Wide-emission zinc telluride selenide quantum dot as well as preparation method and application thereof
By covering long-chain organic ligands and zinc halide modifications on ZnSeTe quantum dots, its emission spectrum band is broadened, solving the problem of narrow spectrum and high preparation cost in the prior art, and achieving high efficiency and low cost Wide spectrum emission, suitable for white light illumination.
Patent Information
- Application Number
- CN202410980893.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
AI Technical Summary
The emission spectrum of existing ZnSeTe quantum dots is concentrated in the blue light wavelength range, with a narrow spectral coverage range, high cost, poor repeatability, and low quantum yield, which cannot meet the needs of white light-emitting diodes in a wide spectrum range.
Inject the tellurium precursor solution and the nucleation selenium precursor solution into the zinc acetate reaction solution under an inert atmosphere to carry out the nucleation reaction to form the zinc-modified quantum dot core, and then add zinc halide to form the inner shell layer, then form the intermediate shell layer and the outer shell layer. , the quantum dot surface is coated with long-chain organic ligands such as oleamine and oleic acid, and the defective emission is introduced by modification of zinc halide, and the emission spectrum band is widened.
It realizes a wide-emitted zinc selenide quantum dot with low preparation cost and simple and efficient process, with high quantum yield and emission spectrum covering the band from green to red, and is suitable for the field of white light illumination.
Smart Images

Figure CN118909617A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of luminescent materials, and in particular to a broad-emission zinc telluride selenide quantum dot and a preparation method and application thereof. Background Art
[0002] White light emitting diodes (WLED) are gradually replacing traditional solid-state lighting sources due to their advantages of high efficiency, energy saving, environmental protection, and long life. Their application areas are also gradually expanding with the advancement of light emitting diode (LED) technology. In pursuit of physical and mental health, users have also put forward higher requirements for the quality and comfort of light. While paying attention to the objective visual effects of light (such as quantum efficiency, brightness, etc.), they also need to consider the non-visual biological effects of light and light radiation to achieve the purpose of healthy lighting. In addition to indicators such as color rendering index, brightness, and flicker, the overlap between the spectrum of WLED and the solar spectrum is an extremely important criterion for judging whether a lamp is a healthy lighting product. Therefore, full-spectrum LED has become a research hotspot of LED technology in recent years. Unlike traditional WLED devices that use blue light chips to excite multi-color phosphors, full-spectrum LEDs put forward new requirements for the selection of luminescent materials, that is, they have a wider coverage band in the visible light range and are closer to the real solar spectrum.
[0003] Quantum dots have shown broad application prospects in the fields of bioimaging, optoelectronic devices, solar cells, etc. due to their unique optical and electrical properties. Zinc telluride selenide (ZnSeTe) quantum dots, as an important II-VI semiconductor material, have a relatively wide optical band gap and tunable spectral emission characteristics. Therefore, the design of efficient and environmentally friendly ZnSeTe quantum dots with wide emission and highly tunable wavelength is gradually becoming a research hotspot in the field of white light illumination.
[0004] However, the emission spectrum of existing ZnSeTe quantum dots is concentrated in the blue light wavelength range, and generally has the defects of narrow spectral coverage and the need for multiple materials. At the same time, the existing preparation methods also have problems such as high cost, poor repeatability, and low quantum yield, which limit their wide application.
[0005] For example, the Chinese invention patent with publication number CN111218284A discloses a core-shell quantum dot and its preparation method and electronic device, wherein the core-shell quantum dot includes a ZnTeSe core, a ZnSeS shell coated outside the ZnTeSe core, and a ZnS shell coated outside the ZnSeS shell. The core-shell quantum dot ZnTeSe / ZnSeS / ZnS of the invention introduces a certain amount of tellurium into the ZnSe core to form a uniform ZnTeSe alloy quantum dot, narrows the bandgap width of the core, and red-shifts the emission wavelength, thereby generating 460-480 nm blue light emission. However, the blue light emission in this range is narrow, and it is impossible to construct a white light-emitting diode covering a wide spectral range.
[0006] For another example, the Chinese invention patent CN117821068A provides a blue light ZnSeTe core-shell quantum dot and a preparation method and a display device thereof, wherein the preparation method comprises the following steps: S1, preparing a core body: adding an activity enhancer, a selenium precursor, a tellurium precursor and a zinc precursor at 220-260°C for mixed reaction to form a blue light ZnSeTe core body; S2, preparing a transition layer: adding an etchant to S1 to etch the blue light ZnSeTe core body; after heating, adding a zinc precursor and a selenium precursor, wherein the selenium precursor is added dropwise at a rate of 4-6 mL / h to form a ZnSe transition layer covering the blue light ZnSeTe core body; S3, preparing an outer shell layer: after cooling, adding a zinc precursor and a sulfur precursor to S2, wherein the zinc precursor is an amine-containing zinc precursor, to form a ZnS outer shell layer covering the transition layer. The preparation of the blue light ZnSeTe core-shell quantum dots is rather complicated, and its photoinduced maximum emission peak wavelength is 450±5 nm. The emission line width is still relatively narrow, and it also cannot meet the requirements of white light-emitting diodes covering a wide spectral range.
[0007] In summary, the use of appropriate synthesis routes and post-processing processes to efficiently and low-cost prepare ZnSeTe quantum dots with wide-spectrum emission characteristics is of great significance for expanding their application in the field of white light lighting. Summary of the invention
[0008] In view of the above-mentioned defects of the prior art, in a first aspect of the present invention, a method for preparing broad-emission zinc telluride selenide quantum dots with low preparation cost, simple process and high efficiency is provided, comprising the following steps: (1) In an inert atmosphere, a tellurium precursor solution and a nucleation selenium precursor solution are injected into a zinc acetate reaction solution to carry out a nucleation reaction; after the nucleation reaction is completed, zinc halide is added and reacted to obtain a reaction solution containing zinc-modified quantum dot cores (ZnSeTe); The zinc acetate reaction solution is prepared by dissolving zinc acetate in a high boiling point solvent and adding oleylamine and oleic acid; the tellurium precursor solution and the nucleation selenium precursor solution are prepared by dissolving tellurium and selenium in a ligand solvent, respectively; (2) In an inert atmosphere, a zinc acetate solution and a shell-forming selenium precursor solution are injected into a reaction solution containing a zinc-modified quantum dot core to react, thereby forming an inner shell layer (ZnSe) on the surface of the zinc-modified quantum dot core; subsequently, a zinc acetate solution and a precursor mixed solution are injected and reacted to form an intermediate shell layer (ZnSeS) on the surface of the inner shell layer; finally, a zinc acetate solution and octanethiol are injected and reacted to form an outer shell layer (ZnS) on the surface of the intermediate shell layer, thereby obtaining a crude reaction solution; The zinc acetate solution is prepared by dissolving zinc acetate in a high boiling point solvent; the shell-forming selenium precursor solution is prepared by dissolving selenium in a ligand solvent; the precursor mixed solution is prepared by dissolving selenium and sulfur in a ligand solvent; (3) The product in the crude reaction solution is purified to obtain broad-emission zinc telluride selenide quantum dots.
[0009] Preferably, the high boiling point solvent includes at least one of 1-octadecene, liquid paraffin and oleic acid.
[0010] Preferably, the ligand solvent includes at least one of tri-n-octylphosphine, diphenylphosphine, oleylamine and octanethiol.
[0011] Preferably, in the step (1), the amount of zinc acetate in the zinc acetate reaction solution is 1.2-3 mmol, the amount of oleylamine is 0.5-1.5 mL, the amount of oleic acid is 2-6 mL, and the amount of the high boiling point solvent is 14-30 mL.
[0012] Preferably, in step (1), the amount of tellurium in the tellurium precursor solution is 0.02-0.05 mmol, and the amount of the ligand solvent is 0.5-2 mL.
[0013] Preferably, in step (1), the amount of selenium in the selenium precursor solution is 0.8-1.5 mmol, and the amount of the ligand solvent is 0.5-2 mL.
[0014] Preferably, in step (1), the zinc halide comprises at least one of zinc chloride, zinc bromide and zinc iodide; and the amount of the zinc halide used is 3-6 mmol.
[0015] Preferably, in step (1), the temperature of the nucleation reaction is 240-320°C, and the reaction time is 1-4 h.
[0016] Preferably, in step (1), the time for adding zinc halide and reacting is 10-90 min.
[0017] Preferably, in step (2), the concentration of the zinc acetate solution is 0.4-0.6 mol / L; the concentration of the shell-forming selenium precursor solution is 0.15-0.55 mol / L; the concentration of selenium in the precursor mixed solution is 0.15-0.55 mol / L, and the concentration of sulfur is 0.15-0.55 mol / L.
[0018] Further preferably, in the reaction of forming the inner shell layer, the intermediate shell layer and the outer shell layer, the amount of zinc acetate solution used is independently 2-5 mL; the amount of shell-forming selenium precursor solution used is 1-2 mL; the amount of precursor mixed solution used is 1-2 mL; and the amount of octanethiol used is 0.6-1.2 mL.
[0019] Preferably, in step (2), the reaction temperatures for forming the inner shell layer and the intermediate shell layer are independently 240-320°C, and the reaction times are independently 10-40 min; the reaction temperature for forming the outer shell layer is 230-320°C, and the reaction time is 0.5-1.5 h.
[0020] In the present invention, those skilled in the art can use hot injection to complete the injection of raw materials, including rapid injection or dropwise addition. The hot injection process can be carried out at a wide range of temperatures. For example, in actual operation, the hot injection operation can be completed at room temperature to 170°C. In addition, after the synthesis is completed, the product can be easily purified using purification reagents such as ethanol and n-octane. Other purification methods in the art can also achieve the purpose of this step.
[0021] In the second aspect of the present invention, there is provided a broad emission zinc telluride selenide quantum dot with high quantum yield and broad spectrum emission, which is prepared by the method of the first aspect of the present invention.
[0022] In the third aspect of the present invention, there is provided an application of the broad-emission zinc telluride selenide quantum dots according to the second aspect of the present invention, specifically an application as a fluorescent emission material in the preparation of a white light lighting device.
[0023] Preferably, the application method comprises the following steps: using broad-emission zinc telluride selenide quantum dots and quantum dots in the blue light emission band as fluorescent emission materials to prepare a white light-emitting diode.
[0024] Based on the above technical scheme, the inventive concept and principle of the present invention is that in the initial stage of synthesizing wide-emission zinc telluride selenide quantum dots, the surface of ZnSeTe quantum dots that are not modified by zinc halides is coated with long-chain organic ligands such as oleylamine and oleic acid. These organic ligands have large steric hindrance and are used to form a ligand layer to passivate the surface of the quantum dots, thereby reducing the surface energy. When zinc halides are added, they bind to the zinc atoms on the surface of the quantum dots in the form of ligands, thereby replacing the original long-chain organic ligands. On the one hand, smaller steric hindrance makes it easy for a large number of precursors to contact the surface of the quantum dots, thereby affecting the morphology of the quantum dots. The binding ability of zinc halides is stronger than that of organic ligands such as oleylamine and oleic acid, and therefore it is easier to bind to the surface of the quantum dots, causing the surface to grow in a selective crystal face. On the other hand, due to the lack of passivation of long-chain ligands, some surface defects are exposed. These defects can form dangling orbits in the band gap, produce strong defect state emission, and thus broaden the fluorescence emission band of zinc telluride selenide quantum dots, so that its emission spectrum can cover the band from green to yellow to red in the visible light range, and is not limited to the blue band. The modification of zinc halide in the present invention does not change the crystal structure of quantum dots, and has a similar morphology and crystal structure to unmodified quantum dots, but its surface state has changed, resulting in a huge change in its emission wavelength.
[0025] It should be noted that the technical means of the present invention is fundamentally different from the scheme using similar raw materials in the prior art. For example, in the literature (Yang Weihai, Yan Shoulei, Wei Chen, et al. Green Synthesis of CdSe Quantum Dots Stabilized by Oleylamine / Oleic Acid [J]. Journal of Analysis and Testing, 2010 (1): 5. DOI: 10.3969 / j.issn.1004-4957.2010.01.001.), liquid paraffin is used as a high-temperature reaction solvent, oleic acid and oleylamine are mixed stabilizers, and CdSe quantum dots are synthesized in one step by high-temperature pyrolysis. The results of the literature show that the absorption spectrum peak of quantum dots stabilized by oleylamine / oleic acid mixed surfactant is sharper and the half-peak width of the fluorescence emission spectrum is narrower. In the present invention, oleylamine and oleic acid are first used to coat ZnSeTe quantum dots, and then the ligand is replaced by zinc halide to form a dangling orbit, achieving a technical effect that is completely different from that of the literature.
[0026] The small size and strong binding ability of inorganic halide molecules help to enhance the stability of quantum dots and improve the carrier migration ability. Its participation in the synthesis of quantum dots as a surface ligand is an emerging strategy that is developing. For example, the inventor's research group provides a method for reducing the fluorescence half-peak width of core-shell indium phosphide quantum dots in the Chinese invention patent with publication number CN115710505A. By doping a certain proportion of ligand zinc halide in the intermediate step of indium phosphide nucleation and shell coating, the zinc halide is absorbed on the surface of the quantum dots as a ligand to alleviate Ostwald ripening and optimize the performance of intrinsic emission. In the present invention, there is a significant difference between defect state emission and intrinsic emission, which is mainly reflected in the red shift of emission wavelength and the broadening of emission peak. Different from the previous scheme of using zinc halide to narrow the line width of indium phosphide quantum dots and improve the photoluminescence quantum yield, the zinc halide modification strategy of the present invention is essentially the introduction of defect state emission, which leads to the red shift of the peak and the broadening of the peak width, while the former is mainly the passivation of the surface of the quantum dots by zinc halide and the performance improvement caused by it.
[0027] Compared with the prior art, the present invention has the following advantages and beneficial effects: The present invention provides a method for preparing broad-emission zinc telluride selenide quantum dots. Through artificially designed defect state emission, the emission wavelength of the zinc telluride selenide quantum dots is red-shifted and broadened without changing the particle size, absorption spectrum and crystal structure of the quantum dots. The method has the advantages of low preparation cost, simple and efficient process.
[0028] The invention provides a broad-emission zinc telluride selenide quantum dot, which has the characteristics of high quantum yield and broad-spectrum emission.
[0029] The present invention provides an application of broad-emission zinc telluride selenide quantum dots, which, as fluorescent emission materials, have broad application prospects in the field of white light illumination. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a transmission electron microscope (TEM) image of the broad emission zinc telluride selenide quantum dots of Example 1; Figure 2 Ultraviolet absorption (UV) and fluorescence (PL) spectra of the broad-emission zinc telluride selenide quantum dots of Example 1; Figure 3 is an X-ray diffraction (XRD) pattern of the broad emission zinc telluride selenide quantum dots of Example 1; Figure 4 This is a transmission electron microscope image of blue-light zinc telluride selenide quantum dots; Figure 5This is the ultraviolet absorption and fluorescence spectra of blue light zinc telluride selenide quantum dots; Figure 6 This is the X-ray diffraction pattern of blue light zinc telluride selenide quantum dots; Figure 7 is the emission spectrum of a white light emitting diode. DETAILED DESCRIPTION
[0031] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0032] Example 1 The preparation method of broad emission zinc telluride selenide quantum dots comprises the following steps: (1) In a 100 mL four-necked flask, 2 mmol of anhydrous zinc acetate, 2 mL of oleic acid, 1 mL of oleylamine and 15 mL of 1-octadecene were added to form a zinc acetate reaction solution, which was heated to 300 °C and introduced with argon. 1 mmol of selenium powder was dissolved in 0.5 mL of diphenylphosphine to obtain a nucleating selenium precursor solution, and 0.02 mmol of tellurium powder was dissolved in 0.5 mL of tri-n-octylphosphine to obtain a tellurium precursor solution. The nucleation selenium precursor solution and the tellurium precursor solution were injected into the flask containing the zinc acetate reaction solution in sequence, and the nucleation reaction was carried out for 1 h while stirring. Subsequently, 3-6 mmol of zinc chloride was weighed and quickly added into the flask and the reaction was continued for 30 min to obtain a reaction solution containing zinc-modified quantum dot cores. (2) Dissolving zinc acetate in oleic acid to prepare a zinc acetate solution with a concentration of 0.4 mol / L; dissolving selenium in tri-n-octylphosphine to prepare a shell-forming selenium precursor solution with a concentration of 0.55 mol / L; dissolving selenium and sulfur in tri-n-octylphosphine to prepare a precursor mixed solution with selenium and sulfur concentrations of 0.55 mol / L; 3 mL of zinc acetate solution and 1.5 mL of shell-forming selenium precursor solution were slowly injected into the reaction solution containing zinc-modified quantum dot cores, and the reaction was carried out at 300 °C for 30 min to complete the growth of the inner shell layer on the zinc-modified quantum dot cores; then 3 mL of zinc acetate solution and 1.5 mL of precursor mixed solution were injected, and the reaction was carried out at 300 °C for 30 min to complete the growth of the middle shell layer; finally, 3 mL of zinc acetate solution and 1 mL of octanethiol were injected, and the reaction was carried out at 230 °C for 30 min to complete the growth of the outer shell layer. After the reaction was completed, the solution was cooled to room temperature to obtain a crude reaction solution; (3) Purify the crude reaction solution with ethanol or n-octane to obtain broad-emission zinc telluride selenide quantum dots.
[0033] The broad emission ZnTe quantum dots prepared in this embodiment were tested and characterized. The microscopic morphology of the broad emission ZnTe quantum dots was observed using a transmission electron microscope. Figure 1 As shown; UV absorption spectrum and fluorescence spectrometer were used to test the broad emission ZnSe quantum dots, and the UV absorption and fluorescence spectra were shown in Figure 2 As shown; X-ray diffractometer was used to characterize the broad emission ZnSe quantum dots, and its XRD spectrum is shown as Figure 3 shown.
[0034] The above test results show that the average particle size of broad-emission zinc telluride selenide quantum dots is 7 nm, the fluorescence peak is 551 nm, and the quantum yield is 50%. Figure 1 It shows that the broad emission ZnTe quantum dots have good dispersion; Figure 2 It shows that the modified quantum dots can cover a wide range of green, yellow and red wavelengths; Figure 3 The spectrum shows that the broad emission zinc telluride selenide quantum dots have a zinc blende structure, which is a common cubic phase structure and also a common structure that can emit fluorescence. Quantum dots with fluorescence emission capability are synthesized through the above steps.
[0035] Example 2 The preparation method of broad emission zinc telluride selenide quantum dots comprises the following steps: (1) In a 100 mL four-necked flask, 1.2 mmol of anhydrous zinc acetate, 2 mL of oleic acid, 0.5 mL of oleylamine and 14 mL of 1-octadecene were added to prepare a zinc acetate reaction solution, which was heated to 240 °C and introduced with argon gas; 0.8 mmol of selenium powder was dissolved in 0.5 mL of diphenylphosphine to obtain a nucleating selenium precursor solution, and 0.02 mmol of tellurium powder was dissolved in 0.5 mL of tri-n-octylphosphine to obtain a tellurium precursor solution; The nucleation selenium precursor solution and the tellurium precursor solution were injected into the flask containing the zinc acetate reaction solution in sequence, and the nucleation reaction was carried out for 4 h while stirring. Subsequently, 3-6 mmol of zinc chloride was weighed and quickly added into the flask and the reaction was continued for 90 min to obtain a reaction solution containing zinc-modified quantum dot cores. (2) Dissolving zinc acetate in oleic acid to prepare a zinc acetate solution with a concentration of 0.4 mol / L; dissolving selenium in tri-n-octylphosphine to prepare a shell-forming selenium precursor solution with a concentration of 0.15 mol / L; dissolving selenium and sulfur in tri-n-octylphosphine to prepare a precursor mixed solution with selenium and sulfur concentrations of 0.15 mol / L; Slowly inject 2 mL of zinc acetate solution and 1 mL of shell-forming selenium precursor solution into the reaction solution containing zinc-modified quantum dot cores, react at 240 °C for 40 min, and complete the growth of the inner shell layer on the zinc-modified quantum dot core; then inject 2 mL of zinc acetate solution and 1 mL of precursor mixed solution, react at 240 °C for 40 min to complete the growth of the middle shell layer; finally inject 3 mL of zinc acetate solution and 0.6 mL of octanethiol, react at 230 °C for 90 min to complete the growth of the outer shell layer, and after the reaction, cool the solution to room temperature to obtain a crude reaction solution; (3) Purify the crude reaction solution with ethanol or n-octane to obtain broad-emission zinc telluride selenide quantum dots.
[0036] Example 3 The preparation method of broad emission zinc telluride selenide quantum dots comprises the following steps: (1) In a 100 mL four-necked flask, 3 mmol of anhydrous zinc acetate, 6 mL of oleic acid, 1.5 mL of oleylamine and 30 mL of 1-octadecene were added to prepare a zinc acetate reaction solution, which was heated to 320 °C and introduced with argon. 1.5 mmol of selenium powder was dissolved in 2 mL of diphenylphosphine to obtain a nucleating selenium precursor solution, and 0.05 mmol of tellurium powder was dissolved in 2 mL of tri-n-octylphosphine to obtain a tellurium precursor solution. The nucleation selenium precursor solution and the tellurium precursor solution were injected into the flask containing the zinc acetate reaction solution in sequence, and the nucleation reaction was carried out for 1 h while stirring. Subsequently, 3-6 mmol of zinc chloride was weighed and quickly added into the flask and the reaction was continued for 10 min to obtain a reaction solution containing zinc-modified quantum dot cores. (2) Dissolving zinc acetate in oleic acid to prepare a zinc acetate solution with a concentration of 0.6 mol / L; dissolving selenium in tri-n-octylphosphine to prepare a shell-forming selenium precursor solution with a concentration of 0.55 mol / L; dissolving selenium and sulfur in tri-n-octylphosphine to prepare a precursor mixed solution with selenium and sulfur concentrations of 0.55 mol / L; Slowly inject 5 mL of zinc acetate solution and 2 mL of shell-forming selenium precursor solution into the reaction solution containing zinc-modified quantum dot cores, react at 320 °C for 10 min, and complete the growth of the inner shell layer on the zinc-modified quantum dot core; then inject 5 mL of zinc acetate solution and 2 mL of precursor mixed solution, react at 320 °C for 10 min to complete the growth of the middle shell layer; finally inject 5 mL of zinc acetate solution and 1.2 mL of octanethiol, react at 320 °C for 30 min to complete the growth of the outer shell layer, and after the reaction, cool the solution to room temperature to obtain a crude reaction solution; (3) Purify the crude reaction solution with ethanol or n-octane to obtain broad-emission zinc telluride selenide quantum dots.
[0037] Comparative Example 1 The preparation method of blue light zinc telluride selenide quantum dots comprises the following steps: (1) In a 100 mL four-necked flask, 2 mmol of anhydrous zinc acetate, 2 mL of oleic acid, 1 mL of oleylamine and 15 mL of 1-octadecene were added to form a zinc acetate reaction solution, which was heated to 300 °C and introduced with argon. 1 mmol of selenium powder was dissolved in 0.5 mL of diphenylphosphine to obtain a nucleating selenium precursor solution, and 0.02 mmol of tellurium powder was dissolved in 0.5 mL of tri-n-octylphosphine to obtain a tellurium precursor solution. The nucleation selenium precursor solution and the tellurium precursor solution were injected into the flask containing the zinc acetate reaction solution in sequence, and the nucleation reaction was carried out for 1 h while stirring to obtain a reaction solution containing quantum dot cores. (2) Dissolving zinc acetate in oleic acid to prepare a zinc acetate solution with a concentration of 0.4 mol / L; dissolving selenium in tri-n-octylphosphine to prepare a shell-forming selenium precursor solution with a concentration of 0.55 mol / L; dissolving selenium and sulfur in tri-n-octylphosphine to prepare a precursor mixed solution with selenium and sulfur concentrations of 0.55 mol / L; 3 mL of zinc acetate solution and 1.5 mL of shell-forming selenium precursor solution were slowly injected into the reaction solution containing the quantum dot core, and the reaction was carried out at 300 °C for 30 min to complete the growth of the inner shell layer on the zinc-modified quantum dot core; then 3 mL of zinc acetate solution and 1.5 mL of the precursor mixed solution were injected, and the reaction was carried out at 300 °C for 30 min to complete the growth of the middle shell layer; finally, 3 mL of zinc acetate solution and 1 mL of octanethiol were injected, and the reaction was carried out at 230 °C for 30 min to complete the growth of the outer shell layer. After the reaction, the solution was cooled to room temperature to obtain a crude reaction solution; (3) The crude reaction solution is purified using ethanol or n-octane to obtain blue light emitting zinc telluride selenide quantum dots.
[0038] The broad emission ZnTe quantum dots prepared in this comparative example were tested and characterized. The microscopic morphology of the blue light ZnTe quantum dots was observed using a transmission electron microscope. Figure 4 As shown; the blue light zinc telluride selenide quantum dots were tested using ultraviolet absorption spectrometer and fluorescence spectrometer, and its ultraviolet absorption and fluorescence spectra are shown in Figure 5 As shown; X-ray diffractometer was used to characterize the blue light zinc telluride selenide quantum dots, and its XRD spectrum is shown as Figure 6 shown.
[0039] The above test results show that the average particle size of blue light zinc telluride selenide quantum dots is 7 nm, the fluorescence peak is 440 nm, and the quantum yield is 32%. Figure 4 It shows that blue light zinc telluride selenide quantum dots also have good dispersion; Figure 5 It shows that unmodified quantum dots can only cover the blue light band in the range of 460-480 nm; Figure 6The spectrum shows that the broad emission zinc telluride quantum dots have a zinc blende structure.
[0040] In order to study the application effect of the broad-emission zinc telluride selenide quantum dots prepared in Example 1, the broad-emission zinc telluride selenide quantum dots and blue-light zinc telluride selenide quantum dots were used together to construct white light-emitting diodes. Take the broad-emission zinc telluride selenide quantum dot and blue-light zinc telluride selenide quantum dot powder, mix them with epoxy resin AB glue, and then add them dropwise to a UV chip with an excitation wavelength of 365 nm, and let it stand and cure for 10 hours. A white light-emitting diode can be obtained after being powered on with a constant current and lit up. The emission spectrum of the white light-emitting diode is measured, and the results are as follows: Figure 7 As shown. Figure 7 It can be seen that by combining quantum dots with two emission bands (broad emission zinc telluride quantum dots and blue light zinc telluride quantum dots) into a diode, white light emission is achieved; white light-emitting diodes have a wider coverage band in the visible light range and are closer to the real solar spectrum.
[0041] The above results show that the present invention broadens the fluorescence emission band of zinc telluride selenide quantum dots through artificially designed guided defect state emission, so that its emission spectrum can cover the band from green to yellow to red in the visible light range, and is not limited to the blue band. For the first time, the present invention uses only zinc telluride selenide quantum dots, and uses wide-emission zinc telluride selenide quantum dots and existing blue-light zinc telluride selenide quantum dots as fluorescence emission materials to construct a white light-emitting diode, which has good application prospects in the field of white light illumination.
[0042] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A method for preparing broad-emission zinc telluride selenide quantum dots, characterized in that: The steps include: (1) In an inert atmosphere, a tellurium precursor solution and a nucleation selenium precursor solution are injected into a zinc acetate reaction solution to carry out a nucleation reaction; after the nucleation reaction is completed, zinc halide is continuously added and reacted to obtain a reaction solution containing zinc-modified quantum dot cores; The zinc acetate reaction solution is prepared by dissolving zinc acetate in a high boiling point solvent and adding oleylamine and oleic acid; the tellurium precursor solution and the nucleation selenium precursor solution are prepared by dissolving tellurium and selenium in a ligand solvent, respectively; (2) In an inert atmosphere, a zinc acetate solution and a shell-forming selenium precursor solution are injected into a reaction solution containing a zinc-modified quantum dot core to react, thereby forming an inner shell layer on the surface of the zinc-modified quantum dot core; subsequently, a zinc acetate solution and a precursor mixed solution are injected and reacted to form an intermediate shell layer on the surface of the inner shell layer; finally, a zinc acetate solution and octanethiol are injected and reacted to form an outer shell layer on the surface of the intermediate shell layer, thereby obtaining a crude reaction solution; The zinc acetate solution is prepared by dissolving zinc acetate in a high boiling point solvent; the shell-forming selenium precursor solution is prepared by dissolving selenium in a ligand solvent; the precursor mixed solution is prepared by dissolving selenium and sulfur in a ligand solvent; (3) The product in the crude reaction solution is purified to obtain broad-emission zinc telluride selenide quantum dots.
2. The method for preparing broad-emission zinc telluride selenide quantum dots according to claim 1, characterized in that: The high boiling point solvent includes at least one of 1-octadecene, liquid paraffin and oleic acid; the ligand solvent includes at least one of tri-n-octylphosphine, diphenylphosphine, oleylamine and octanol.
3. The method for preparing broad emission zinc telluride selenide quantum dots according to claim 1, characterized in that: In the step (1), the amount of zinc acetate in the zinc acetate reaction solution is 1.2-3 mmol, the amount of oleylamine is 0.5-1.5 mL, the amount of oleic acid is 2-6 mL, and the amount of the high boiling point solvent is 14-30 mL; the amount of tellurium in the tellurium precursor solution is 0.02-0.05 mmol, and the amount of the ligand solvent is 0.5-2 mL; the amount of selenium in the selenium precursor solution is 0.8-1.5 mmol, and the amount of the ligand solvent is 0.5-2 mL.
4. The method for preparing broad emission zinc telluride selenide quantum dots according to claim 1, characterized in that: In the step (1), the zinc halide includes at least one of zinc chloride, zinc bromide and zinc iodide; and the amount of the zinc halide used is 3-6 mmol.
5. The method for preparing broad emission zinc telluride selenide quantum dots according to claim 1, characterized in that: In the step (1), the temperature of the nucleation reaction is 240-320°C, the reaction time is 1-4 h, and the time for adding zinc halide and reacting is 10-90 min.
6. The method for preparing broad emission zinc telluride selenide quantum dots according to claim 1, characterized in that: In the step (2), the concentration of the zinc acetate solution is 0.4-0.6 mol / L; the concentration of the shell-forming selenium precursor solution is 0.15-0.55 mol / L; the concentration of selenium in the precursor mixed solution is 0.15-0.55 mol / L, and the concentration of sulfur is 0.15-0.55 mol / L.
7. The method for preparing broad emission zinc telluride selenide quantum dots according to claim 6, characterized in that: In the reaction of forming the inner shell layer, the middle shell layer and the outer shell layer, the amount of zinc acetate solution used is 2-5 mL respectively; the amount of shell-forming selenium precursor solution used is 1-2 mL; the amount of precursor mixed solution used is 1-2 mL; and the amount of octanethiol used is 0.6-1.2 mL.
8. The method for preparing broad emission zinc telluride selenide quantum dots according to claim 1, characterized in that: In the step (2), the temperature of the reaction for forming the inner shell layer and the intermediate shell layer is independently 240-320°C, and the reaction time is independently 10-40 min; the reaction for forming the outer shell layer is 230-320°C, and the reaction time is 0.5-1.5 h.
9. A broad emission zinc telluride selenide quantum dot, characterized in that: The method is prepared according to any one of claims 1 to 9.