Modified spherical silicon and application thereof in dealcoholized condensed silicone sealant
By modifying the sphere silicone twice, it is closely combined with the dehydrogenated condensation silicone sealant during the curing process, the existing silicone sealant is solved in the field of waterproof sealing of building exterior walls. The problem of this has significantly improved the performance of the sealant.
Patent Information
- Application Number
- CN202411085237.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to modified spherical silica and application of the modified spherical silica in the field of dealcoholization condensation type silicone sealant. Background Art
[0002] Spherical silicon, also known as spherical silicon powder, is an amorphous silicon powder made from quartz minerals. Spherical silicon has the advantages of high dielectric properties, high heat resistance, high moisture resistance, high filling volume, low expansion, low stress, and low friction coefficient. It is widely used in high-tech fields such as home building materials, aerospace, fine chemicals, electronic substrates, and daily cosmetics.
[0003] Silicone sealant is a silicone rubber adhesive made of polydimethylsiloxane as the main raw material, supplemented with crosslinking agents, catalysts, fillers and other additives. It is crosslinked and cured at room temperature through the action of moisture in the air. Silicone sealant has the characteristics of good sealing, strong adhesion, high toughness, good weather resistance, and adaptability to environmental changes. It is widely used in home furnishing, building materials, and electronics. Dealcoholization condensation type silicone sealant is based on terminal hydroxyl polydimethylsiloxane. By adding alkoxy-containing crosslinking agents, the alkoxy crosslinking agents are hydrolyzed under the action of moisture, and then condensed with terminal hydroxyl polydimethylsiloxane to remove small molecule alcohols, thereby obtaining a sealant.
[0004] CN111019594A discloses an alcohol-type silicone sealant and a preparation method thereof. The silicone sealant described in the invention has the characteristics of long-term storage stability, excellent weather resistance, and high displacement capacity, and its various technical indicators all meet the GB / T14683-F-50 standard, and is non-corrosive to most building materials. In addition, the silicone sealant of the invention releases alcohol small molecules during the curing process, which is more environmentally friendly than the current dealkonone oxime type products.
[0005] CN115109559A discloses a high-strength silicone sealant, which contains a silane-modified crosslinking agent containing a polyether chain segment with multiple hydrolyzable groups. The silane-modified crosslinking agent has multiple hydrolyzable groups. The hydrolyzed silanol groups can react with α,ω-dihydroxy polydimethylsiloxane to significantly improve the cohesive strength of the silicone sealant. At the same time, the silane-modified crosslinking agent contains a flexible polyether chain segment, which can improve the elasticity of the high-strength silicone sealant. It is expected to further expand the scope of use of silicone sealants.
[0006] CN117467401A discloses an anti-aging silicone sealant and a preparation method thereof. The invention adds a modified filler to the silicone sealant, wherein the modified filler is a spherical silica mixture with a gradient median particle size loaded with a hindered phenol structure compound. Firstly, silica has high stability, good formability and workability, and the addition of silica can improve the flexibility and durability of the silicone sealant.
[0007] With the continuous development of technology, the formula and application occasions of silicone sealants are also constantly updated. In the field of building exterior wall waterproof sealing, sealants are required to have better water resistance and higher strength. In the application of existing sealants in this field, there are still problems such as water resistance and strength that cannot meet the application requirements. Summary of the invention
[0008] In order to solve the above technical problems, the present invention provides a modified spherical silica, which is modified twice to introduce active functional groups capable of reacting with dealcoholization condensation type silicone sealant on the surface of the spherical silica. During the curing and cross-linking process of the dealcoholization condensation type silicone sealant, the active functional groups on the surface of the spherical silica participate in the curing and cross-linking reaction, so that the spherical silica and the dealcoholization condensation type silicone sealant are tightly combined through chemical bonds, thereby improving the strength and water barrier properties of the dealcoholization condensation type silicone sealant.
[0009] In order to achieve the above object, the present invention adopts the following technical solutions: A preparation process of modified spherical silicon is as follows: Step 1: Add 10-15 parts of spherical silica to 100-200 mL of a 10 wt% sodium hydroxide aqueous solution, stir in a water bath at 70-80° C. for 3-5 hours, cool to room temperature after the reaction, filter, wash with water, and dry at 60° C. for 10-12 hours to obtain surface hydroxylated spherical silica; Step 2: adding 1-3 parts of an amino-containing silane coupling agent to 50-100 mL of a 90 wt% ethanol aqueous solution for hydrolysis, and adjusting the pH value of the ethanol aqueous solution to 7.5-10 with a pH adjuster, wherein the pH adjuster includes one of sodium hydroxide or potassium hydroxide; Step 3: Add the surface hydroxylated spherical silica prepared in step 1 to the hydrolysis solution prepared in step 2; reflux the reaction for 2 to 3 hours under stirring, filter, wash and dry to obtain aminosilane coupling agent-modified spherical silica.
[0010] Step 4: Add the aminosilane coupling agent-modified spherical silica prepared in step 3 to a container containing 100-200 mL of toluene, introduce nitrogen to replace the air, then add 3-5 parts of epoxy-containing silane coupling agent to the container, react at 30-80°C for 1-2h, filter, wash and dry to obtain surface-modified spherical silica.
[0011] In the step 1, the median particle size D50 of the spherical silicon is 1-5 μm; In the step 2, the amino-containing silane coupling agent is selected from: one of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane or γ-aminopropylmethyldiethoxysilane; In step 4, the epoxy-containing silane coupling agent is selected from: γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane; The present invention also provides modified spheroidal silica obtained by the preparation process of the modified spheroidal silica.
[0012] The invention also provides an application of the modified spherical silica in dealcoholization condensation type silicone sealant.
[0013] The specific application methods are as follows: The dealcoholization condensation type silicone sealant comprises the following components in parts by weight: 100 parts of α, ω-dihydroxy polydimethylsiloxane, 10-30 parts of dimethyl silicone oil, 30-100 parts of modified spherical silica, 5-10 parts of fumed silica, 8-15 parts of a crosslinking agent, and 0.5-3 parts of a catalyst.
[0014] The viscosity of the α,ω-dihydroxy polydimethylsiloxane at 25° C. is 20000-100000 mPa·s; The viscosity of the dimethyl silicone oil at 25° C. is 100-1000 mPa·s; The modified spheroidal silica is the modified spheroidal silica obtained by the preparation process of the modified spheroidal silica of the present invention; The fumed silica is a hydrophobic fumed silica, and the specific surface area of the hydrophobic fumed silica is 100-300 m 2 / g; The crosslinking agent is selected from: a combination of one or more of methyltrimethoxysilane, vinyltrimethoxysilane, methyltriethoxysilane, vinyltriethoxysilane, tetramethoxysilane and tetraethoxysilane; The catalyst is selected from the group consisting of one or more of isopropyl titanate, butyl titanate, dibutyltin dilaurate, and stannous octoate.
[0015] The preparation process of the dealcoholization condensation type silicone sealant is as follows: 100 parts of α, ω-dihydroxy polydimethylsiloxane, 10-30 parts of dimethyl silicone oil, 30-100 parts of modified spherical silica, and 5-10 parts of fumed silica are heated in a planetary mixer, and the mixture is mixed at a vacuum of 0.09 MPa and a rotation speed of 100-200 rpm for 30-60 minutes to obtain a mixture, and then 8-15 parts of a cross-linking agent and 0.5-3 parts of a catalyst are added to the mixture, and the mixture is mixed at a vacuum of 0.09 MPa and a rotation speed of 100-200 rpm for 30-60 minutes to prepare a dealcoholization condensation type silicone sealant.
[0016] Compared with the prior art, the present invention has the following beneficial effects: The modified spherical silica prepared by the process of the present invention is firstly treated on the surface of the spherical silica with an amino-containing silane coupling agent, and the alkoxy groups of the aminosilane coupling agent are hydrolyzed to generate silanol groups, which are dehydrated and condensed with the silanol groups on the surface of the spherical silica to obtain amino-modified spherical silica, and then the epoxy groups of the epoxy-containing silane coupling agent are reacted with the amino groups on the surface of the amino-modified spherical silica to graft the alkoxy groups of the epoxysilane coupling agent onto the surface of the spherical silica, which not only organically modifies the surface of the spherical silica but also retains the alkoxy groups that can react.
[0017] After the obtained modified spherical silica is added to the silicone sealant, during the curing and cross-linking stage, the alkoxy groups on the surface of the spherical silica are hydrolyzed and undergo a dehydration condensation reaction with the matrix component α, ω-dihydroxypolydimethylsiloxane and the cross-linking agent component of the dealcoholization condensation type silicone sealant, so that the spherical silica can be bonded to the molecular structure of the silicone sealant through chemical bonds, which can not only improve the mechanical properties of the dealcoholization condensation type silicone sealant, but also improve its water-barrier performance. DETAILED DESCRIPTION
[0018] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0019] Example 1 A preparation process of modified spherical silicon is as follows: Step 1: add 10 parts of spherical silica with a median particle size D50 of 2 µm to 150 mL of a 10 wt% sodium hydroxide aqueous solution, stir in a water bath at 75°C for 3 h, cool to room temperature after the reaction, filter, wash with water, and dry at 60°C for 10 h to obtain surface hydroxylated modified spherical silica; Step 2: adding 2 parts of γ-aminopropyltriethoxysilane to 80 mL of 90 wt% ethanol aqueous solution for hydrolysis, and adjusting the pH value of the ethanol aqueous solution to 8 with sodium hydroxide; Step 3: adding the surface hydroxylated spherulite prepared in step 1 to the hydrolysis solution in step 2; reflux reaction for 2 hours under stirring, filtering, washing and drying to obtain aminosilane coupling agent-modified spherulite; Step 4: Add the aminosilane coupling agent-modified spherical silica prepared in step 3 into a container containing 100 mL of toluene, introduce nitrogen to replace the air, then add 4 parts of γ-glycidyloxypropyltrimethoxysilane to the container, react at 45°C for 1 hour, filter, wash and dry to obtain surface-modified spherical silica.
[0020] Example 2 A preparation process of modified spherical silicon is as follows: Step 1: Add 12 parts of spherical silica with a median particle size D50 of 2 µm to 180 mL of a 10 wt% sodium hydroxide aqueous solution, stir in a water bath at 75°C for 4 h, cool to room temperature after the reaction, filter, wash with water, and dry at 60°C for 12 h to obtain surface hydroxylated spherical silica; Step 2: adding 3 parts of γ-aminopropyltrimethoxysilane to 80 mL of 90 wt% ethanol aqueous solution for hydrolysis, and adjusting the pH value of the ethanol aqueous solution to 8 with potassium hydroxide; Step 3: adding the surface hydroxylated spherulite prepared in step 1 to the hydrolysis solution in step 2; reflux reaction for 3 hours under stirring, filtering, washing and drying to obtain aminosilane coupling agent-modified spherulite; Step 4: Add the aminosilane coupling agent-modified spherical silica prepared in step 3 into a container containing 150 mL of toluene, introduce nitrogen to replace the air, then add 5 parts of γ-glycidyloxypropyltriethoxysilane to the container, react at 50°C for 2 hours, filter, wash and dry to obtain surface-modified spherical silica.
[0021] Example 3 A preparation process of modified spherical silicon is as follows: Step 1: Add 15 parts of spherical silica with a median particle size D50 of 5 µm to 200 mL of a 10 wt% sodium hydroxide aqueous solution, stir in a water bath at 80°C for 5 h, cool to room temperature after the reaction, filter, wash with water, and dry at 60°C for 12 h to obtain surface hydroxylated spherical silica; Step 2: adding 3 parts of γ-aminopropyltrimethoxysilane to 80 mL of 90 wt% ethanol aqueous solution for hydrolysis, and adjusting the pH value of the ethanol aqueous solution to 9 with sodium hydroxide; Step 3: adding the surface hydroxylated spherulite prepared in step 1 to the hydrolysis solution in step 2; reflux reaction for 3 hours under stirring, filtering, washing and drying to obtain aminosilane coupling agent-modified spherulite; Step 4: Add the aminosilane coupling agent-modified spherical silica prepared in step 3 into a container containing 200 mL of toluene, introduce nitrogen to replace the air, then add 5 parts of γ-glycidyloxypropyltrimethoxysilane to the container, react at 50°C for 2 hours, filter, wash and dry to obtain surface-modified spherical silica.
[0022] Comparative Example 1 A preparation process of modified spherical silicon is as follows: Step 1: add 10 parts of spherical silica with a median particle size D50 of 2 µm to 150 mL of a 10 wt% sodium hydroxide aqueous solution, stir in a water bath at 75°C for 3 h, cool to room temperature after the reaction, filter, wash with water, and dry at 60°C for 10 h to obtain surface hydroxylated modified spherical silica; Step 2: adding 2 parts of γ-aminopropyltriethoxysilane to 80 mL of 90 wt% ethanol aqueous solution for hydrolysis, and adjusting the pH value of the ethanol aqueous solution to 8 with sodium hydroxide; Step 3: Add the surface hydroxylated spherical silica prepared in step 1 to the hydrolyzed solution of step 2; reflux the reaction for 2 hours under stirring, filter, wash and dry to obtain aminosilane coupling agent-modified spherical silica.
[0023] Comparative Example 2 A preparation process of modified spherical silicon is as follows: Step 1: add 10 parts of spherical silica with a median particle size D50 of 2 µm to 150 mL of a 10 wt% sodium hydroxide aqueous solution, stir in a water bath at 75°C for 3 h, cool to room temperature after the reaction, filter, wash with water, and dry at 60°C for 10 h to obtain surface hydroxylated modified spherical silica; Step 2: adding 2 parts of γ-glycidyloxypropyltrimethoxysilane to 80 mL of 90 wt% ethanol aqueous solution for hydrolysis, and adjusting the pH value of the ethanol aqueous solution to 8 with sodium hydroxide; Step 3: Add the surface hydroxylated spherical silica prepared in step 1 to the hydrolyzed solution of step 2; reflux the reaction for 2 hours under stirring, filter, wash and dry to obtain epoxy silane coupling agent-modified spherical silica.
[0024] Application Example 1 The dealcoholization condensation type silicone sealant comprises the following components in parts by weight: 100 parts of α, ω-dihydroxy polydimethylsiloxane, 15 parts of dimethyl silicone oil, 40 parts of modified spherical silica, 6 parts of fumed silica, 10 parts of a crosslinking agent, and 1 part of a catalyst; The viscosity of the α,ω-dihydroxy polydimethylsiloxane at 25° C. is 30000 mPa·s; The viscosity of the dimethyl silicone oil at 25° C. is 200 mPa·s; The modified spheroidal silica is the modified spheroidal silica obtained by the modified spheroidal silica preparation process of Example 1 of the present invention; The fumed silica is a hydrophobic fumed silica, and the specific surface area of the hydrophobic fumed silica is 200 m 2 / g; The cross-linking agent is methyltrimethoxysilane; The catalyst is isopropyl titanate; The preparation process of the dealcoholization condensation type silicone sealant is as follows: 100 parts of α, ω-dihydroxy polydimethylsiloxane, 15 parts of dimethyl silicone oil, 40 parts of modified spherical silica, and 6 parts of fumed silica are heated in a planetary mixer, and the mixture is mixed at a vacuum of 0.09 MPa and a rotation speed of 100 rpm for 30 minutes to obtain a mixture. Thereafter, 10 parts of a cross-linking agent and 1 part of a catalyst are added to the mixture, and the mixture is mixed at a vacuum of 0.09 MPa and a rotation speed of 150 rpm for 40 minutes to prepare the dealcoholization condensation type silicone sealant.
[0025] Application Example 2 The dealcoholization condensation type silicone sealant comprises the following components in parts by weight: 100 parts of α, ω-dihydroxy polydimethylsiloxane, 20 parts of dimethyl silicone oil, 50 parts of modified spherical silica, 8 parts of fumed silica, 12 parts of a crosslinking agent, and 2 parts of a catalyst; The viscosity of the α,ω-dihydroxy polydimethylsiloxane at 25° C. is 40000 mPa·s; The viscosity of the dimethyl silicone oil at 25° C. is 100 mPa·s; The modified spheroidal silica is the modified spheroidal silica obtained by the modified spheroidal silica preparation process of Example 2 of the present invention; The fumed silica is a hydrophobic fumed silica, and the specific surface area of the hydrophobic fumed silica is 100 m 2 / g; The cross-linking agent is methyltriethoxysilane; The catalyst is dibutyltin dilaurate; The preparation process of the dealcoholization condensation type silicone sealant is as follows: 100 parts of α, ω-dihydroxy polydimethylsiloxane, 20 parts of dimethyl silicone oil, 50 parts of modified spherical silica, and 8 parts of fumed silica are heated in a planetary mixer, and the mixture is mixed at a vacuum of 0.09 MPa and a rotation speed of 150 rpm for 40 minutes to obtain a mixture. Thereafter, 12 parts of a cross-linking agent and 2 parts of a catalyst are added to the mixture, and the mixture is mixed at a vacuum of 0.09 MPa and a rotation speed of 150 rpm for 50 minutes to prepare the dealcoholization condensation type silicone sealant.
[0026] Application Example 3 The dealcoholization condensation type silicone sealant comprises the following components in parts by weight: 100 parts of α, ω-dihydroxy polydimethylsiloxane, 30 parts of dimethyl silicone oil, 60 parts of modified spherical silica, 10 parts of fumed silica, 15 parts of a crosslinking agent, and 2 parts of a catalyst; The viscosity of the α,ω-dihydroxy polydimethylsiloxane at 25° C. is 50000 mPa·s; The viscosity of the dimethyl silicone oil at 25° C. is 150 mPa·s; The modified spheroidal silica is the modified spheroidal silica obtained by the modified spheroidal silica preparation process of Example 3 of the present invention; The fumed silica is a hydrophobic fumed silica, and the specific surface area of the hydrophobic fumed silica is 200 m 2 / g; The cross-linking agent is methyltriethoxysilane; The catalyst is dibutyltin dilaurate; The preparation process of the dealcoholization condensation type silicone sealant is as follows: 100 parts of α, ω-dihydroxy polydimethylsiloxane, 30 parts of dimethyl silicone oil, 60 parts of modified spherical silica, and 10 parts of fumed silica are heated in a planetary mixer, and the mixture is mixed at a vacuum of 0.09 MPa and a rotation speed of 150 rpm for 50 minutes to obtain a mixture. Thereafter, 15 parts of a cross-linking agent and 2 parts of a catalyst are added to the mixture, and the mixture is mixed at a vacuum of 0.09 MPa and a rotation speed of 150 rpm for 60 minutes to prepare the dealcoholization condensation type silicone sealant.
[0027] Comparative Application Example 1 The dealcoholization condensation type silicone sealant comprises the following components in parts by weight: 100 parts of α, ω-dihydroxy polydimethylsiloxane, 15 parts of dimethyl silicone oil, 40 parts of spherical silica, 6 parts of fumed silica, 10 parts of a crosslinking agent, and 1 part of a catalyst; The viscosity of the α,ω-dihydroxy polydimethylsiloxane at 25° C. is 30000 mPa·s; The viscosity of the dimethyl silicone oil at 25° C. is 200 mPa·s; The spherical silica is the unmodified spherical silica with a median particle size D50 of 2 μm used in Example 1 of the present invention; The fumed silica is a hydrophobic fumed silica, and the specific surface area of the hydrophobic fumed silica is 200 m 2 / g; The cross-linking agent is methyltrimethoxysilane; The catalyst is isopropyl titanate; The preparation process of the dealcoholization condensation type silicone sealant is as follows: 100 parts of α, ω-dihydroxy polydimethylsiloxane, 15 parts of dimethyl silicone oil, 40 parts of spherical silica, and 6 parts of fumed silica are heated in a planetary mixer, and the mixture is mixed at a vacuum of 0.09 MPa and a rotation speed of 100 rpm for 30 minutes to obtain a mixture. Thereafter, 10 parts of a cross-linking agent and 1 part of a catalyst are added to the mixture, and the mixture is mixed at a vacuum of 0.09 MPa and a rotation speed of 150 rpm for 40 minutes to prepare the dealcoholization condensation type silicone sealant.
[0028] Comparative Application Example 2 The dealcoholization condensation type silicone sealant comprises the following components in parts by weight: 100 parts of α, ω-dihydroxy polydimethylsiloxane, 15 parts of dimethyl silicone oil, 40 parts of modified spherical silica, 6 parts of fumed silica, 10 parts of a crosslinking agent, and 1 part of a catalyst; The viscosity of the α,ω-dihydroxy polydimethylsiloxane at 25° C. is 30000 mPa·s; The viscosity of the dimethyl silicone oil at 25° C. is 200 mPa·s; The modified spheroidal silica is the modified spheroidal silica obtained by the modified spheroidal silica preparation process of Comparative Example 1 of the present invention; The fumed silica is a hydrophobic fumed silica, and the specific surface area of the hydrophobic fumed silica is 200 m 2 / g; The cross-linking agent is methyltrimethoxysilane; The catalyst is isopropyl titanate; The preparation process of the dealcoholization condensation type silicone sealant is as follows: 100 parts of α, ω-dihydroxy polydimethylsiloxane, 15 parts of dimethyl silicone oil, 40 parts of modified spherical silica, and 6 parts of fumed silica are heated in a planetary mixer, and the mixture is mixed at a vacuum of 0.09 MPa and a rotation speed of 100 rpm for 30 minutes to obtain a mixture. Thereafter, 10 parts of a cross-linking agent and 1 part of a catalyst are added to the mixture, and the mixture is mixed at a vacuum of 0.09 MPa and a rotation speed of 150 rpm for 40 minutes to prepare the dealcoholization condensation type silicone sealant.
[0029] Comparative Application Example 3 The dealcoholization condensation type silicone sealant comprises the following components in parts by weight: 100 parts of α, ω-dihydroxy polydimethylsiloxane, 15 parts of dimethyl silicone oil, 40 parts of modified spherical silica, 6 parts of fumed silica, 10 parts of a crosslinking agent, and 1 part of a catalyst; The viscosity of the α,ω-dihydroxy polydimethylsiloxane at 25° C. is 30000 mPa·s; The viscosity of the dimethyl silicone oil at 25° C. is 200 mPa·s; The modified spheroidal silica is the modified spheroidal silica obtained by the modified spheroidal silica preparation process of Comparative Example 2 of the present invention; The fumed silica is a hydrophobic fumed silica, and the specific surface area of the hydrophobic fumed silica is 200 m 2 / g; The cross-linking agent is methyltrimethoxysilane; The catalyst is isopropyl titanate; The preparation process of the dealcoholization condensation type silicone sealant is as follows: 100 parts of α, ω-dihydroxy polydimethylsiloxane, 15 parts of dimethyl silicone oil, 40 parts of modified spherical silica, and 6 parts of fumed silica are heated in a planetary mixer, and the mixture is mixed at a vacuum of 0.09 MPa and a rotation speed of 100 rpm for 30 minutes to obtain a mixture. Thereafter, 10 parts of a cross-linking agent and 1 part of a catalyst are added to the mixture, and the mixture is mixed at a vacuum of 0.09 MPa and a rotation speed of 150 rpm for 40 minutes to prepare the dealcoholization condensation type silicone sealant.
[0030] Performance Testing (1) Surface drying time test: The surface drying time was determined with reference to GB / T 13477.5-2002 "Test methods for building sealing materials Part 5: Determination of surface drying time". The specific test method is: place a 30×100mm mold frame on a glass plate, fill the mold frame with sealant, and do not mix air. Scrape the sample with a scraper to make it uniform in thickness, then let it stand, and then gently touch the sample at three different locations on the test piece with the end of your finger, repeat the above operation until no sample adheres to your finger, and record the time.
[0031] (2) Tensile strength and elongation at break test Referring to GB / T 528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber", the specific test method is: prepare the sample into a dumbbell-shaped sample according to the provisions of GB / T2941, stretch it at a speed of 500mm / min, record the tensile stress and distance when the sample is stretched to fracture, and calculate the elongation at fracture.
[0032] (3) Waterproof performance test The glue was squeezed out from a paper mold with a diameter of 5 mm and a thickness of 3 mm, and then naturally cured at room temperature for 24 hours before use. Three parallel samples from each group were taken for room temperature immersion test in deionized water. The cured glue sample was dried at 105°C for 1 hour, and the dry weight M1 was measured. After soaking for 24 hours, it was wiped dry with a dry cloth and the wet weight M2 was measured. The water absorption rate was calculated according to the water absorption rate (‰): δ = (M2-M1) / M1×1000. The specific results are shown in Table 1.
[0033] Table 1 Performance test results of dealcoholization condensation type silicone sealant obtained in each application example and comparative application example
[0034] According to the experimental results in Table 1, the modified spherical silica prepared in Examples 1-3, when applied to dealcoholization condensation type silicone sealant, the obtained silicone sealant is superior to the spherical silica modified by ordinary silane coupling agent in terms of surface drying time, mechanical properties, water absorption and adhesion, and is even better than the unmodified spherical silica.
[0035] The modified spherical silica obtained by the modification process of the present invention is firstly surface treated with an aminosilane coupling agent, and then an epoxy-containing silane coupling agent is used to react with the amino groups on the surface of the amino-modified spherical silica, so that the alkoxy groups of the epoxysilane coupling agent are grafted onto the surface of the spherical silica, which not only organically modifies the surface of the spherical silica, but also retains the alkoxy groups that can react, thereby improving the mechanical properties of the dealcoholization condensation type silicone sealant and improving its water barrier properties.
[0036] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the defined scope, they should all fall within the protection scope of the present invention.
Claims
1. A method for preparing modified spherical silicon used in dealcoholization condensation type silicone sealant, characterized in that: The following steps are included: Step 1: Add 10-15 parts of spherical silica to 100-200 mL of a 10 wt% sodium hydroxide aqueous solution, stir in a water bath at 70-80° C. for 3-5 hours, cool to room temperature after the reaction, filter, wash with water, and dry at 60° C. for 10-12 hours to obtain surface hydroxylated spherical silica; Step 2: adding 1-3 parts of an amino-containing silane coupling agent to 50-100 mL of a 90 wt% ethanol aqueous solution for hydrolysis, and adjusting the pH value of the ethanol aqueous solution to 7.5-10 with a pH adjuster; Step 3: adding the surface hydroxylated spherical silica prepared in step 1 to the hydrolysis solution prepared in step 2; Reflux reaction for 2 to 3 hours under stirring conditions, filter, wash and dry to obtain spherical silica modified with an aminosilane coupling agent; Step 4: Add the aminosilane coupling agent-modified spherical silica prepared in step 3 to a container containing 100-200 mL of toluene, introduce nitrogen to replace the air, then add 3-5 parts of epoxy-containing silane coupling agent to the container, and react at 30-80°C for 1-2h, filter, wash and dry to obtain surface-modified spherical silica.
2. The method for preparing modified spherical silicon for use in dealcoholization condensation type silicone sealant according to claim 1, characterized in that: The median particle size D50 of the spherical silicon is 1-5 μm.
3. The method for preparing modified spherical silicon for use in dealcoholization condensation type silicone sealant according to claim 1, characterized in that: The amino-containing silane coupling agent in step 2 is selected from: one of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane or γ-aminopropylmethyldiethoxysilane; the pH adjuster in step 2 is selected from one of sodium hydroxide or potassium hydroxide.
4. The method for preparing modified spherical silicon for use in dealcoholization condensation type silicone sealant according to claim 1, characterized in that: The epoxy-containing silane coupling agent in step 4 is selected from: γ-glycidyloxypropyltrimethoxysilane or γ-glycidyloxypropyltriethoxysilane.
5. A modified spherical silicon used in dealcoholization condensation type silicone sealant, characterized in that: The modified spherical silica is obtained by any one of the preparation methods of claims 1-4.
6. Application of modified spherical silicon in dealcoholization condensation type silicone sealant, characterized in that: The modified spherical silica obtained by any one of the preparation methods of claims 1-4 is added to a dealcoholization condensation type silicone sealant and mixed; the formula of the dealcoholization condensation type silicone sealant is as follows: 100 parts of α, ω-dihydroxypolydimethylsiloxane, 10-30 parts of dimethyl silicone oil, 30-100 parts of modified spherical silica, 5-10 parts of fumed silica, 8-15 parts of a cross-linking agent, and 0.5-3 parts of a catalyst; the modified spherical silica is obtained by the preparation process of the modified spherical silica according to any one of claims 1-4.
7. The use of modified spherical silica in dealcoholization condensation type silicone sealant according to claim 6, characterized in that: The viscosity of the α,ω-dihydroxy polydimethylsiloxane at 25° C. is 20000-100000 mPa·s.
8. The use of modified spherical silica in dealcoholization condensation type silicone sealant according to claim 6, characterized in that: The fumed silica is a hydrophobic fumed silica, and the specific surface area of the hydrophobic fumed silica is 100-300 m 2 / g.
9. The use of modified spherical silica in dealcoholization condensation type silicone sealant according to claim 6, characterized in that: The crosslinking agent is selected from: methyltrimethoxysilane, vinyltrimethoxysilane, methyltriethoxysilane, vinyltriethoxysilane, tetramethoxysilane, tetraethoxysilane or a combination thereof.
10. The use of modified spherical silica in dealcoholization condensation type silicone sealant according to claim 6, characterized in that: The catalyst is selected from the group consisting of one or more of isopropyl titanate, butyl titanate, dibutyltin dilaurate, and stannous octoate.