 8 g tannic acid were added, heated to 65 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain modified ZnO / TiO2 coated hollow glass microspheres;

[0093] S3. Silver deposition: 5.5 g of silver nitrate was dissolved in 200 mL of water, 25 wt% ammonia solution was added dropwise until the precipitate disappeared, 20 g of modified ZnO / TiO2 coated hollow glass microspheres were added, stirred and mixed for 15 min, 100 mL of an aqueous solution containing 8.5 g of glucose was added dropwise, heated to 92 ° C, stirred for 3 h, centrifuged, washed, and dried to obtain silver-deposited modified ZnO / TiO2 coated hollow glass microspheres;

[0094] S4. Carbonization: The silver-deposited modified ZnO / TiO2 coated hollow glass microspheres were heated to 1300°C and carbonized for 3 h to obtain the product;

[0095] S5. Alkali treatment: 10 g of the product obtained in step S4 was added to 100 mL of a 11 wt% KOH solution, stirred at 45 ° C for 30 min, centrifuged, washed, and dried to obtain an alkali-treated product;

[0096] S6. Flame retardant modification: The alkali-treated product was added to a 13 wt% phytic acid solution, stirred for reaction for 20 min, centrifuged, washed, dried, and then added to a 5 wt% aluminum nitrate solution, stirred for reaction for 30 min, centrifuged, washed, dried to obtain the product.

[0097] Comparative Preparation Example 6

[0098] Compared with Preparation Example 3, the difference is that no phytic acid solution is added in step S6.

[0099] The details are as follows:

[0100] S6. Flame retardant modification: add the alkali-treated product into a 5 wt% aluminum nitrate solution, stir and react for 30 minutes, centrifuge, wash, and dry to obtain the product.

[0101] Comparative Preparation Example 7

[0102] Compared with Preparation Example 3, the difference is that no aluminum nitrate solution is added in step S6.

[0103] The details are as follows:

[0104] S6. Flame retardant modification: the alkali-treated product was added into a 13 wt % phytic acid solution, stirred for reaction for 20 min, centrifuged, washed, and dried to obtain the product.

[0105] Example 1

[0106] This embodiment provides a composite coating containing nano-bead material.

[0107] Raw material composition (parts by weight): 15 parts of the nano-bead material prepared in Preparation Example 1, 150 parts of water-based polyurethane, 0.3 parts of silane coupling agent KH570, 0.2 parts of leveling agent BYK-530 (purchased from BYK Chemical Company), 0.1 parts of defoaming agent QX-202G (purchased from Changzhou Jiangdong Additive Co., Ltd.), and 150 parts of water.

[0108] The preparation method comprises the following steps: adding the nano-bead material into water, adding the silane coupling agent KH570, stirring for reaction, adjusting the pH value of the solution to 8.5, stirring and dispersing for 1 hour, adding the waterborne polyurethane, the leveling agent BYK-530 and the defoaming agent QX-202G, stirring and dispersing for 2 hours, and obtaining a composite coating containing the nano-bead material.

[0109] Example 2

[0110] This embodiment provides a composite coating containing nano-bead material.

[0111] Raw material composition (parts by weight): 20 parts of the nano-bead material obtained in Preparation Example 2, 170 parts of water-based polyurethane, 0.5 parts of silane coupling agent KH570, 0.4 parts of leveling agent BYK-530 (purchased from BYK Chemical Company), 0.3 parts of defoaming agent QX-202G (purchased from Changzhou Jiangdong Additive Co., Ltd.), and 200 parts of water.

[0112] The preparation method comprises the following steps: adding the nano-bead material into water, adding the silane coupling agent KH570, stirring for reaction, adjusting the pH value of the solution to 9.5, stirring and dispersing for 2 hours, adding the waterborne polyurethane, the leveling agent BYK-530 and the defoaming agent QX-202G, stirring and dispersing for 4 hours, and obtaining a composite coating containing the nano-bead material.

[0113] Example 3

[0114] This embodiment provides a composite coating containing nano-bead material.

[0115] Raw material composition (parts by weight): 17 parts of the nano-bead material obtained in Preparation Example 3, 160 parts of water-based polyurethane, 0.4 parts of silane coupling agent KH570, 0.3 parts of leveling agent BYK-530 (purchased from BYK Chemical Company), 0.2 parts of defoaming agent QX-202G (purchased from Changzhou Jiangdong Additive Co., Ltd.), and 170 parts of water.

[0116] The preparation method comprises the following steps: adding the nano-bead material into water, adding the silane coupling agent KH570, stirring for reaction, adjusting the pH value of the solution to 9, stirring and dispersing for 1.5 hours, adding waterborne polyurethane, leveling agent BYK-530 and defoamer QX-202G, stirring and dispersing for 3 hours, and obtaining a composite coating containing the nano-bead material.

[0117] Embodiment 4-6

[0118] Compared with Example 3, the difference is that the nano-microbead material is prepared by Preparation Examples 4-6.

[0119] Comparative Examples 1-5

[0120] Compared with Example 3, the difference is that the nano-bead material is prepared by Comparative Preparation Examples 1-5.

[0121] Comparative Examples 6-7

[0122] Compared with Example 6, the difference is that the nano-microbead material is prepared by Comparative Preparation Examples 6 and 7.

[0123] Test Example 1 Thermal Insulation Performance

[0124] A blank glass plate and a glass plate coated with a composite coating containing nano-bead material obtained in Examples 1-6 or Comparative Examples 1-7 (all with a film thickness of 1 mm) were placed in an insulation foam box of the same specification, and thermocouple thermometers were installed inside the insulation box (about 15 cm away from the glass plate) and on the glass surface to measure temperature changes. The simulated heat source was a 500W iodine tungsten lamp, which was fixed above the insulation box, about 30 cm away from the glass plate, and the thermometer reading was recorded after 5 minutes. When sunlight was used as the heat source, the thermometer reading was recorded after 30 minutes. The results are shown in Table 1.

[0125] Table 1

[0126] Group Temperature after 5 minutes of iodine tungsten lamp (℃) Temperature after 30 minutes of sunlight (℃) Blank Group 97.8 14.5 Example 1 65.3 7.8 Example 2 65.7 7.9 Example 3 64.9 7.5 Example 4 64.2 7.4 Example 5 64.0 7.4 Example 6 63.8 7.2 Comparative Example 1 74.2 8.9 Comparative Example 2 75.5 9.1 Comparative Example 3 78.9 9.7 Comparative Example 4 76.9 9.3 Comparative Example 5 75.2 9.2 Comparative Example 6 67.9 8.2 Comparative Example 7 68.2 8.4

[0127] It can be seen from the above table that the composite coatings containing nano-bead materials prepared in Examples 1-6 of the present invention have good thermal insulation properties.

[0128] Test Example 2

[0129] The composite coatings containing nano-bead materials prepared in Examples 1-6 or Comparative Examples 1-7 were subjected to performance tests. The results are shown in Table 2.

[0130] According to GB / T6739-2006 "Determination of paint film hardness by pencil method for paints and varnishes" and GB / T1720-1979 "Determination of paint film adhesion", the hardness and adhesion are tested using a coated glass sheet with a film thickness of 1 mm.

[0131] According to GB / T1733-1993 “Determination of water resistance of paint films” (Method A), soak the coated glass sheet (film thickness 1 mm) in (23±2)℃ distilled water for 24 hours and observe the coating condition.

[0132] According to GB / T1735-2009 “Determination of heat resistance of paints and varnishes”, place a glass sheet (film thickness 1.2 mm) in an oven and heat it to (100±5)°C and maintain it for 3 hours to observe whether the coating changes.

[0133] Place the coating in a laboratory and store it under natural conditions (temperature 18-35°C, humidity 40%-90%) for 6 months to observe whether there is obvious settling or stratification and other adverse conditions to determine its storage stability.

[0134] Table 2

[0135]

[0136] It can be seen from the above table that the composite coatings containing nano-bead materials prepared in Examples 1-6 of the present invention have good comprehensive properties.

[0137] Test Example 3

[0138] The composite coatings containing nano-bead materials prepared in Examples 1-6 or Comparative Examples 1-7 were tested for mechanical properties. The results are shown in Table 3.

[0139] In accordance with GB / T1040.1-2018, an electronic universal testing machine was used to test the tensile strength and elongation at break of square samples of the coating (100mm×10mm×2mm), and the clamp rising rate was 500mm / min.

[0140] Table 3

[0141] Group Tensile strength(MPa) Elongation at break (%) Example 1 32 185 Example 2 34 187 Example 3 37 188 Example 4 42 192 Example 5 40 190 Example 6 45 195 Comparative Example 1 26 169 Comparative Example 2 27 165 Comparative Example 3 29 174 Comparative Example 4 23 159 Comparative Example 5 30 180 Comparative Example 6 40 187 Comparative Example 7 38 185

[0142] It can be seen from the above table that the composite coatings containing nano-bead materials prepared in Examples 1-6 of the present invention have good mechanical strength.

[0143] Test Example 4 Test of oxygen index

[0144] The composite coatings containing nano-bead materials prepared in Examples 1-6 or Comparative Examples 1-7 were tested for limiting oxygen index. The results are shown in Table 4.

[0145] Oxygen index test: The coating is made into rectangular strips of 150mm×50mm, 5 in each group, and the flame burns for 3 minutes. The oxygen concentration when it reaches 50mm from the top is the oxygen index of the sample.

[0146] Table 4

[0147]

[0148]

[0149] It can be seen from the above table that the composite coatings containing nano-bead materials prepared in Examples 1-6 of the present invention have good flame retardant properties.

[0150] Test Example 5: UV Shielding Performance

[0151] The composite coatings containing nano-bead materials prepared in Examples 1-6 or Comparative Examples 1-7 were tested for UV shielding performance. The results are shown in Table 5.

[0152] The test is conducted using the method in GB / T18830-2009 and UV-visible diffuse reflection. The formula is as follows:

[0153]

[0154] Where: Ε(λ) is the spectral radiation intensity of sunlight, W / (m 2 ·nm); ε(λ) is the relative erythema effect value; T i (λ) is the spectral transmittance of the sample at wavelength λ; Δλ is the wavelength interval, nm.

[0155] Table 5

[0156]

[0157]

[0158] It can be seen from the above table that the composite coatings containing nano-bead materials prepared in Examples 1-6 of the present invention have good ultraviolet shielding performance.

[0159] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A composite coating containing nano-bead material, characterized in that: The invention is prepared from the following raw materials in parts by weight: 15-20 parts of nano-bead material, 150-170 parts of waterborne polyurethane, 0.3-0.5 parts of silane coupling agent, 0.2-0.4 parts of leveling agent, 0.1-0.3 parts of defoaming agent and 150-200 parts of water.

2. The composite coating containing nano-bead material according to claim 1, characterized in that: The preparation method of the nano-microsphere material comprises the following steps: S1. Preparation of ZnO / TiO2 coated hollow glass microspheres: dissolving zinc acetate and tetrabutyl titanate in ethanol, adding hollow glass microspheres, dropping ammonia solution, adding polyethylene glycol, heating and stirring to react, centrifuging, washing, drying, calcining, and obtaining ZnO / TiO2 coated hollow glass microspheres; S2. Tannic acid modification: adding Tris-HCl solution and alkali into water, adjusting the pH value of the aqueous solution, adding ZnO / TiO2 coated hollow glass microspheres and tannic acid, heating and stirring to react, centrifuging, washing, drying, and obtaining modified ZnO / TiO2 coated hollow glass microspheres; S3. Silver deposition: dissolve silver nitrate in water, add aqueous ammonia solution until the precipitate disappears, add modified ZnO / TiO2 coated hollow glass microspheres, stir and mix evenly, add aqueous glucose solution, heat and stir to react, centrifuge, wash, and dry to obtain silver-deposited modified ZnO / TiO2 coated hollow glass microspheres; S4. Carbonization: heat and carbonize the silver-deposited modified ZnO / TiO2 coated hollow glass microspheres to obtain the product.

3. The composite coating containing nano-bead material according to claim 2, characterized in that: In step S1, the mass ratio of zinc acetate, tetrabutyl titanate, hollow glass microspheres and polyethylene glycol is 5-7:10-12:25-30:1-2, the concentration of the ammonia solution is 24-25wt%, the temperature of the heating and stirring reaction is 50-60°C, the time is 2-4h, and the calcination temperature is 450-550°C, and the time is 1-3h.

4. The composite coating containing nano-bead material according to claim 2, characterized in that: In step S2, the pH value of the aqueous solution is adjusted to 8.5-9.5, the mass ratio of the ZnO / TiO2 coated hollow glass microspheres and tannic acid is 15-20:7-10, the temperature of the heating and stirring reaction is 60-70°C, and the time is 1-3h.

5. The composite coating containing nano-bead material according to claim 2, characterized in that: In step S3, the mass ratio of silver nitrate, modified ZnO / TiO2 coated hollow glass microspheres and glucose is 4-7:15-25:7-10, the concentration of the ammonia solution is 24-25wt%, the temperature of the heating and stirring reaction is 90-95°C, and the time is 2-4h.

6. The composite coating containing nano-bead material according to claim 2, characterized in that: The carbonization temperature in step S4 is 1200-1400° C. and the time is 2-4 hours.

7. The composite coating containing nano-bead material according to claim 2, characterized in that: The method for preparing the nano-bead material further comprises the following steps after step S4: S5. alkali treatment: adding the product obtained in step S4 to alkali solution, stirring for reaction, centrifuging, washing, and drying to obtain an alkali-treated product; S6. flame retardant modification: adding the alkali-treated product to a phytic acid solution, stirring for reaction, centrifuging, washing, and drying, and then adding it to an aluminum salt solution, stirring for reaction, centrifuging, washing, and drying to obtain a product.

8. The composite coating containing nano-bead material according to claim 7, characterized in that: The alkali solution in step S5 is a 10-12wt% NaOH or KOH solution, the stirring reaction temperature is 40-50°C, and the time is 20-40min; the concentration of the phytic acid solution in step S6 is 12-15wt%, the concentration of the aluminum salt solution is 4-6wt%, and the aluminum salt is selected from at least one of aluminum chloride, aluminum nitrate, and aluminum sulfate.

9. A method for preparing a composite coating containing nano-bead material according to any one of claims 1 to 8, characterized in that: The following steps are involved: Add the nano-bead material into water, add the silane coupling agent, stir to react, adjust the solution pH to 8.5-9.5, stir and disperse for 1-2 hours, add waterborne polyurethane, leveling agent and defoamer, stir and disperse for 2-4 hours, and obtain a composite coating containing the nano-bead material.

10. Use of the composite coating containing the nano-bead material according to any one of claims 1 to 8 in thermal insulation building materials.

Citation Information

Patent Citations

  • Heat reflection paint with hollow glass microballoon

    CN101712835B

  • Method for preparing nano silver and titanium dioxide thin films on surfaces of hollow glass beads

    CN103007931A

  • SiO2 aerogel coating and preparation method thereof

    CN117264505A

Cited By

  • Aqueous aerogel heat-insulation thick intermediate coat and preparation method thereof

    CN120272060A