High-performance OLED OCA optical adhesive and preparation method thereof
By introducing isosorbide acrylate and other monomers to thermally polymerize OCA optical adhesive, the bonding and adhesion problems of curved screens were solved, and a high-performance OCA optical adhesive was achieved. It has excellent filling properties, adhesion and yellowing resistance, ensuring the reliability of the product in different environments.
Patent Information
- Application Number
- CN202411077403.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-08
AI Technical Summary
Existing OCA optical adhesives cannot meet the high bonding and filling performance, adhesion and mechanical tensile properties required for curved screens, and also suffer from yellowing and bubble rebound problems.
Isosorbide acrylate is used as a hard monomer and is thermally polymerized with (meth)acrylate, hydroxyl-containing (meth)acrylate and nitrogen-containing functional (meth)acrylate to prepare acrylic resin. Combined with crosslinking agent, photoinitiator, silane coupling agent and antioxidant, a high-performance OCA optical adhesive is formed.
It achieves excellent bonding and filling performance, adhesion and mechanical tensile properties, avoids bubble rebound, has yellowing resistance, and ensures the reliability and stability of the product in different environments.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of optical adhesives, and in particular relates to a high-performance OLED OCA optical adhesive and a preparation method thereof. Background Art
[0002] OCA optical adhesive is a double-sided pressure-sensitive adhesive without a substrate. It has the advantages of being colorless and transparent, with a transmittance of more than 90%, high adhesion and small shrinkage after curing. It is used to fill the gap between the touch layer and the screen, and mainly plays the role of bonding, light transmission, display enhancement and buffering.
[0003] It is understood that curved screen is a popular screen design style for future smartphones. Its curved design extends people's vision beyond the screen, freeing the field of vision from the constraints of the border, greatly improving our visual experience.
[0004] However, OLED curved screens also place higher demands on the performance of OCA optical adhesives. Unlike ordinary flat screens, in order to effectively fill the curved part of the screen and fill the ink step difference, OCA optical adhesives not only need excellent fitting and filling performance, adhesion and mechanical tensile properties, but also do not have undesirable phenomena such as static bubble rebound and reliability test bubble rebound. Conventional OCA optical adhesive products on the market cannot meet these requirements.
[0005] In consideration of domestic substitution of advanced functional materials, the development of OLED OCA optical adhesive suitable for bonding curved screens has attracted more and more attention. However, the OCA optical adhesive disclosed in CN115124928A and CN116694270A uses hexafluoroantimonate, which may cause yellowing during use.
[0006] The OCA optical adhesive disclosed in CN115678440A uses thermal cross-linking curing in the later stage of curing, which will affect the efficiency and yield rate in actual production. Summary of the invention
[0007] The purpose of the present invention is to provide a high-performance OLED OCA optical adhesive and a preparation method thereof. The 3D curved screen has a certain curvature, resulting in a high step difference, and the OCA optical adhesive is required to have an excellent fitting and filling effect. Also because of the curvature of the curved screen, the OCA optical adhesive will be continuously subjected to the effect of internal stress, so the OCA optical adhesive is required to have excellent adhesion and mechanical tensile properties to avoid the risk of degumming. The present invention introduces isosorbide acrylate as a hard monomer, and prepares an acrylic resin through thermal polymerization with (meth) alkyl acrylate, hydroxyl-containing (meth) acrylate and nitrogen-containing functional (meth) acrylate, and further formulates it into an OCA optical adhesive. The introduction of bio-based isosorbide groups, coupled with the ingenious design of the composition formula, can comprehensively improve the comprehensive performance of OCA optical adhesive, giving it outstanding high adhesion, light transmittance and yellowing resistance, meeting the requirements of reliability testing, and ensuring the reliability of the product in different environments.
[0008] In the first aspect, the present invention provides a high-performance OLED OCA optical adhesive, characterized in that it includes the following raw materials: acrylic resin, cross-linking agent, photoinitiator, silane coupling agent, antioxidant; wherein
[0009] The raw materials for preparing the acrylic resin include, by weight: 45-65 parts of alkyl (meth)acrylate, 5-20 parts of hydroxyl (meth)acrylate, 5-25 parts of isosorbide (meth)acrylate, 1-5 parts of nitrogen-containing functional (meth)acrylate, 0.05-1 parts of chain transfer agent, 0.05-1 parts of grafting monomer, and 0.4-0.8 parts of initiator.
[0010] In one embodiment of the present application, the initiator is one or more of azobisisobutyronitrile, azobisisoheptanenitrile, and dibenzoyl peroxide.
[0011] In one embodiment of the present application, the raw materials of the high-performance OLED OCA optical adhesive and the preparation method thereof include, by weight: 100 parts of acrylic resin, 0.01-2 parts of cross-linking agent, 0.01-1.5 parts of photoinitiator, 0.01-2 parts of silane coupling agent, and 0.01-2 parts of antioxidant.
[0012] In one embodiment of the present application, the cross-linking agent is one or more of the isocyanate curing agents L75, N75, and N3390.
[0013] In one embodiment of the present application, the photoinitiator is one or more of 1-hydroxycyclohexyl phenyl ketone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, 4-acryloylhydroxybenzoic acid benzophenone, and benzophenone.
[0014] In one embodiment of the present application, the silane coupling agent is one or more of KH550, KH560, and KH570.
[0015] In one embodiment of the present application, the antioxidant is one or more of IRGANOX 1726, IRGANOX 1010, and IRGANOX 1076 produced by BASF of Germany.
[0016] In one embodiment of the present application, the (meth)acrylic acid alkyl ester is one or more of n-butyl acrylate, n-butyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, n-octyl acrylate, n-octyl methacrylate, dodecyl acrylate, dodecyl methacrylate, isononyl acrylate, and isodecyl acrylate.
[0017] In one embodiment of the present application, the hydroxyl-containing (meth)acrylate is one or more of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, and hydroxybutyl methacrylate.
[0018] In one embodiment of the present application, the isosorbide (meth)acrylate is one or more of isosorbide acrylate and isosorbide methacrylate.
[0019] In one embodiment of the present application, the nitrogen-containing functional (meth)acrylate is one or more of acrylamide, methacrylamide, N-hydroxyethyl acrylamide, N-vinyl pyrrolidone, 4-acryloylmorpholine, dimethylaminoethyl acrylate, dimethylaminoethyl methacrylate, and N,N-dimethylacrylamide.
[0020] In one embodiment of the present application, the chain transfer agent is one or more of dodecyl mercaptan, isooctyl thioglycolate, 2-mercaptoethanol, isooctyl 3-mercaptopropionate, and pentaerythritol tetrakis (3-mercaptobutyrate).
[0021] In one embodiment of the present application, the grafting monomer is one or more of 2-isocyanatoethyl acrylate and 2-isocyanatoethyl methacrylate.
[0022] In one embodiment of the present application, the thickness of the OCA optical adhesive is 100-150 μm.
[0023] In a second aspect, the present invention provides a method for preparing the high-performance OLED OCA optical adhesive as described above, comprising the following steps:
[0024] (1) adding alkyl (meth)acrylate, hydroxyl (meth)acrylate, isosorbide (meth)acrylate, nitrogen-containing functional (meth)acrylate, chain transfer agent and organic solvent into a reaction kettle, stirring and introducing nitrogen, heating to 65° C. and keeping the temperature for 40 min, adding the first batch of initiator, and reacting for 2 h;
[0025] (2) Raise the temperature to 70°C, add the second batch of initiator, and react for 2 hours;
[0026] (3) Raise the temperature to 78°C, add the third batch of initiator, and reflux for 3 hours;
[0027] (4) After reaching the end point of the reaction, oxygen was introduced to cool the temperature to 50°C, a grafting monomer was added, the reaction was continued for 5 hours, and the temperature was lowered and the material was discharged to obtain an acrylic resin;
[0028] (5) mixing and stirring the acrylic resin, crosslinking agent, photoinitiator, silane coupling agent, and antioxidant, and filtering the mixture through a 200-500 mesh filter bag to obtain an OLED OCA optical adhesive;
[0029] (6) The optical adhesive is uniformly coated on the heavy release film, the solvent is dried, the light release film is compounded, and the mixture is aged at 40° C. for 3 days to finally obtain the OCA optical adhesive.
[0030] In one embodiment of the present application, the organic solvent is one or more of ethyl acetate, butyl acetate, butanone, and cyclohexanone; the weight proportion of the organic solvent may be 122-185 parts.
[0031] In one embodiment of the present application, the weight portion of the first batch of initiators is 0.1-0.3 parts; the weight portion of the second batch of initiators is 0.1-0.3 parts, and the weight portion of the third batch of initiators is 0.1-0.4 parts.
[0032] In one embodiment of the present application, the solid content of the acrylic resin is 35-45%.
[0033] In one embodiment of the present application, the weight average molecular weight of the acrylic resin is 400,000-600,000 g / mol.
[0034] The beneficial effects of the present invention are:
[0035] (1) The high-performance OLED OCA optical adhesive of the present invention has excellent bonding and filling performance, good fluidity under high temperature and high pressure, and can effectively wet and fill different ink step differences, fully ensuring the bonding yield;
[0036] (2) The high-performance OLED OCA optical adhesive of the present invention has excellent room temperature and high temperature bonding properties and mechanical tensile properties, has sufficient strength to support the curved surface, and does not have undesirable phenomena such as static bubble rebound and reliability test bubble rebound, thereby ensuring the reliability of the product in different environments;
[0037] (3) The high-performance OLED OCA optical adhesive of the present invention has excellent optical properties and yellowing resistance;
[0038] (4) The OCA optical adhesive of the present invention is obtained by solution thermal polymerization, and the synthesis process is simple and stable. Compared with UV-type OCA, it has low requirements on coating equipment and the process is more stable and reliable.
[0039] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention are realized and obtained by the structures particularly pointed out in the description. DETAILED DESCRIPTION
[0040] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] In the following examples, all the raw materials and reagents used are commercially available.
[0042] Example 1
[0043] The composition of the OLED OCA optical adhesive of this embodiment is shown in the following table:
[0044]
[0045]
[0046] (1) Add the above-mentioned 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, hydroxyethyl acrylate, isosorbide acrylate, acrylamide, dodecyl mercaptan, and ethyl acetate into a reaction kettle equipped with a thermometer and a stirring device, stir and mix evenly, and introduce nitrogen. Heat to 65°C and keep warm for 40 minutes, add 0.15g of azobisisobutyronitrile, and react for 2 hours. Then heat to 70°C, add 0.15g of azobisisobutyronitrile, and react for 2 hours. Finally, heat to 78°C, add 0.2g of azobisisobutyronitrile, and reflux for 3 hours. After reaching the end point of the reaction, introduce oxygen and cool to 50°C, add the grafting monomer 2-isocyanoethyl methacrylate, react for 5 hours, cool and discharge to obtain acrylic resin.
[0047] (2) The acrylic resin, N3390, 1-hydroxycyclohexyl phenyl ketone, KH560, and IRGANOX 1010 are mixed and stirred evenly, and filtered through a 200-500 mesh filter bag to obtain an OLED OCA optical adhesive.
[0048] (3) The above-mentioned OLED OCA optical adhesive is evenly coated on the heavy release film, the solvent is dried at medium to high temperature, the light release film is attached, and it is aged at 40° C. for 3 days to finally obtain the OCA optical adhesive.
[0049] Example 2
[0050] The composition of the OLED OCA optical adhesive of this embodiment is shown in the following table:
[0051] Specific components Weight / g 2-Ethylhexyl acrylate 60 Hydroxyethyl acrylate 18 Isosorbide acrylate 19 Acrylamide 3 Dodecyl mercaptan 0.2 2-Isocyanoethyl Methacrylate 0.5 Azobisisobutyronitrile 0.45 Ethyl acetate 130 L75 0.14 1-Hydroxycyclohexylphenyl ketone 0.15 KH560 0.2 IRGANOX1010 0.2
[0052] (1) Add the above-mentioned 2-ethylhexyl acrylate, hydroxyethyl acrylate, isosorbide acrylate, acrylamide, dodecyl mercaptan, and ethyl acetate to a reactor equipped with a thermometer and a stirring device, stir and mix evenly, and introduce nitrogen. Heat to 65°C and keep warm for 40 minutes, add 0.1g of azobisisobutyronitrile, and react for 2 hours. Then heat to 70°C, add 0.15g of azobisisobutyronitrile, and react for 2 hours. Finally, heat to 78°C, add 0.2g of azobisisobutyronitrile, and reflux for 3 hours. After reaching the end point of the reaction, introduce oxygen and cool to 50°C, add the grafting monomer 2-isocyanoethyl methacrylate, react for 5 hours, cool and discharge to obtain acrylic resin.
[0053] (2) The acrylic resin, L75, 1-hydroxycyclohexyl phenyl ketone, KH560, and IRGANOX 1010 are mixed and stirred evenly, and filtered through a 200-500 mesh filter bag to obtain an OLED OCA optical adhesive.
[0054] (3) The above-mentioned OLED OCA optical adhesive is evenly coated on the heavy release film, the solvent is dried at medium to high temperature, the light release film is attached, and it is aged at 40° C. for 3 days to finally obtain the OCA optical adhesive.
[0055] Example 3
[0056] The composition of the OLED OCA optical adhesive of this embodiment is shown in the following table:
[0057] Specific components Weight / g 2-Ethylhexyl acrylate 55 2-Ethylhexyl Methacrylate 10 Hydroxyethyl acrylate 16 Isosorbide Methacrylate 17 N,N-Dimethylacrylamide 2 Pentaerythritol tetrakis(3-mercaptobutyrate) 0.2 2-Isocyanoethyl acrylate 0.5 Azobisisobutyronitrile 0.3 Azobis(2-isoheptanonitrile) 0.3 Ethyl acetate 100 Butanone 30 L75 0.14 2,4,6-Trimethylbenzoyl-diphenylphosphine oxide 0.2 KH570 0.3 IRGANOX1726 0.18
[0058] (1) Add the above-mentioned 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, hydroxyethyl acrylate, isosorbide methacrylate, N,N-dimethylacrylamide, pentaerythritol tetrakis (3-mercaptobutyrate), ethyl acetate, and butanone into a reaction kettle equipped with a thermometer and a stirring device, stir and mix evenly, and introduce nitrogen. Heat to 65°C and keep warm for 40 minutes, add 0.15g of azobisisobutyronitrile, and react for 2 hours. Then heat to 70°C, add 0.15g of initiator azobisisobutyronitrile, and react for 2 hours. Finally, heat to 78°C, add 0.3g of initiator azobisisoheptanenitrile, and reflux for 3 hours. After reaching the end point of the reaction, introduce oxygen and cool to 50°C, add grafted monomer 2-isocyanoethyl methacrylate, react for 5 hours, cool and discharge to obtain acrylic resin.
[0059] (2) The acrylic resin, L75, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, KH570, and IRGANOX 1726 are mixed and stirred uniformly, and filtered through a 200-500 mesh filter bag to obtain an OLED OCA optical adhesive.
[0060] (3) The above-mentioned OLED OCA optical adhesive is evenly coated on the heavy release film, the solvent is dried at medium to high temperature, the light release film is attached, and it is aged at 40° C. for 3 days to finally obtain the OCA optical adhesive.
[0061] Example 4
[0062] The composition of the OLED OCA optical adhesive of this embodiment is shown in the following table:
[0063] Specific components Weight / g n-Octyl acrylate 58 2-Ethylhexyl Methacrylate 6 Hydroxybutyl acrylate 11.5 Isosorbide acrylate 20 N-vinyl pyrrolidone 4.5 Pentaerythritol tetrakis(3-mercaptobutyrate) 0.4 2-Isocyanoethyl Methacrylate 0.4 Azobisisobutyronitrile 0.45 Ethyl acetate 150 N3390 0.2 1-Hydroxycyclohexylphenyl ketone 0.18 KH550 0.5 IRGANOX1010 0.4
[0064] (1) Add the above-mentioned n-octyl acrylate, 2-ethylhexyl methacrylate, hydroxybutyl acrylate, isosorbide acrylate, N-vinyl pyrrolidone, pentaerythritol tetra(3-mercaptobutyrate), and ethyl acetate into a reaction kettle equipped with a thermometer and a stirring device, stir and mix evenly, and introduce nitrogen. Heat to 65°C and keep warm for 40 minutes, add 0.15g of azobisisobutyronitrile, and react for 2 hours. Then heat to 70°C, add 0.15g of azobisisobutyronitrile, and react for 2 hours. Finally, heat to 78°C, add 0.15g of azobisisobutyronitrile, and reflux for 3 hours. After reaching the end point of the reaction, introduce oxygen and cool to 50°C, add the grafting monomer 2-isocyanoethyl methacrylate, react for 5 hours, cool and discharge to obtain acrylic resin.
[0065] (2) The acrylic resin, N3390, 1-hydroxycyclohexyl phenyl ketone, KH550 and IRGANOX1010 are mixed and stirred evenly, and filtered through a 200-500 mesh filter bag to obtain an OLED OCA optical adhesive.
[0066] (3) The OLED OCA optical adhesive is evenly coated on the heavy release film, the solvent is dried at medium to high temperature, the light release film is attached, and the film is aged at 40° C. for 3 days to finally obtain the OCA optical adhesive.
[0067] Example 5
[0068] The composition of the OLED OCA optical adhesive of this embodiment is shown in the following table:
[0069] Specific components Weight / g Isononyl acrylate 55 2-Ethylhexyl Methacrylate 8.5 Hydroxypropyl acrylate 12 Isosorbide Methacrylate 15 Isosorbide acrylate 5 Acrylamide 4.5 Pentaerythritol tetrakis(3-mercaptobutyrate) 0.4 2-Isocyanoethyl acrylate 0.4 Azobisisobutyronitrile 0.6 Ethyl acetate 100 Cyclohexanone 70 N3390 0.3 1-Hydroxycyclohexylphenylketone 0.2 KH560 0.6 IRGANOX1076 0.4
[0070] (1) Add the above-mentioned isononyl acrylate, 2-ethylhexyl methacrylate, hydroxypropyl acrylate, isosorbide methacrylate, isosorbide acrylate, acrylamide, pentaerythritol tetra(3-mercaptobutyrate), ethyl acetate and cyclohexanone into a reaction kettle equipped with a thermometer and a stirring device, stir and mix evenly, and introduce nitrogen. Heat to 65°C and keep warm for 40 minutes, add 0.2g of azobisisobutyronitrile, and react for 2 hours. Then heat to 70°C, add 0.2g of azobisisobutyronitrile, and react for 2 hours. Finally, heat to 78°C, add 0.2g of azobisisobutyronitrile, and reflux for 3 hours. After reaching the end point of the reaction, introduce oxygen and cool to 50°C, add grafting monomer 2-isocyanoethyl acrylate, react for 5 hours, cool and discharge to obtain acrylic resin.
[0071] (2) The acrylic resin, N3390, 1-hydroxycyclohexyl phenyl ketone, KH560, and IRGANOX 1076 are mixed and stirred uniformly, and filtered through a 200-500 mesh filter bag to obtain an OLED OCA optical adhesive.
[0072] (3) The OLED OCA optical adhesive is evenly coated on the heavy release film, the solvent is dried at medium to high temperature, the light release film is attached, and the film is aged at 40° C. for 3 days to finally obtain the OCA optical adhesive.
[0073] Comparative Example 1
[0074] The composition of the OCA optical adhesive of this comparative example is shown in the following table
[0075] Specific components Weight / g 2-Ethylhexyl acrylate 55 2-Ethylhexyl Methacrylate 10 Hydroxyethyl acrylate 17 Isobornyl acrylate 15 Acrylamide 3 Dodecyl mercaptan 0.2 2-Isocyanoethyl Methacrylate 0.5 Azobisisobutyronitrile 0.5 Ethyl acetate 123 N3390 0.14 1-Hydroxycyclohexylphenylketone 0.15 KH560 0.2 IRGANOX1010 0.2
[0076] (1) Add the above-mentioned 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, hydroxyethyl acrylate, isobornyl acrylate, acrylamide, dodecyl mercaptan, and ethyl acetate into a reaction kettle equipped with a thermometer and a stirring device, stir and mix evenly, and introduce nitrogen. Heat to 65°C and keep warm for 40 minutes, add 0.15g of azobisisobutyronitrile, and react for 2 hours. Then heat to 70°C, add 0.15g of azobisisobutyronitrile, and react for 2 hours. Finally, heat to 78°C, add 0.2g of azobisisobutyronitrile, and reflux for 3 hours. After reaching the end point of the reaction, introduce oxygen and cool to 50°C, add the grafting monomer 2-isocyanoethyl methacrylate, react for 5 hours, cool and discharge to obtain acrylic resin.
[0077] (2) The acrylic resin, N3390, 1-hydroxycyclohexyl phenyl ketone, KH560, and IRGANOX 1010 are mixed and stirred evenly, and filtered through a 200-500 mesh filter bag to obtain an OLED OCA optical adhesive.
[0078] (3) The OLED OCA optical adhesive is evenly coated on the heavy release film, the solvent is dried at medium to high temperature, the light release film is attached, and the film is aged at 40° C. for 3 days to finally obtain the OCA optical adhesive.
[0079] Performance Testing
[0080] The physical properties of the OCA optical adhesives prepared in Examples 1-5 of the present invention and Comparative Example 1 were tested, and the test methods are listed as follows:
[0081] Optical properties: Cut OCA into 50mm*50mm strips, remove the light release film, attach it to optical quartz glass, remove the heavy release film, and test the optical properties of the series using a spectrophotometer in a constant temperature and humidity room.
[0082] Adhesion: Cut OCA into 25mm*15cm strips, tear off the light release film, apply 50μm PET, then tear off the heavy film, stick it to a transparent glass plate, roll it back and forth three times with a 2Kg roller, let it stand in a constant temperature and humidity room for 20 minutes, and then use a tensile testing machine to peel off the test sample in a 180° direction at a speed of 300mm / min.
[0083] Dielectric constant: stack the OCA onto a sample with a thickness of more than 500μm (actual thickness T), then remove the light release film, laminate it onto a metal electrode (area S), and attach another metal electrode to it. Clamp the two metal electrodes with a clip, adjust the test frequency, record the inherent capacitance (Cp) value, and calculate the dielectric constant = Cp×T / (8.854×S), where 8.854 is a constant.
[0084] Stretching: Cut the OCA optical adhesive into a width of 6.5cm, remove the release film and stack it into samples with a thickness of 0.7mm, then cut it into 25mm width, tear off the release film on one end of the sample and use invisible tape to cut an effective length of 25mm, tear off the release film on the other side, stick the invisible tape into a handle, fix it on the fixture and use a tensile machine for testing.
[0085] Storage modulus and loss factor tanδ were measured using TA hybrid rheometer DHR-2. OCA optical adhesive was laminated and stacked to a sample with a thickness of 1mm±0.05mm, without wrinkles or bubbles, and a circular sample with a diameter of 0.8mm was made using a tool and tested according to the operating procedures. Test conditions: 1Hz, 0.1% strain. Creep recovery test conditions: 40kPa, 25℃, creep 600s, recovery 600s.
[0086] The physical properties of OLED OCA optical glue are shown in the following table:
[0087]
[0088] It can be seen from the data in the above table that the OCA optical adhesive prepared by the present invention has excellent adhesion and mechanical tensile properties.
[0089] In addition, tanδ(50℃) and tanδ(100℃) are between 0.6-0.8, which can ensure that OCA has good fluidity under high temperature and high pressure, effectively wet and fill the screen and ink step difference, and fully ensure the bonding yield.
[0090] In addition, the storage modulus at room temperature is greater than 160,000Pa, which can effectively ensure that there is sufficient strength to support the curved surface during the bonding production process to avoid bubble rebound.
[0091] The physical properties of OLED OCA optical adhesive after UV curing are shown in the following table;
[0092] UV curing conditions: high pressure mercury lamp, energy > 3000mj / cm 2 ; LED light (365nm), energy>4000mj / cm 2 Here, UV curing is adopted under high pressure mercury lamp, with energy of 3500mj / cm 2.
[0093]
[0094]
[0095] From the data in the above table, it can be seen that the OCA optical adhesive prepared by the present invention exhibits outstanding bonding performance, mechanical tensile performance and optical performance after UV curing. The storage modulus after UV is greater than 200000Pa, and the colloid can effectively prevent bubble rebound.
[0096] Surface bonding and reliability testing
[0097] Tear off the light OCA optical adhesive film and attach it to the upper polarized light of the OLED module, tear off the heavy film on the other side, and bond it to the curved cover with a 30μm ink step difference on all sides. The bonding pressure is 0.35MPa, and then degassing and bonding are carried out at 50℃ / 0.5MPa / 25min. Observe the bubbles on the edge of the ink. Finally, UV curing is carried out under a high-pressure mercury lamp with an energy of 3500mj / cm 2 . Observe again to see if there are any bubbles bouncing back.
[0098] The samples after simulated bonding were placed in cold and hot shock (-40℃*30min / 85℃*30min, 200 cycles), high temperature and high humidity (85℃*85%RH, 500h), high temperature (85℃, 500h), low temperature (-40℃, 500h), QUV (0.63W / m 2 ,340nm,500h) test box, put 20 pieces for each condition, take them out for observation after the test, if there is no bubble rebound, no whitening, no yellowing, no warping or debonding, it is OK; if any piece has the above defects, it is NG.
[0099] project Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 Hot and cold shock OK OK OK OK OK OK High temperature and humidity OK OK OK OK OK NG high temperature OK OK OK OK OK OK Low temperature OK OK OK OK OK OK QUV OK OK OK OK OK OK
[0100] It can be seen from the above test results that the OLED OCA optical adhesive prepared by the present invention exhibits excellent aging performance, with no bubble rebound, no whitening, no yellowing, and no warping and debonding. The reliability of the product in different environments is guaranteed, and the stability and service life of the terminal product are comprehensively improved. However, one piece of the comparative example had bubble reappearance under high temperature and high humidity aging conditions.
[0101] The difference between Comparative Example 1 and Example 1 is that isosorbide acrylate is not used in the raw materials. Therefore, isosorbide acrylate is introduced as a hard monomer, and the composition composed of the isosorbide structure and other components synergistically improves the comprehensive performance of the OCA optical adhesive, giving it outstanding high adhesion, light transmittance and yellowing resistance, meeting the requirements of the reliability test, and ensuring the reliability of the product in different environments.
[0102] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A high-performance OLED OCA optical adhesive, characterized in that: Including the following ingredients: Acrylic resin, crosslinking agent, photoinitiator, silane coupling agent, antioxidant; in The raw materials for preparing the acrylic resin include, by weight: 45-65 parts of alkyl (meth)acrylate, 5-20 parts of hydroxyl (meth)acrylate, 5-25 parts of isosorbide (meth)acrylate, 1-5 parts of nitrogen-containing functional (meth)acrylate, 0.05-1 parts of chain transfer agent, 0.05-1 parts of grafting monomer, and 0.4-0.8 parts of initiator.
2. The high-performance OLED OCA optical adhesive according to claim 1, characterized in that: The raw materials of the high-performance OLED OCA optical adhesive and the preparation method thereof include, by weight: 100 parts of acrylic resin, 0.01-2 parts of cross-linking agent, 0.01-1.5 parts of photoinitiator, 0.01-2 parts of silane coupling agent, and 0.01-2 parts of antioxidant.
3. The high-performance OLED OCA optical adhesive and preparation method thereof according to claim 1, characterized in that: The cross-linking agent is one or more of isocyanate curing agents L75, N75, and N3390.
4. The high performance OLED OCA optical adhesive according to claim 1, characterized in that: The (meth)acrylic acid alkyl ester is one or more of n-butyl acrylate, n-butyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, n-octyl acrylate, n-octyl methacrylate, dodecyl acrylate, dodecyl methacrylate, isononyl acrylate, and isodecyl acrylate; The hydroxyl-containing (meth)acrylate is one or more of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, and hydroxybutyl methacrylate.
5. The high performance OLED OCA optical adhesive according to claim 1, characterized in that: The isosorbide (meth)acrylate is one or more of isosorbide acrylate and isosorbide methacrylate.
6. The high performance OLED OCA optical adhesive according to claim 1, characterized in that: The nitrogen-containing functional (meth)acrylate is one or more of acrylamide, methacrylamide, N-hydroxyethyl acrylamide, N-vinyl pyrrolidone, 4-acryloylmorpholine, dimethylaminoethyl acrylate, dimethylaminoethyl methacrylate, and N,N-dimethylacrylamide.
7. The high performance OLED OCA optical adhesive according to claim 1, characterized in that: The chain transfer agent is one or more of dodecyl mercaptan, isooctyl thioglycolate, 2-mercaptoethanol, isooctyl 3-mercaptopropionate, and pentaerythritol tetrakis (3-mercaptobutyrate).
8. The high performance OLED OCA optical adhesive according to claim 1, characterized in that: The grafting monomer is one or more of 2-isocyanatoethyl acrylate and 2-isocyanatoethyl methacrylate.
9. The high performance OLED OCA optical adhesive according to claim 1, characterized in that: The thickness of the OCA optical adhesive is 100-150 μm.
10. A method for preparing a high-performance OLED OCA optical adhesive according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) adding alkyl (meth)acrylate, hydroxyl (meth)acrylate, isosorbide (meth)acrylate, nitrogen-containing functional (meth)acrylate, chain transfer agent and organic solvent into a reaction kettle, stirring and introducing nitrogen, heating to 65° C. and keeping the temperature for 40 min, adding the first batch of initiator, and reacting for 2 h; (2) Raise the temperature to 70°C, add the second batch of initiator, and react for 2 hours; (3) Raise the temperature to 78°C, add the third batch of initiator, and reflux for 3 hours; (4) After reaching the end point of the reaction, oxygen was introduced to cool the temperature to 50°C, a grafting monomer was added, the reaction was continued for 5 hours, and the temperature was lowered and the material was discharged to obtain an acrylic resin; (5) mixing and stirring the acrylic resin, crosslinking agent, photoinitiator, silane coupling agent, and antioxidant, and filtering the mixture through a 200-500 mesh filter bag to obtain an OLED OCA optical adhesive; (6) The optical adhesive is uniformly coated on the heavy release film, the solvent is dried, the light release film is compounded, and the mixture is aged at 40° C. for 3 days to finally obtain the OCA optical adhesive.
Citation Information
Cited By
Adhesive for flexible OLED (Organic Light Emitting Diode) display panel, adhesive layer, support film and preparation method of support film
CN119931556A