Preparation method of normal-temperature low-pressure biomass particles
By using the preparation method of low-pressure biomass particles in the biomass fuel, the use of specific raw materials and processes to improve the calorific value and combustion performance of the fuel, the problem of low calorific value of biomass fuel is solved, and the goal of resource recycling and environmental protection is achieved. Prove broad market prospects and development potential.
Patent Information
- Application Number
- CN202411171296.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The low calorific value of existing biomass fuels leads to excessive combustion rates in the precision processing industry, interfering with production processes, and preparation technology limits fuel quality improvement and limits its application potential in a wider range of fields.
Using the preparation method of low-pressure biomass granules at room temperature, the cow dung, black pine leaves, poplar chips, cinders, vegetable oils, bonding aids and combustion aids in a specific proportion, and fermentation and extrusion into a column by stacking. shaped particles significantly improve the calorific value and combustion performance of the fuel.
It significantly improves the calorific value and combustion performance of biomass fuels, reduces dependence on fossil fuels, maximizes the recycling of resources, reduces production costs, and takes solid steps in the field of environmental protection.
Smart Images

Figure BDA0005009346550000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of biomass pellet fuel, and in particular to a method for preparing biomass pellets at room temperature and low pressure. Background Art
[0002] Biomass fuel, as a way of converting agricultural and forestry waste (such as straw, sawdust, bagasse, rice bran, etc.) into energy through combustion, is in sharp contrast to fossil fuels. However, under the current environmental protection policy framework, direct combustion of such biomass is regarded as a highly polluting behavior, so its application is mostly limited to traditional stoves in rural areas and strictly restricted in cities. The main application form of biomass fuel focuses on molded fuel, which is an innovative clean energy solution. It is made into a solid form (block, granular, etc.) that is easy to burn directly through fine processing of agricultural and forestry waste - including crushing, proportioning, molding, drying and other processes. Thanks to the low ignition point and high purity of the raw materials, biomass molded fuel exhibits efficient combustion characteristics, but at the same time, its fast combustion rate also brings a double-edged sword effect.
[0003] Rapid combustion means that energy is released in a concentrated manner in a short period of time, which is not a problem for ordinary applications and can even meet the needs efficiently. However, in the precision machining industry, this feature may become a challenge. Because a stable and lasting heat source is the key to ensuring fine control of the production process, and the explosive heat release of biomass fuels may cause sudden temperature changes, interfere with the production process, and damage product quality and even equipment safety.
[0004] Current biomass fuel preparation technologies mostly rely on simple extrusion molding of raw materials. This practice limits the improvement of fuel quality, resulting in a low calorific value of the final product, which in turn limits the application potential of biomass fuel in a wider range of fields. In view of the environmental pressure and carbon emissions caused by the consumption of coal resources, the development of a high-efficiency, low-carbon and environmentally friendly biomass fuel has become an urgent need for scientific research and industry. This new type of fuel aims to significantly increase calorific value output through advanced processing technology, reduce dependence on traditional energy sources such as coal, thereby effectively alleviating environmental pollution and promoting green and sustainable development. In short, exploring efficient and environmentally friendly biomass fuel preparation technologies, aiming to achieve energy structure optimization and environmentally friendly protection, is a hot topic and trend in current research. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a method for preparing biomass particles at room temperature and low pressure.
[0006] On one hand, the present invention provides a biomass pellet, comprising the following raw materials in parts by weight: 20-30 parts of cow dung, 10-15 parts of black pine leaves, 5-8 parts of poplar sawdust, 15-20 parts of coal slag, 8-12 parts of vegetable oil, 3-6 parts of bonding aid, and 1-3 parts of combustion aid.
[0007] Preferably, the bonding aid is prepared by the following method:
[0008] Corn stalks, peanut shells and rice husks with a mass ratio of 1:1:0.3-0.5 are dried and mixed evenly, then crushed through a 100-200 mesh sieve to obtain a mixed powder, the mixed powder with a mass ratio of 1:5-8 and a 40% mass fraction hydrogen peroxide solution are mixed evenly, 0.5M sodium hydroxide solution is added to adjust the pH to 8-9, and stirred at 60-80°C for 15-30 minutes; then centrifuged at 8000-10000 rpm for 3-5 minutes to obtain a suspension, the pH of the suspension is adjusted to 9-10, a precipitant is added to precipitate lignin in the suspension, and the suspension is filtered, dried, crushed and sieved to obtain a bonding agent.
[0009] Preferably, the precipitant comprises starch, calcium chloride and sodium bicarbonate in a mass ratio of 1:0.5-0.8:0.1-0.3.
[0010] Preferably, the mass ratio of the precipitant to the suspension is 0.05-0.08:1.
[0011] Preferably, the combustion aid comprises potassium nitrate and magnesium powder in a mass ratio of 0.3-0.5:1.
[0012] Another aspect of the present invention provides a method for preparing biomass particles at room temperature and low pressure, which adopts the following technical scheme:
[0013] S1, the mass parts of cow dung, black pine leaves, coal slag, poplar sawdust, vegetable oil, bonding aid, combustion aid are stirred evenly, crushed, and passed through a 100-200 mesh sieve to obtain a mixture;
[0014] S2, inoculating a starter into the mixture, and fermenting by stacking fermentation to obtain a fermented product;
[0015] S3, extruding the fermented product into cylindrical particles, and drying at 100° C. for 12-24 hours to obtain room temperature and low pressure biomass particles.
[0016] Preferably, the fermentation agent comprises Propionibacterium freudenreichii, protease and Bacillus subtilis in a mass ratio of 1:0.3-0.5:0.5-0.8.
[0017] Preferably, the inoculation method is specifically as follows: diluting the starter in deionized water 10-15 times its own weight, and then inoculating in the form of spraying.
[0018] Preferably, the stacking fermentation method specifically includes: the mixture is stacked at a height of 2-2.5 m and undergoes a fermentation process of 3-5 days.
[0019] In summary, the present invention has the following beneficial effects:
[0020] The present invention effectively solves the problem of low calorific value of crop biomass fuel combustion, not only significantly improves the economic value of crop waste, but also enhances the energy density of biomass fuel. This promotes the maximum recycling of resources, and takes solid steps in the field of environmental protection, showing extremely high social promotion value and environmental friendliness. It effectively reduces dependence on limited and increasingly depleted fossil fuels, bringing significant cost savings to enterprises; as a green alternative to traditional energy sources such as coal and oil, it heralds a new energy path for sustainable development, showing broad market prospects and huge development potential. The combustion rate is accelerated, allowing the fuel to be converted into thermal energy more quickly; at the same time, the combustion process becomes more sufficient and thorough, ensuring the maximum utilization of the fuel, thereby achieving a significant increase in calorific value. DETAILED DESCRIPTION
[0021] The present application is further described in detail below in conjunction with the examples, but is not limited thereto. Other features and advantages disclosed in the present application will become apparent from the following detailed description and examples, which should not be construed as limiting.
[0022] Example 1
[0023] A method for preparing biomass particles at room temperature and low pressure comprises the following steps:
[0024] S1, 20 parts of cow dung, 10 parts of black pine leaves, 5 parts of poplar sawdust, 15 parts of coal slag, 8 parts of vegetable oil, 3 parts of bonding aid, and 1 part of combustion improver were stirred evenly, crushed, and passed through a 200-mesh sieve to obtain a mixture;
[0025] S2, Propionibacterium freudenreichii, protease and Bacillus subtilis in a mass ratio of 1:0.3:0.5 are diluted in deionized water 10 times their own weight, and then inoculated into the mixture in the form of spraying, and fermented by stacking fermentation. The stacking height of the mixture is 2m. After a fermentation process for 3 days, a fermentation product is obtained, wherein the mass ratio of the starter to the mixture is 1:20;
[0026] S3, extruding the fermented product into cylindrical particles, and drying at 80° C. for 24 hours to obtain room temperature and low pressure biomass particles.
[0027] The bonding aid is prepared by the following method: corn stalks, peanut shells and rice husks with a mass ratio of 1:1:0.3 are dried and mixed evenly, and then crushed through a 200-mesh sieve to obtain a mixed powder; the mixed powder with a mass ratio of 1:5 and a hydrogen peroxide solution with a mass fraction of 40% are mixed evenly, 0.5M sodium hydroxide solution is added to adjust the pH to 8, and stirred at 60°C for 30 minutes; then centrifuged at 8000rpm for 5 minutes to obtain a suspension, the pH of the suspension is adjusted to 9, a precipitant is added to precipitate lignin in the suspension, and the suspension is filtered, dried, crushed and sieved to obtain the bonding aid.
[0028] The precipitant is starch, calcium chloride and sodium bicarbonate in a mass ratio of 1:0.5:0.1; the mass ratio of the precipitant to the suspension is 0.05:1.
[0029] Among them, the combustion aid is potassium nitrate and magnesium powder with a mass ratio of 0.3:1.
[0030] Example 2
[0031] A method for preparing biomass particles at room temperature and low pressure comprises the following steps:
[0032] S1, 30 parts of cow dung, 15 parts of black pine leaves, 8 parts of poplar sawdust, 20 parts of coal slag, 12 parts of vegetable oil, 6 parts of bonding aid, and 3 parts of combustion aid were mixed evenly, crushed, and passed through a 100-mesh sieve to obtain a mixture;
[0033] S2, Propionibacterium freudenreichii, protease and Bacillus subtilis in a mass ratio of 1:0.5:0.8 are diluted in deionized water 15 times their own weight, and then inoculated into the mixture in the form of spraying, and fermented by stacking fermentation. The stacking height of the mixture is 2.5m. After a fermentation process for 5 days, a fermentation product is obtained, wherein the mass ratio of the starter to the mixture is 1:25;
[0034] S3, extruding the fermented product into cylindrical particles, and drying at 100° C. for 12 hours to obtain room temperature and low pressure biomass particles.
[0035] The bonding aid is prepared by the following method: corn stalks, peanut shells and rice husks with a mass ratio of 1:1:0.5 are dried and mixed evenly, and then crushed through a 200-mesh sieve to obtain a mixed powder; the mixed powder with a mass ratio of 1:8 and a hydrogen peroxide solution with a mass fraction of 40% are mixed evenly, 0.5M sodium hydroxide solution is added to adjust the pH to 9, and stirred at 80°C for 15 minutes; then centrifuged at 10000rpm for 3 minutes to obtain a suspension, the pH of the suspension is adjusted to 10, a precipitant is added to precipitate lignin in the suspension, and the bonding aid is obtained by filtering, drying, crushing and screening.
[0036] The precipitant is starch, calcium chloride and sodium bicarbonate in a mass ratio of 1:0.8:0.3; the mass ratio of the precipitant to the suspension is 0.08:1.
[0037] Among them, the combustion aid is potassium nitrate and magnesium powder with a mass ratio of 0.5:1.
[0038] Example 3
[0039] A method for preparing biomass particles at room temperature and low pressure comprises the following steps:
[0040] S1, 25 parts of cow dung, 12 parts of black pine leaves, 7 parts of poplar sawdust, 18 parts of coal slag, 10 parts of vegetable oil, 5 parts of bonding aid, and 2 parts of combustion aid were mixed and evenly crushed, and passed through a 200 mesh sieve to obtain a mixture;
[0041] S2, Propionibacterium freudenreichii, protease and Bacillus subtilis in a mass ratio of 1:0.4:0.6 are diluted in deionized water 13 times their own weight, and then inoculated into the mixture in the form of spraying, and fermented by stacking fermentation. The stacking height of the mixture is 2.3m. After a fermentation process for 4 days, a fermentation product is obtained, wherein the mass ratio of the starter to the mixture is 1:23;
[0042] S3, extruding the fermented product into cylindrical particles, and drying at 90° C. for 18 hours to obtain room temperature and low pressure biomass particles.
[0043] The bonding aid is prepared by the following method: corn stalks, peanut shells and rice husks with a mass ratio of 1:1:0.4 are dried and mixed evenly, and then crushed through a 200-mesh sieve to obtain a mixed powder; the mixed powder with a mass ratio of 1:7 and a hydrogen peroxide solution with a mass fraction of 40% are mixed evenly, 0.5M sodium hydroxide solution is added to adjust the pH to 8, and stirred at 70°C for 25 minutes; then centrifuged at 9000rpm for 4 minutes to obtain a suspension, the pH of the suspension is adjusted to 9, a precipitant is added to precipitate lignin in the suspension, and the suspension is filtered, dried, crushed and sieved to obtain the bonding aid.
[0044] The precipitant is starch, calcium chloride and sodium bicarbonate in a mass ratio of 1:0.7:0.2; the mass ratio of the precipitant to the suspension is 0.06:1.
[0045] Among them, the combustion aid is potassium nitrate and magnesium powder with a mass ratio of 0.4:1.
[0046] Example 4
[0047] A method for preparing biomass particles at room temperature and low pressure comprises the following steps:
[0048] S1, 22 parts of cow dung, 13 parts of black pine leaves, 6 parts of poplar sawdust, 16 parts of coal slag, 9 parts of vegetable oil, 4 parts of bonding aid, and 1 part of combustion aid were mixed and evenly crushed, and passed through a 100-mesh sieve to obtain a mixture;
[0049] S2, Propionibacterium freudenreichii, protease and Bacillus subtilis in a mass ratio of 1:0.3:0.7 are diluted in deionized water 12 times their own weight, and then inoculated into the mixture in the form of spraying, and fermented by stacking fermentation, the stacking height of the mixture is 2.1m, and after a fermentation process of 3 days, a fermentation product is obtained, wherein the mass ratio of the starter to the mixture is 1:20;
[0050] S3. Extruding the fermented product into cylindrical particles, and drying at 85° C. for 16 hours to obtain room temperature and low pressure biomass particles.
[0051] The bonding aid is prepared by the following method: corn stalks, peanut shells and rice husks with a mass ratio of 1:1:0.5 are dried and mixed evenly, and then crushed through a 200-mesh sieve to obtain a mixed powder; the mixed powder with a mass ratio of 1:6 and a hydrogen peroxide solution with a mass fraction of 40% are mixed evenly, 0.5M sodium hydroxide solution is added to adjust the pH to 8, and stirred at 65°C for 20 minutes; then centrifuged at 8000rpm for 3 minutes to obtain a suspension, the pH of the suspension is adjusted to 9, a precipitant is added to precipitate lignin in the suspension, and the suspension is filtered, dried, crushed and sieved to obtain the bonding aid.
[0052] The precipitant is starch, calcium chloride and sodium bicarbonate in a mass ratio of 1:0.6:0.1; the mass ratio of the precipitant to the suspension is 0.07:1.
[0053] Among them, the combustion aid is potassium nitrate and magnesium powder with a mass ratio of 0.3:1.
[0054] Comparative Example 1
[0055] A method for preparing biomass particles at room temperature and low pressure comprises the following steps:
[0056] S1, 22 parts of cow dung, 13 parts of black pine leaves, 6 parts of poplar sawdust, 16 parts of coal slag, 9 parts of vegetable oil, 4 parts of bonding aid, stir evenly, crush, and pass through a 100 mesh sieve to obtain a mixture;
[0057] S2, Propionibacterium freudenreichii, protease and Bacillus subtilis in a mass ratio of 1:0.3:0.7 are diluted in deionized water 12 times their own weight, and then inoculated into the mixture in the form of spraying, and fermented by stacking fermentation. The stacking height of the mixture is 2.1m. After a fermentation process for 3 days, a fermentation product is obtained, wherein the mass ratio of the starter to the mixture is 1:20;
[0058] S3. Extruding the fermented product into cylindrical particles, and drying at 85° C. for 16 hours to obtain room temperature and low pressure biomass particles.
[0059] The bonding aid is prepared by the following method: corn stalks, peanut shells and rice husks with a mass ratio of 1:1 and 0.5 are dried and mixed evenly, and then crushed through a 200-mesh sieve to obtain a mixed powder; the mixed powder with a mass ratio of 1:6 and a hydrogen peroxide solution with a mass fraction of 40% are mixed evenly, 0.5M sodium hydroxide solution is added to adjust the pH to 8, and stirred at 65°C for 20 minutes; then centrifuged at 8000rpm for 3 minutes to obtain a suspension, the pH of the suspension is adjusted to 9, a precipitant is added to precipitate lignin in the suspension, and the suspension is filtered, dried, crushed and sieved to obtain the bonding aid.
[0060] The precipitant is starch, calcium chloride and sodium bicarbonate in a mass ratio of 1:0.6:0.1; the mass ratio of the precipitant to the suspension is 0.07:1.
[0061] Comparative Example 2
[0062] A method for preparing biomass particles at room temperature and low pressure comprises the following steps:
[0063] S1, 22 parts of cow dung, 13 parts of black pine leaves, 6 parts of poplar sawdust, 16 parts of coal slag, 9 parts of vegetable oil, 4 parts of bonding aid, and 1 part of combustion aid were mixed and evenly crushed, and passed through a 100-mesh sieve to obtain a mixture;
[0064] S2, Propionibacterium freudenreichii, protease and Bacillus subtilis in a mass ratio of 1:0.3:0.7 are diluted in deionized water 12 times their own weight, and then inoculated into the mixture in the form of spraying, and fermented by stacking fermentation. The stacking height of the mixture is 2.1m. After a fermentation process for 3 days, a fermentation product is obtained, wherein the mass ratio of the starter to the mixture is 1:20;
[0065] S3. Extruding the fermented product into cylindrical particles, and drying at 85° C. for 16 hours to obtain room temperature and low pressure biomass particles.
[0066] The bonding aid is prepared by the following method: corn stalks, peanut shells and rice husks in a mass ratio of 1:1 and 0.5 are dried and mixed evenly, then crushed through a 200-mesh sieve to obtain a mixed powder, the mixed powder in a mass ratio of 1:6 and a hydrogen peroxide solution with a mass fraction of 40% are mixed evenly, 0.5M sodium hydroxide solution is added to adjust the pH to 8, and stirred at 65°C for 20 minutes; then centrifuged at 8000rpm for 3 minutes to obtain a suspension, the pH of the suspension is adjusted to 9, filtered, dried, crushed and sieved to obtain the bonding aid.
[0067] Among them, the combustion aid is potassium nitrate and magnesium powder with a mass ratio of 0.3:1.
[0068] Comparative Example 3
[0069] A method for preparing biomass particles at room temperature and low pressure comprises the following steps:
[0070] S1, 22 parts of cow dung, 13 parts of black pine leaves, 6 parts of poplar sawdust, 16 parts of coal slag, 9 parts of vegetable oil, 4 parts of bonding aid, and 1 part of combustion aid were mixed and evenly crushed, and passed through a 100-mesh sieve to obtain a mixture;
[0071] S2, Propionibacterium freudenreichii, protease and Bacillus subtilis in a mass ratio of 1:0.3:0.7 are diluted in deionized water 12 times their own weight, and then inoculated into the mixture in the form of spraying, and fermented by stacking fermentation. The stacking height of the mixture is 2.1m. After a fermentation process for 3 days, a fermentation product is obtained, wherein the mass ratio of the starter to the mixture is 1:20;
[0072] S3. Extruding the fermented product into cylindrical particles, and drying at 85° C. for 16 hours to obtain room temperature and low pressure biomass particles.
[0073] The bonding agent is prepared by the following method: corn stalks, peanut shells and rice husks with a mass ratio of 1:1:0.5 are dried and mixed evenly, and then crushed through a 200-mesh sieve to obtain a mixed powder.
[0074] The combustion aid is potassium nitrate and magnesium powder with a mass ratio of 0.3:1.
[0075] Comparative Example 4
[0076] A method for preparing biomass particles at room temperature and low pressure comprises the following steps:
[0077] S1, 22 parts of cow dung, 13 parts of black pine leaves, 6 parts of poplar sawdust, 16 parts of coal slag, 9 parts of vegetable oil, 4 parts of bonding aid, and 1 part of combustion aid were mixed and evenly crushed, and passed through a 100-mesh sieve to obtain a mixture;
[0078] S2, diluting Propionibacterium freudenreichii, protease and Bacillus subtilis in a mass ratio of 1:0.3:0.7 in deionized water 12 times their own weight, and then inoculating them into the mixture in the form of spraying, and after a fermentation process for 3 days, obtaining a fermentation product, wherein the mass ratio of the starter to the mixture is 1:20;
[0079] S3. Extruding the fermented product into cylindrical particles, and drying at 85° C. for 16 hours to obtain room temperature and low pressure biomass particles.
[0080] The bonding aid is prepared by the following method: corn stalks, peanut shells and rice husks with a mass ratio of 1:1 and 0.5 are dried and mixed evenly, and then crushed through a 200-mesh sieve to obtain a mixed powder; the mixed powder with a mass ratio of 1:6 and a hydrogen peroxide solution with a mass fraction of 40% are mixed evenly, 0.5M sodium hydroxide solution is added to adjust the pH to 8, and stirred at 65°C for 20 minutes; then centrifuged at 8000rpm for 3 minutes to obtain a suspension, the pH of the suspension is adjusted to 9, a precipitant is added to precipitate lignin in the suspension, and the suspension is filtered, dried, crushed and sieved to obtain the bonding aid.
[0081] The precipitant is starch, calcium chloride and sodium bicarbonate in a mass ratio of 1:0.6:0.1; the mass ratio of the precipitant to the suspension is 0.07:1.
[0082] The combustion aid is potassium nitrate and magnesium powder with a mass ratio of 0.3:1.
[0083] Performance Testing
[0084] The combustion performance of the biomass particles prepared in Examples 1-4 and Comparative Examples 1-4 was tested respectively, and the results are shown in the following table.
[0085] Table 1
[0086]
[0087] The test results show that in the process of preparing biomass particles, the particles prepared according to Examples 1-4 exhibited higher calorific value, better combustion performance and extremely low smoke emission. In contrast, the biomass particles prepared in Comparative Examples 1-4 showed low combustion efficiency and were accompanied by higher smoke. This also shows that the reasonable ratio of the combustion aid and the precipitant plays an important role in improving the combustion performance and environmental performance of the biomass particles.
Claims
1. A biomass particle, characterized in that: The invention comprises the following raw materials in parts by weight: 20-30 parts of cow dung, 10-15 parts of black pine leaves, 5-8 parts of poplar wood chips, 15-20 parts of coal slag, 8-12 parts of vegetable oil, 3-6 parts of bonding aid and 1-3 parts of combustion aid.
2. A biomass particle according to claim 1, characterized in that: The bonding aid is prepared by the following method: Corn stalks, peanut shells and rice husks with a mass ratio of 1:1:0.3-0.5 are dried and mixed evenly, then crushed through a 100-200 mesh sieve to obtain a mixed powder, the mixed powder with a mass ratio of 1:5-8 and a 40% mass fraction hydrogen peroxide solution are mixed evenly, 0.5M sodium hydroxide solution is added to adjust the pH to 8-9, and stirred at 60-80°C for 15-30 minutes; then centrifuged at 8000-10000 rpm for 3-5 minutes to obtain a suspension, the pH of the suspension is adjusted to 9-10, a precipitant is added to precipitate lignin in the suspension, and the suspension is filtered, dried, crushed and sieved to obtain a bonding agent.
3. A biomass particle according to claim 2, characterized in that: The precipitant comprises starch, calcium chloride and sodium bicarbonate in a mass ratio of 1:0.5-0.8:0.1-0.
3.
4. The biomass particle according to claim 2, characterized in that: The mass ratio of the precipitant to the suspension is 0.05-0.08:
1.
5. The biomass particle according to claim 1, characterized in that: The combustion improver comprises potassium nitrate and magnesium powder in a mass ratio of 0.3-0.5:
1.
6. A method for preparing normal temperature and low pressure biomass particles according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: S1, the mass parts of cow dung, black pine leaves, coal slag, poplar sawdust, vegetable oil, bonding aid, combustion aid are stirred evenly, crushed, and passed through a 100-200 mesh sieve to obtain a mixture; S2, inoculating a starter into the mixture, and fermenting by stacking fermentation to obtain a fermented product; S3, extruding the fermented product into cylindrical particles, and drying at 80-100° C. for 12-24 hours to obtain room temperature and low pressure biomass particles.
7. The method for preparing normal temperature and low pressure biomass particles according to claim 6, characterized in that: The fermentation agent comprises Propionibacterium freudenreichii, protease and Bacillus subtilis in a mass ratio of 1:0.3-0.5:0.5-0.8, and the mass ratio of the fermentation agent to the mixture is 1:20-25.
8. The method for preparing normal temperature and low pressure biomass particles according to claim 6, characterized in that: The inoculation method is specifically as follows: diluting the starter in deionized water 10-15 times its own weight, and then inoculating in a spraying form.
9. The method for preparing normal temperature and low pressure biomass particles according to claim 6, characterized in that: The stacking fermentation method specifically includes: the mixture is stacked at a height of 2-2.5 m and undergoes a fermentation process of 3-5 days.
Citation Information
Patent Citations
Method for processing biological particles using lignin in paper-making waste liquid
CN101069977A
Biomass fuel particles with high bonding degree
CN106753663A
Preparation method of biomass particles
CN109321306A
Biomass granular fuel prepared by using waste
CN110699139A
Ecological solid fuel and process for preparing the same
KR102155762B1