Regulation and control method for metastable austenitic stainless steel deformation-induced phase change product and application of regulation and control method
By constructing a mathematical model to regulate the deformation-induced phase transition products of metastable austenite stainless steel, the problem of deformation-induced martensite content control in the existing technology is solved, material strength and toughness improvement and delay crack prevention are achieved, and forming process parameters are optimized.
Patent Information
- Application Number
- CN202410943516.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is difficult to accurately control the deformation-induced martensite content in metastable austenitic stainless steel, resulting in uneven distribution of deformation-induced phases during stamping and bending deformation, causing delayed cracking problems.
By constructing a mathematical model of volume fractions and deformation parameters of phase change product in metastable austenitic stainless steel, as well as a mathematical model of the proportion of volume fractions of phase change product in heating process to initial volume fractions and heating parameters, cylinder uniaxial compression is used Experiment and heating experiments regulate the generation and distribution of deformation-induced phase change products.
Accurate control of the deformation-induced phase change products of metastable austenitic stainless steel, improve the strength and toughness of the material and prevent delayed cracking, optimize the forming process parameters, and avoid the formation and delayed cracking of uneven phase change products during bending. .
Smart Images

Figure CN118910395A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal material processing engineering, and more specifically, relates to a control method for deformation-induced phase transformation products of metastable austenitic stainless steel and an application thereof. Background Art
[0002] With the rapid economic development of my country, Cr-Ni and Cr-Mn metastable austenitic stainless steel sheets and strips are widely used in the fields of automobiles and home appliances, mainly in the rolling, bending and deep drawing processes of the sheets and strips. Metastable austenitic stainless steel has corrosion resistance and deformation-induced phase transformation characteristics. The uniform and appropriate amount of deformation-induced martensite not only improves the strength of the material, but also improves the toughness of the material. Therefore, its hot-rolled annealed sheet can obtain the best combination of high strength, toughness and corrosion resistance after cold rolling deformation with a small reduction rate. It belongs to the green low-carbon steel grade, and its stamping and bending workpieces are widely used in lightweight automobiles, modern vegetable greenhouses and other fields. However, during the stamping and bending deformation process of this small deformation cold-rolled steel sheet, the further bending deformation brings about the uneven distribution of the deformation-induced martensite phase, which in turn causes the problem of delayed cracking.
[0003] After searching, the Chinese patent application document with the number of 201780005708.8 and the application publication date of January 17, 2017 disclosed the warm rolling of steel containing metastable austenite. The patent publicly records that controlling the cold rolling temperature can control the amount of deformation-induced martensite. The patent only mentions that when the steel is at a temperature greater than 80°F and not exceeding 250°F, the amount of martensite formed decreases with increasing temperature. However, how to accurately control the content of martensite requires further research.
[0004] Metastable austenitic stainless steel has deformation-induced phase transformation characteristics. Reasonable regulation of its deformation-induced phase transformation products is conducive to obtaining better strength and toughness of products and preventing delayed cracking of products. Therefore, it is very important to reasonably regulate the deformation parameters during the deformation process and the heating parameters during the heating process. Summary of the invention
[0005] 1. Problem to be solved
[0006] Aiming at the deformation-induced phase transformation characteristics of metastable austenitic stainless steel and its special influence on material properties (such as toughness, delayed cracking, etc.), the present invention provides a control method for the deformation-induced phase transformation products of metastable austenitic stainless steel based on a mathematical model. Through the uniaxial compression test of the cylinder and its heating test, a mathematical model of the volume fraction of the phase transformation products in the deformation process and the deformation parameters, as well as a mathematical model of the ratio of the volume fraction of the phase transformation products in the heating process to the initial volume fraction and the heating parameters are constructed, so as to achieve a method for regulating the deformation-induced phase transformation products. And then it can be applied in the forming process of metastable austenitic stainless steel products.
[0007] 2. Technical solution
[0008] In order to solve the above problems, the technical solution adopted by the present invention is as follows:
[0009] The method for regulating the deformation induced phase transformation products of metastable austenitic stainless steel of the present invention refers to a method for regulating the deformation induced phase transformation products of metastable austenitic stainless steel with deformation induced phase transformation characteristics by constructing a mathematical model of the volume fraction of the phase transformation products in its deformation process and the deformation parameters, and constructing a mathematical model of the ratio of the volume fraction of the phase transformation products in its heating process to the initial volume fraction and the heating parameters.
[0010] A method for regulating deformation-induced phase transformation products of metastable austenitic stainless steel, comprising the following steps:
[0011] S1. Compression deformation process
[0012] Take metastable austenitic stainless steel at different deformation temperatures T d , different equivalent strain rates Different equivalent strain ε d Compression tests were carried out under the condition of , and multiple groups of compression deformation specimens were obtained; the volume fraction F of the deformation-induced phase change product in each compression deformation specimen was measured V , construct F V With T d , ε d Mathematical model of time:
[0013] S2. Heating and insulation process
[0014] For the compression deformation sample obtained in step S1, at different heating temperatures T s The heating and heat preservation process is carried out at different heat preservation times t to obtain multiple groups of heating and heat preservation samples; the volume fraction F of the residual product of deformation induced phase change in each heating and heat preservation sample is measured Vr , calculate F Vr Account for F V Percentage ξ, construct ξ and T s Mathematical model between ξ and t: ξ=f(T s ,t).
[0015] Furthermore, the volume fraction of deformation-induced phase change products (F V ) and deformation temperature (T d / ℃)、Equivalent strain (ε d ), equivalent strain rate The mathematical model between is shown in formula (1), which is completed by using the cylindrical uniaxial compression test of the solution treated cylindrical specimen at different deformation temperatures, equivalent strains, and equivalent strain rates:
[0016]
[0017] In the formula, a1~a 13 are all constants. The unknown coefficients a1~a are determined by fitting equation (1) according to the volume fraction of deformation-induced phase change products obtained at different deformation temperatures, equivalent strains and equivalent strain rates. 13 , a mathematical model between the volume fraction of deformation-induced phase transformation products of a specific metastable austenitic stainless steel and the deformation temperature, equivalent strain, and equivalent strain rate was obtained.
[0018] Furthermore, the ratio of the residual volume fraction of the deformation-induced phase change product to the initial volume fraction during the heating process (ξ) is related to the heating temperature (T s ) and the holding time (t) are shown in formula (2). This model is completed by means of isothermal heating experiments of cylindrical uniaxial isothermal compression specimens at different heating temperatures and holding times:
[0019]
[0020] In the formula, b1~b7 are all constants. According to the ratio of the residual volume fraction in the heating process to the initial volume fraction obtained at different heating temperatures and holding times, the unknown coefficients b1~b7 are determined by fitting formula (2), and the mathematical model between the ratio of the residual volume fraction of the deformation induced phase transformation product of a specific metastable austenitic stainless steel in the heating process to the initial volume fraction and the heating temperature and holding time is obtained.
[0021] Furthermore, the residual volume fraction (F Vr ) can be calculated by equation (1) and (2) and by equation (3).
[0022]
[0023] Furthermore, the metastable austenitic stainless steel is a Cr-Ni series (such as 300 series) or Cr-Mn series (such as 200 series) metastable austenitic stainless steel, which will undergo deformation-induced phase transformation behavior under certain deformation conditions, and the phase transformation product is ε martensite or α′ martensite.
[0024] Furthermore, the deformation temperature T d 25~150℃, equivalent strain rate 0.1~10.0s -1 , equivalent strain ε d 0.2~0.6; Heating temperature T s The temperature is 75-125℃, and the insulation time t is 0-15s.
[0025] Furthermore, the volume fraction of deformation-induced phase change products FV and the volume fraction of the residual product induced by deformation transformation F Vr All of them are obtained by XRD detection or ferrite instrument detection. When the phase transformation product is mainly α′ martensite, the volume fraction F of the deformation-induced phase transformation product is detected by ferrite instrument. V and the volume fraction of the residual product induced by deformation transformation F Vr .
[0026] A metastable austenitic stainless steel product, wherein the forming process of the metastable austenitic stainless steel product is cold rolling, warm rolling, bending or stamping, and the above-mentioned control method is used to obtain the parameters in the corresponding compression deformation process and the parameters in the heating and insulation process, wherein the forming process parameters are composed of the parameters in the compression deformation process and the parameters in the heating and insulation process.
[0027] Furthermore, we construct F through formula (1) V = 0, determine the critical deformation temperature under a specific equivalent strain and equivalent strain rate, or determine the critical equivalent strain under a specific deformation temperature and equivalent strain rate;
[0028] For a specific equivalent strain and equivalent strain rate, when the deformation temperature is higher than the critical deformation temperature, or for a specific deformation temperature and equivalent strain rate, when the equivalent strain of deformation is less than the critical equivalent strain, deformation induced phase transformation products will not be generated under the corresponding deformation conditions.
[0029] Furthermore, the critical surface when ξ=0 is constructed by formula (2) to determine the critical heating temperature under a specific holding time condition, or to determine the critical holding time under a specific heating temperature;
[0030] For a specific holding time, when the heating temperature is greater than the critical heating temperature, or for a specific heating temperature, when the holding time is greater than the critical holding time, under the corresponding heating conditions, the deformation induced martensite phase is completely dissolved.
[0031] Furthermore, equations (1), (2), and (3) can be used to calculate the volume fraction of deformation-induced phase change products under specific deformation conditions, and can also be used to calculate the residual volume fraction of existing deformation-induced phase change products under specific heating conditions.
[0032] Furthermore, the constructed mathematical model equations (1), (2), (3) and their critical values can be used to control the process parameters of cold rolling, warm rolling, bending, stamping and other forming processes of metastable austenitic stainless steel plates.
[0033] 3. Beneficial effects
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] Aiming at the deformation-induced phase transformation characteristics of Cr-Ni or Cr-Mn metastable austenitic stainless steels and their special influence on the toughness and delayed cracking of the materials, the present invention adopts a cylindrical uniaxial compression test and a heating test to obtain the volume fraction of deformation-induced phase transformation products at different deformation temperatures, equivalent strains and equivalent strain rates, and the residual volume fraction during the heating process, constructs a mathematical model of the volume fraction of the phase transformation products during the deformation process and the deformation parameters, and constructs a mathematical model of the ratio of the volume fraction of the phase transformation products during the heating process to the initial volume fraction and the heating parameters, so as to achieve a method for regulating the deformation-induced phase transformation products. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 is the critical surface when ξ=0, t=200s;
[0037] Figure 2 is the critical surface when ξ=0, t=300s;
[0038] Figure 3 is the critical surface when ξ=0, t=400s;
[0039] Figure 4 The bent parts are 2.8mm thick cold-rolled steel plates with a reduction rate of 10% and bent at room temperature (Figure a, cracks appear when bent to 120°) and bent parts with warm bending at 100°C (Figure b, cracks appear when bent to 180°). DETAILED DESCRIPTION
[0040] The present invention is further described below in conjunction with specific embodiments.
[0041] The present invention provides a method for regulating deformation induced phase transformation products of metastable austenitic stainless steel. The method aims at the deformation induced phase transformation characteristics of metastable austenitic stainless steel and its special influence on microstructure and performance, and proposes a method for controlling the volume fraction of deformation induced phase transformation products in a specific forming process by constructing a mathematical model.
[0042] Specifically, taking Cr-Mn metastable austenitic stainless steel 201Cu as an example, a cylindrical specimen of φ5mm×10mm was used at a deformation temperature (T d ) range, 0.1~10.0s -1 The equivalent strain rate Range, equivalent strain (ε d) range, complete the equiaxial compression test to obtain compression specimens at different deformation temperatures, true strains, and strain rates, and cut 1mm thick thin slice specimens on the longitudinal section of the specimens. The volume fraction of the α′ phase in the thin slice specimens was tested using a ferrite instrument, and the volume fraction of the deformation-induced α′ phase at different deformation temperatures, true strains, and strain rates shown in Table 1 was obtained, and the deformation-induced phase transformation model of 201Cu steel was fitted as shown in formula (4).
[0043]
[0044] The above cylindrical sample was tested at 25℃ and 1.0s. -1 Complete the compression deformation of 0.2 strain at 25℃ and 5.0s -1 Complete the compression deformation of 0.4 strain (Note: According to the experimental equipment capacity and the actual bending speed of 0.01 ~ 5.0s -1 Two different compression speeds were selected within the strain rate range), and then the samples were kept at 75, 100, 125, and 150 °C for 5, 10, and 15 seconds, respectively, to obtain cylindrical uniaxial specimens compressed and heated under different processes. A 1 mm thick thin slice was cut from the longitudinal section of the sample, and the volume fraction of the α′ phase in the thin slice was tested using a ferrite instrument to obtain the residual volume fraction (F) of the deformation-induced α′ phase at different holding temperatures and holding times as shown in Table 2. Vr ), and its percentage of the initial volume fraction (ξ), and the inverse phase transformation model of the deformation-induced phase transformation of 201Cu steel during the heating process is fitted as shown in formula (5).
[0045]
[0046] Construct F through formula (4) V = 0, and the critical surfaces when ξ = 0 and the holding time (t) are 200, 300, and 400 s respectively are constructed by equation (5). The above surfaces are coupled as follows: Figures 1 to 3 As shown. Figures 1 to 3 The cold rolling and warm strip bending process of 201Cu can be determined, that is, the specific reduction coefficient (h / h0) corresponding to the small reduction rate cold rolling process, which is related to the equivalent strain ε d Calculated according to formula (6)), rolling speed (v r , which is related to the strain rate Calculated according to formula (7), the temperature for warm bending is selected between the two surfaces (T s) and the corresponding holding time (t), which ensures that the deformation toughening (the result of deformation-induced phase transformation) effect obtained by cold rolling with a small reduction rate (such as 5-10%) will not disappear (that is, the deformation-induced phase transformation products are partially retained), and can also avoid the formation of uneven phase transformation products caused by deformation-induced phase transformation during the bending process, which leads to delayed cracking of stamped or bent parts in the bending forming part. A 2.8mm thick cold-rolled sheet was obtained by cold rolling a 3.3mm thick solid solution hot-rolled plate at a reduction rate of 15%. A 30mm wide and 200mm long bending specimen was processed in the transverse direction perpendicular to the rolling direction. A 3.0mm diameter indenter was further used for a cold bending test. The specimen cracked when bent to 120° (such as Figure 4 a); according to Figures 1 to 3 The bending specimen was placed in a water bath, kept at 100°C for 300s, and then subjected to warm bending in a water bath. The specimen was bent to 180° without cracking (e.g. Figure 4 b). This shows that the application of the above model in the specific bending process is effective.
[0047]
[0048] Where α is the bite angle during the strip rolling process; h / h0 is the reduction coefficient, that is, the ratio of the thickness after rolling to the thickness before rolling; v r is the rolling speed.
[0049] Table 1
[0050]
[0051] Table 2
[0052]
[0053] The above-mentioned embodiments have elaborated on the purpose and implementation effects of the present invention in detail. It should be understood that the above-mentioned embodiments are only descriptions of the preferred embodiments of the present invention, and do not limit the concept and scope of the present invention. All modifications, equivalent substitutions, improvements, etc. made by engineers and technicians in this field or using the technical concept and technical solutions of the present invention within the spirit and principles of the present invention and without departing from the design concept of the present invention are within the protection scope of the present invention.
Claims
1. A method for regulating deformation-induced phase transformation products of metastable austenitic stainless steel, characterized in that: The steps are: S1. Compression deformation process Take metastable austenitic stainless steel at different deformation temperatures T d , different equivalent strain rates Different equivalent strain ε d Compression tests were carried out under the condition of , and multiple groups of compression deformation specimens were obtained; the volume fraction F of the deformation-induced phase change product in each compression deformation specimen was measured V , construct F V With T d , ε d Mathematical model of time: S2. Heating and heat preservation process For the compression deformation sample obtained in step S1, at different heating temperatures T s The heating and heat preservation process is carried out at different heat preservation times t to obtain multiple groups of heating and heat preservation samples; the volume fraction F of the residual product of deformation induced phase change in each heating and heat preservation sample is measured Vr , calculate F Vr Account for F V Percentage ξ, construct ξ and T s Mathematical model between ξ and t: s ,t).
2. The method for controlling the deformation-induced phase transformation products of metastable austenitic stainless steel according to claim 1, characterized in that: F V With T d , ε d The mathematical model between is as follows: In the formula, a1~a 13 are all constants.
3. The method for controlling the deformation-induced phase transformation products of metastable austenitic stainless steel according to claim 1, characterized in that: ξ and T s The mathematical model between t and t is as follows: Wherein, b1~b7 are all constants.
4. The method for controlling the deformation-induced phase transformation products of metastable austenitic stainless steel according to any one of claims 1 to 3, characterized in that: Metastable austenitic stainless steel is Cr-Ni or Cr-Mn metastable austenitic stainless steel.
5. The method for controlling the deformation-induced phase transformation products of metastable austenitic stainless steel according to any one of claims 1 to 3, characterized in that: Deformation temperature T d 25~150℃, equivalent strain rate 0.1~10.0s -1 , equivalent strain ε d 0.2~0.6; Heating temperature T s The temperature is 75-125℃, and the insulation time t is 0-15s.
6. The method for controlling the deformation-induced phase transformation products of metastable austenitic stainless steel according to any one of claims 1 to 3, characterized in that: The deformation-induced phase transformation product is ε martensite or α′ martensite.
7. The method for controlling the deformation-induced phase transformation products of metastable austenitic stainless steel according to claim 6, characterized in that: Volume fraction of deformation-induced phase change products F V and the volume fraction of the residual product induced by deformation transformation F Vr All of them are obtained by XRD detection or ferrite instrument detection. When the phase transformation product is mainly α′ martensite, the volume fraction F of the deformation-induced phase transformation product is detected by ferrite instrument. V and the volume fraction of the residual product induced by deformation transformation F Vr .
8. Metastable austenitic stainless steel products, characterized in that: The metastable austenitic stainless steel product is formed by cold rolling, warm rolling, bending or stamping, and the control method described in any one of claims 1 to 7 is used to obtain the parameters in the corresponding compression deformation process and the parameters in the heating and insulation process, wherein the forming process parameters are composed of the parameters in the compression deformation process and the parameters in the heating and insulation process.
9. The metastable austenitic stainless steel product according to claim 8, characterized in that: Construct F by formula (1) V = 0, determine the critical deformation temperature under a specific equivalent strain and equivalent strain rate, or determine the critical equivalent strain under a specific deformation temperature and equivalent strain rate; For a specific equivalent strain and equivalent strain rate, when the deformation temperature is higher than the critical deformation temperature, or for a specific deformation temperature and equivalent strain rate, when the equivalent strain of deformation is less than the critical equivalent strain, deformation induced phase transformation products will not be generated under the corresponding deformation conditions.
10. The metastable austenitic stainless steel product according to claim 8, characterized in that: The critical surface when ξ=0 is constructed by formula (2) to determine the critical heating temperature under a specific holding time condition, or to determine the critical holding time under a specific heating temperature; For a specific holding time, when the heating temperature is greater than the critical heating temperature, or for a specific heating temperature, when the holding time is greater than the critical holding time, under the corresponding heating conditions, the deformation induced martensite phase is completely dissolved.