External refining composite slag-conditioning deoxidizer and preparation method thereof
Through the composite slag-mixed deoxidant of the Al-Si-Ca ternary system, the harmlessly treated industrial waste aluminum ash is combined with silica, which solves the problem of difficult and high cost of aluminum deoxidant in the furnace refining in the outside furnace. , achieving high purity and stability of molten steel, reducing production costs and being safe and environmentally friendly.
Patent Information
- Application Number
- CN202410971937.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
The use of aluminum-containing deoxidants in the existing furnace refining is difficult to remove fine inclusions in the later stage of smelting, resulting in blockage of continuous casting water outlets, and the high cost of aluminum increases production costs, and industrial waste aluminum ash cannot be effectively utilized, resulting in waste of resources and Safety hazards.
Using the composite slag mixing and deoxidant of the Al-Si-Ca ternary system, the industrial waste aluminum ash is combined with silica after harmless treatment, and a composite slag mixing and deoxidant is prepared from the furnace, which is stearic acid As a bonding agent, it promotes molding and reduces ash and smoke, avoids problems caused by excessive aluminum or silicon.
Effectively utilize industrial waste aluminum ash, reduce enterprise costs, improve the purity and performance stability of molten steel, avoid the existence of oxygen and impurities, reduce the content of oxygen, hydrogen and nitrogen in molten steel, and enhance the purity and performance stability of molten steel.
Smart Images

Figure BDA0004953491370000051 
Figure BDA0004953491370000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of off-furnace refining of molten steel, and in particular to an off-furnace refining composite slag-adjusting and deoxidizing agent and a preparation method thereof. Background Art
[0002] Ladle Furnace (LF) refers to the metallurgical process of moving the molten steel that has been initially refined in a converter, open hearth or electric furnace to another container for refining. It is also called "ladle metallurgy" or "secondary metallurgy", which is to divide the traditional steelmaking process into two steps: primary refining and refining. During primary refining, the charge is melted, dephosphorized, desulfurized, impurities are removed and main alloying is performed in a furnace in an oxidizing atmosphere to obtain primary molten steel. Refining is to degas, deoxidize, desulfurize, remove inclusions and fine-tune the composition of the primary molten steel in a container in a vacuum, inert gas or reducing atmosphere. Implementation of LF can improve the quality of steel, shorten the smelting time, optimize the process and reduce production costs.
[0003] Deoxidizers are usually used in the refining process outside the furnace. Aluminum-containing deoxidizers are a very widely used deoxidizer in the prior art, such as aluminum wire, aluminum iron, aluminum alloy, etc. The advantage of using aluminum-containing deoxidation is that the grain size is finer and the performance is better, but its inclusion removal is relatively difficult, especially in the later stage of smelting. It is very difficult to remove the fine inclusions produced by aluminum deoxidation. During the casting process, Al2O3 inclusions accumulate on the nozzle wall, which can easily cause continuous casting nozzle blockage. At the same time, due to the high price of aluminum, the production cost is high. Summary of the invention
[0004] One of the purposes of the present invention is to provide a composite slag-adjusting and deoxidizing agent for off-furnace refining based on the above-mentioned problems. The composite slag-adjusting and deoxidizing agent is an Al-Si-Ca ternary system. On the one hand, it can simultaneously utilize the reducing properties of aluminum and silica and avoid the problems caused by excessive aluminum or silicon. On the other hand, the aluminum in the composite slag-adjusting and deoxidizing agent comes from aluminum ash from industrial waste, thereby achieving effective utilization of waste and reducing enterprise costs.
[0005] The second object of the present invention is to provide a method for preparing the above-mentioned composite slag-adjusting and deoxidizing agent for off-furnace refining.
[0006] The technical solution adopted by the present invention is as follows:
[0007] A composite slag-adjusting and deoxidizing agent for off-furnace refining, the raw materials of which include 70%-95% aluminum source, 1%-25% silica, and 2%-20% binder in terms of mass percentage; wherein the aluminum source is obtained from industrial waste aluminum ash after harmless treatment.
[0008] In a preferred embodiment of the present invention, the raw materials include, by mass percentage, 80%-90% aluminum source, 5%-15% silica, and 4%-10% binder.
[0009] Industrial waste aluminum ash mainly includes scum and skimming floating on the upper layer of aluminum liquid during the metallurgical melting process of electrolytic aluminum, cast aluminum, and recycled aluminum, as well as the residue remaining after subsequent treatment processes such as ash roasting and ball milling. Its composition is mainly metal aluminum and non-metallic oxides, of which aluminum oxide usually accounts for more than 60%, and other oxides include silicon oxide, magnesium oxide, sodium oxide, iron oxide, calcium oxide, aluminum nitride, etc. Usually, according to the production and processing flow of aluminum ash, the industry classifies aluminum ash into primary aluminum ash, secondary aluminum ash and residual ash. The aluminum ash just shoveled out of the aluminum melting furnace is usually called primary aluminum ash or aluminum slag. The aluminum content is as high as more than 60%, and it is basically in a high temperature state. It is usually directly transferred to the ash roasting machine to directly separate the metal aluminum contained in it, and it flows out from the bottom of the crucible of aluminum roasting to become an aluminum ingot. During the roasting process, a certain amount of flux is added to increase the temperature and promote the separation of aluminum liquid and aluminum ash. Most of the added flux is mainly fluoride with low melting point, which leads to further complexity of aluminum ash composition. The upper aluminum ash obtained in the roasting process is usually called "secondary aluminum ash". The particle size of secondary aluminum ash is usually around 200 mesh. Subsequently, the roasted aluminum ash enters the ball mill again, and the ductility of aluminum is used to deform the metal aluminum. Under the grinding action of the ball mill, inorganic substances such as alumina become finer and finer. Then the metal aluminum can be separated by screening. The fine powder under the sieve is the final residual ash. At present, the large-scale reuse of industrial waste aluminum ash is a very challenging issue, and there is no solution that can be widely promoted. If it is discarded at will, it will cause serious waste of resources. On the other hand, industrial waste aluminum ash has the following dangerous characteristics: (1) Reactivity: It may react violently with water or other substances to produce harmful gases or heat, which may cause dangerous events such as combustion and explosion in severe cases. (2) Corrosiveness: It may cause corrosion damage to the contacting materials. Failure to do so may result in serious consequences.
[0010] In the present invention, industrial waste aluminum ash is harmlessly treated and then prepared into a composite slag-adjusting deoxidizer for off-furnace refining, which provides a new idea for the reuse of industrial waste aluminum ash. It is combined with silica to prepare the composite slag-adjusting deoxidizer for off-furnace refining, which can promote the effective utilization of resources and reduce enterprise costs on the one hand, and on the other hand, can simultaneously utilize the deoxidation effects of aluminum and silica, avoid the problems caused by excessive aluminum or silicon in off-furnace refining, effectively remove oxygen and impurities in molten steel, and improve the purity and performance stability of molten steel.
[0011] In a preferred embodiment of the present invention, the binder is selected from stearic acid, cellulose, starch, and dextrin, among which stearic acid is preferred.
[0012] The binder in the present invention bonds the aluminum source and silica, promotes the molding of the final composite slag-adjusting deoxidizer product, and the molded product is easy to transport. When transported to the refining furnace outside the LF furnace, it is not easy to generate dust and smoke, which is environmentally friendly. The amount of the binder has a great influence on the product. If the amount of the binder is too little, the binding effect cannot be fully exerted, the molding of the product is affected, and the problems of looseness and cracking are prone to occur. If the amount of the binder is too much, the product may be too greasy, affecting its performance and appearance, and even affecting the properties of molten steel.
[0013] In a preferred embodiment of the present invention, the aluminum source is prepared from industrial waste aluminum ash by the following harmless treatment method:
[0014] (1) Mixing industrial waste aluminum ash with calcium hydroxide and adding the mixture into an aluminum ash processing machine;
[0015] (2) adding water to the aluminum ash treatment machine, mixing and discharging the generated steam; heating the reaction and stopping the discharging of steam;
[0016] (3) Add water for a second time, discharge steam at the same time, heat to carry out a secondary reaction, stop discharging steam after the reaction, discharge the gas generated by the reaction, and collect the solid material.
[0017] In a preferred embodiment of the present invention, in step (1), the mass ratio of industrial waste aluminum ash to calcium hydroxide is 100:0.1-5; and the particle size of calcium hydroxide does not exceed 10 mm.
[0018] In a preferred embodiment of the present invention, in step (2), when water is added, the liquid-to-solid ratio is 0.5-1.5:1; the reaction is heated to 50°C-100°C and the reaction is carried out for 1-30 minutes until the reaction becomes stable.
[0019] In a preferred embodiment of the present invention, in step (3), when water is added for the second time, the liquid-to-solid ratio is 0.5-1.5:1; the secondary reaction is carried out at 50-100°C, and the secondary reaction lasts for 0.5-10h until the reaction is complete; the exhausted gas is treated and discharged after meeting the standards.
[0020] The harmless treatment method provided by the present invention is particularly suitable for the treatment of secondary aluminum ash.
[0021] In a preferred embodiment of the present invention, the nitrogen content in the aluminum source does not exceed 6 wt %, and the fluorine leaching amount does not exceed 100 mg / mL.
[0022] A method for preparing a composite slag-adjusting and deoxidizing agent for off-furnace refining comprises the following steps:
[0023] (1) Mixing and heating: taking the aluminum source and silica in the formula amount, mixing them, adding them into a mixing mill, and stirring and mixing them under heating conditions;
[0024] (2) Adding a binder: Add the binder to the mixer and continue to stir and mix at a constant temperature;
[0025] (3) Ball pressing: The stirred and heated material is transferred to a double-roll ball press, and the stirring is continued. After cooling, the material is pressed into balls of 3-5 mm.
[0026] In a preferred embodiment of the present invention, in step (1), the temperature is heated to 100°C-150°C, the stirring speed is 30-60rpm, and the mixing time is 30-60min; in step (3), the pressure of the ball press is 1000-1500KN and the rotation speed is 10-20r / min.
[0027] The beneficial effects of the present invention are:
[0028] The present invention provides a composite slag-adjusting deoxidizer for off-furnace refining, which is prepared from harmlessly treated industrial waste aluminum ash and silica. On the one hand, it provides a new idea for the reuse of industrial waste aluminum ash, promotes the effective utilization of resources, and reduces enterprise costs. On the other hand, the composite slag-adjusting deoxidizer for off-furnace refining is an Al-Si-Ca ternary system, which simultaneously utilizes the deoxidation effect of aluminum and silica, and avoids the problems caused by excessive aluminum or silicon in off-furnace refining, effectively removes oxygen and impurities in molten steel, and improves the purity and performance stability of molten steel. DETAILED DESCRIPTION
[0029] All features disclosed in this specification, or steps in all methods or processes disclosed, except mutually exclusive features and / or steps, can be combined in any manner.
[0030] Any feature disclosed in this specification (including any additional claims and abstract), unless otherwise stated, may be replaced by other equivalent or alternative features having similar purposes. That is, unless otherwise stated, each feature is only an example of a series of equivalent or similar features. Specific embodiments
[0032] Preparation Example 1
[0033] This preparation example provides a method for harmless treatment of industrial waste aluminum ash, comprising the following steps:
[0034] (1) Take 3.5 tons of waste aluminum ash and 0.035 tons of calcium hydroxide powder produced by smelting, add them into a mixer, stir and mix them evenly, and then transfer them into an aluminum ash processor.
[0035] (2) Add 2.05 tons of water to the aluminum ash processing machine, open the steam valve, heat to 50°C, the material begins to react violently, then close the steam valve, react for 10 minutes, and the reaction becomes gentle.
[0036] (3) Open the steam valve, add 2 tons of water, and continue the reaction for 2.5 hours after the temperature rises to 70°C. Close the steam valve, open the exhaust valve to discharge the generated gas, open the discharge valve, and collect the solid material to obtain harmless aluminum ash. After testing, the water content of the obtained harmless aluminum ash is about 10%.
[0037] (4) The exhaust gas is dedusted by a dust collector, cooled by a cooler, absorbed by a two-stage sulfuric acid tower as a by-product of ammonium sulfate, and then sprayed with two stages of alkaline water and one stage of clean water before it meets the emission standards.
[0038] Preparation Example 2
[0039] This preparation example provides a method for harmless treatment of industrial waste aluminum ash, comprising the following steps:
[0040] (1) Take 3.8 tons of waste aluminum ash and 0.05 tons of calcium hydroxide powder produced by smelting, add them into a mixer, stir and mix them evenly, and then transfer them into an aluminum ash processor.
[0041] (2) Add 3 tons of water to the aluminum ash processing machine, open the steam valve, heat to 70°C, the material begins to react violently, then close the steam valve and react for 15 minutes, the reaction tends to be gentle.
[0042] (3) Open the steam valve, add 2.5 tons of water, and continue the reaction for 5 hours after the temperature rises to 80°C. Close the steam valve, open the exhaust valve to discharge the generated gas, open the discharge valve, collect the solid material, and obtain harmless aluminum ash. After testing, the water content of the obtained harmless aluminum ash is about 8%.
[0043] (4) The exhaust gas is dedusted by a dust collector, cooled by a cooler, absorbed by a two-stage sulfuric acid tower as a by-product of ammonium sulfate, and then sprayed with two stages of alkaline water and one stage of clean water before it meets the emission standards.
[0044] The test data of the materials in Preparation Example 1 and Preparation Example 2 are shown in Table 1.
[0045] Table 1 Material test data in preparation example
[0046]
[0047] It can be seen from the data in Table 1 that after the smelting waste aluminum ash is treated by the harmless treatment method provided by the present invention, the nitrogen content and fluorine leaching amount are significantly reduced. Combined with the "GB5085 Hazardous Waste Identification Standard" and YB / T4703-2018, it removes its hazardous characteristics and greatly reduces the possibility of dangerous incidents during the secondary utilization process.
[0048] Example 1
[0049] This embodiment provides a composite slag-adjusting and deoxidizing agent for off-furnace refining, which is composed of the following raw materials: 85 kg of aluminum source, 10 kg of silica, and 5 kg of stearic acid. Among them, the aluminum source is the harmless aluminum ash prepared in Preparation Example 1.
[0050] The composite slag-adjusting deoxidizer for off-furnace refining provided in this embodiment is prepared by the following method:
[0051] (1) Mixing and heating: Take the formulated amount of aluminum source (i.e. harmless aluminum ash) and silica, mix them and add them to a mixing mill. Stir and mix at a speed of 40 rpm while heating, and heat to 150°C within 60 minutes.
[0052] (2) Adding a binder: Add stearic acid to the mixer and continue to stir and mix while maintaining the temperature until the stearic acid is completely melted and the materials are stirred evenly.
[0053] (3) Ball pressing: The stirred and heated material is transferred to a double-roll ball press, stirred at a speed of 15 rpm, cooled to room temperature, and pressed into 3-5 mm balls at a pressure of 1200 KN.
[0054] Example 2
[0055] This embodiment provides a composite slag-adjusting and deoxidizing agent for off-furnace refining, which is composed of the following raw materials: 75 kg of aluminum source, 22 kg of silica, and 3 kg of stearic acid. Among them, the aluminum source is the harmless aluminum ash prepared in Preparation Example 1.
[0056] The preparation method of the composite slag-adjusting and deoxidizing agent for off-furnace refining provided in this embodiment is the same as that in Example 1.
[0057] Example 3
[0058] This embodiment provides a composite slag-adjusting and deoxidizing agent for off-furnace refining, which is composed of the following raw materials: 82 kg of aluminum source, 11 kg of silica, and 7 kg of stearic acid. Among them, the aluminum source is the harmless aluminum ash prepared in Preparation Example 2.
[0059] The composite slag-adjusting deoxidizer for off-furnace refining provided in this embodiment is prepared by the following method:
[0060] (1) Mixing and heating: Take the formulated amount of aluminum source (i.e. harmless aluminum ash) and silica, mix them and add them to a mixing mill. Stir and mix at a speed of 60 rpm while heating, and heat to 120° C. within 40 minutes.
[0061] (2) Adding a binder: Add stearic acid to the mixer and continue to stir and mix while maintaining the temperature until the stearic acid is completely melted and the materials are stirred evenly.
[0062] (3) Ball pressing: The stirred and heated material is transferred to a double-roll ball press, stirred at a speed of 20 rpm, cooled to room temperature, and pressed into 3-5 mm balls at a pressure of 1500 KN.
[0063] Example 4
[0064] This embodiment provides a composite slag-adjusting and deoxidizing agent for off-furnace refining, which is composed of the following raw materials: 90 kg of aluminum source, 6 kg of silica, and 4 kg of stearic acid. Among them, the aluminum source is the harmless aluminum ash prepared in Preparation Example 1.
[0065] The preparation method of the composite slag-adjusting and deoxidizing agent for off-furnace refining provided in this embodiment is the same as that in Example 1.
[0066] Example 5
[0067] This embodiment provides a composite slag-adjusting and deoxidizing agent for off-furnace refining, which is composed of the following raw materials: 84 kg of aluminum source, 6 kg of silica, and 10 kg of stearic acid. Among them, the aluminum source is the harmless aluminum ash prepared in Preparation Example 1.
[0068] The preparation method of the composite slag-adjusting and deoxidizing agent for off-furnace refining provided in this embodiment is the same as that in Example 3.
[0069] Example 6
[0070] This embodiment provides a composite slag-adjusting and deoxidizing agent for off-furnace refining, which is composed of the following raw materials: 85 kg of aluminum source, 10 kg of silica, and 5 kg of dextrin. Among them, the aluminum source is the harmless aluminum ash prepared in Preparation Example 1.
[0071] The preparation method of the composite slag-adjusting and deoxidizing agent for off-furnace refining provided in this embodiment is the same as that in Example 1.
[0072] Example 7
[0073] This embodiment provides a composite slag-adjusting and deoxidizing agent for off-furnace refining, which is composed of the following raw materials: 85 kg of aluminum source, 10 kg of silica, and 5 kg of cellulose. Among them, the aluminum source is the harmless aluminum ash prepared in Preparation Example 1.
[0074] The preparation method of the composite slag-adjusting and deoxidizing agent for off-furnace refining provided in this embodiment is the same as that in Example 1.
[0075] Example 8
[0076] This embodiment provides a composite slag-adjusting and deoxidizing agent for off-furnace refining, which is composed of the following raw materials: 94 kg of aluminum source, 4 kg of silica, and 2 kg of stearic acid. Among them, the aluminum source is the harmless aluminum ash prepared in Preparation Example 1.
[0077] The preparation method of the composite slag-adjusting and deoxidizing agent for off-furnace refining provided in this embodiment is the same as that in Example 1.
[0078] Comparative Example 1
[0079] This comparative example provides an off-furnace refining composite slag-adjusting deoxidizer, which is composed of the following raw materials: 60 kg of aluminum source, 18 kg of silica, and 22 kg of stearic acid. Among them, the aluminum source is the harmless aluminum ash prepared in Preparation Example 1.
[0080] The preparation method of the composite slag-adjusting and deoxidizing agent for off-furnace refining provided in this embodiment is the same as that in Example 1.
[0081] Comparative Example 2
[0082] This comparative example provides an off-furnace refining composite slag-adjusting deoxidizer, which is composed of the following raw materials: 90 kg of aluminum source, 9 kg of silica, and 1 kg of stearic acid. Among them, the aluminum source is the harmless aluminum ash prepared in Preparation Example 1.
[0083] The preparation method of the composite slag-adjusting and deoxidizing agent for off-furnace refining provided in this embodiment is the same as that in embodiment 1. During the preparation process, it was found that some spherical particles were loose and cracked. After analysis, it was found that this was caused by too little stearic acid in the formula.
[0084] Test example
[0085] The composite slag-adjusting deoxidizers prepared in Examples 1-8 and Comparative Example 1 were used in the off-furnace refining process of low-carbon molten steel, and the contents of oxygen, hydrogen and nitrogen in the molten steel were compared before and after the addition of the composite slag-adjusting deoxidizer. The amount of the composite slag-adjusting deoxidizer used per ton of molten steel was 1.2 kg. After testing, before the addition of the deoxidizer, the contents of oxygen, hydrogen and nitrogen in the molten steel (in mass percentage) were 0.216%, 0.0278% and 0.0223% respectively. After the addition of different composite slag-adjusting deoxidizers, the contents of carbon, oxygen, hydrogen and nitrogen in the molten steel are shown in Table 2.
[0086] Table 2 Test data of molten steel treated with different composite slag deoxidizers
[0087]
[0088] It can be seen from the data in Table 2 that after using the composite slag-adjusting deoxidizer of Examples 1-8 of the present invention, the contents of oxygen, hydrogen and nitrogen in the molten steel are all reduced. Compared with Examples 1 and 3-5, the contents of oxygen, hydrogen and nitrogen in the molten steel treated with the composite slag-adjusting deoxidizer in Examples 2 and 6-8 are higher. The contents of oxygen, hydrogen and nitrogen in the molten steel treated with the composite slag-adjusting deoxidizer in Comparative Example 1 are significantly higher than those in the molten steel treated with the composite slag-adjusting deoxidizer in Examples 1-8. It can be seen that the composition and content of the composite slag-adjusting deoxidizer have an impact on the treatment effect of the molten steel.
[0089] Therefore, the present invention is not limited to the above-mentioned specific embodiments. The present invention extends to any new features or any new combination disclosed in this specification, and any new method or process steps or any new combination disclosed.
Claims
1. A composite slag-adjusting and deoxidizing agent for off-furnace refining, characterized in that: The raw materials include 70%-95% aluminum source, 1%-25% silica and 2%-20% binder in terms of mass percentage; wherein the aluminum source is obtained from industrial waste aluminum ash after harmless treatment.
2. The composite slag-adjusting and deoxidizing agent for off-furnace refining according to claim 1, characterized in that: The raw materials include, by mass percentage, 80%-90% of aluminum source, 5%-15% of silica, and 4%-10% of binder.
3. The composite slag-adjusting and deoxidizing agent for off-furnace refining according to claim 1 or 2, characterized in that: The binder is selected from stearic acid, cellulose, starch, and dextrin, wherein stearic acid is preferred.
4. The composite slag-adjusting and deoxidizing agent for off-furnace refining according to claim 3, characterized in that: The aluminum source is prepared from industrial waste aluminum ash by the following harmless treatment method: (1) Mixing industrial waste aluminum ash with calcium hydroxide and adding the mixture into an aluminum ash processing machine; (2) Add water to the aluminum ash treatment machine, mix and discharge the generated steam at the same time; heat to react and stop discharging the steam; (3) Add water for a second time and discharge the steam at the same time, heat to carry out a secondary reaction, stop discharging the steam after the reaction, and discharge the gas generated by the reaction; collect the solid discharge to obtain.
5. The composite slag-adjusting and deoxidizing agent for off-furnace refining according to claim 4, characterized in that: In step (1), the mass ratio of industrial waste aluminum ash to calcium hydroxide is 100:0.1-5; and the particle size of calcium hydroxide does not exceed 10 mm.
6. The composite slag-adjusting and deoxidizing agent for off-furnace refining according to claim 4, characterized in that: In step (2), when water is added, the liquid-to-solid ratio is 0.5-1.5:1; the mixture is heated to 50°C-100°C for reaction, and the reaction is carried out for 1-30 minutes until the reaction becomes stable.
7. The composite slag-adjusting and deoxidizing agent for off-furnace refining according to claim 4, characterized in that: In step (3), when water is added for the second time, the liquid-to-solid ratio is 0.5-1.5:1; the mixture is heated to 50-100°C for a secondary reaction, and the secondary reaction lasts for 0.5-10 hours until the reaction is complete; and the exhausted gas is treated and discharged after meeting the standards.
8. The composite slag-adjusting and deoxidizing agent for off-furnace refining according to any one of claims 4 to 7, characterized in that: In the aluminum source, the nitrogen content does not exceed 6wt%, and the fluorine leaching amount does not exceed 100mg / mL.
9. A method for preparing a composite slag-adjusting and deoxidizing agent for off-furnace refining, characterized in that: It includes the following steps: (1) Mixing and heating: taking the aluminum source and silica in the formula amount, mixing them, adding them into a mixing mill, and stirring and mixing them under heating conditions; (2) Adding a binder: Add the binder to the mixer and continue to stir and mix at a constant temperature; (3) Ball pressing: The stirred and heated material is transferred to a double-roll ball press, and the stirring is continued. After cooling, the material is pressed into balls of 3-5 mm.
10. The preparation method according to claim 9, characterized in that: In step (1), the temperature is heated to 100°C-150°C, the stirring speed is 30-60rpm, and the mixing time is 30-60min; in step (3), the pressure of the ball press is 1000-1500KN and the rotation speed is 10-20r / min.