Method for green extraction and recovery of platinum group metals from solid wastes and low-grade ores
Through the coupling technology of direct bio-leaching of sulfide and indirect bio-leaching of oxides, combined with multi-process processing, the problem of difficulty in extracting platinum group metals in metal-based solid waste and low-grade ores is solved, and the efficient and low-carbon platinum group is achieved Metal recycling.
Patent Information
- Application Number
- CN202411124994.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-16
AI Technical Summary
The prior art has problems of high energy consumption, high carbon emissions, high cost and heavy pollution when extracting platinum group metals from metal-based solid waste and low-grade ores. Especially when the platinum group metal content is extremely low, traditional processes It is difficult to achieve efficient and green recycling.
The direct bio-evaporation of sulfide and indirect bio-evaporation of oxides are used to couple the processes of ball milling, reselection, flotation, adsorption and electrolysis to achieve green extraction and recovery of platinum group metals in series through multiple processes.
It realizes efficient extraction and recycling of low-content platinum group metals, reduces energy consumption and carbon emissions, improves recovery and purity, and solves the cost and pollution problems in traditional processes.
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of solid waste recovery, and specifically relates to a method for green extraction and recovery of platinum group metals from solid waste and low-grade ores. Background Art
[0002] Metal-based solid wastes such as non-ferrous tailings, steel tailings, non-ferrous smelting dust, steel smelting dust, gold beneficiation tailings, and quite a few low-grade gold-bearing ores such as sulfide-poor gold ores, polysulfide gold ores, polymetallic gold ores, gold-bearing copper ores, gold-bearing pyrite ores, etc. contain different concentrations of gold and other platinum group metals. Since these metal-based solid wastes and gold-bearing ores are of various types, complex structures, and varied components, and the occurrence forms, states, and valence states of gold and other platinum group metals vary greatly, and the concentration of platinum group metals is extremely low (1-10 mg / kg), this poses a great challenge to the extraction and recovery of gold and other platinum group metals.
[0003] Generally, the extraction and recovery technologies of platinum group metals in solid materials mainly include pyrometallurgical processes and hydrometallurgical processes; for metal-based solid waste and low-grade ores with low platinum group metal content (1-10 mg / kg), the traditional recovery process is first pyrometallurgical enrichment and then hydrometallurgical separation. First, the platinum group metals are captured by reduction melting to form an enriched alloy, and the smoke / alloy rich in the target metal is then separated and recovered by a hydrometallurgical process. Pyrometallurgical enrichment requires a high-temperature atmosphere, a variety of expensive additives and a complex reaction process, with high energy consumption, large carbon emissions and low yields. The concentrated NaOH alkaline leaching, concentrated HCI leaching, concentrated H2SO4 leaching and even direct wet leaching of aqua regia are plagued by many problems such as high cost, heavy pollution and difficulty in impurity removal, and their industrial commercialization also faces huge challenges. Green, efficient and low-carbon extraction technologies for low-content platinum group metals in metal-based solid waste and low-grade ores need to be studied urgently. Summary of the invention
[0004] The present application discloses a method for solidifying silty soft soil by using activated cementitious materials, which is centered on the coupling of direct bioleaching enrichment of sulfides and indirect bioleaching enrichment of oxides, with ball milling, gravity separation and flotation as pre-treatment, and impurity removal, adsorption and electrolysis as post-treatment. The green extraction and recovery of low-content platinum group metals in metal-based solid waste and low-grade ores are achieved through the series connection of multiple processes such as gravity separation, flotation, bioleaching-circulation enrichment, adsorption and electrolysis.
[0005] In order to solve the above technical problems, this application provides the following technical solutions: A method for green extraction and recovery of platinum group metals from solid waste and low-grade ores, comprising the following steps: Step S1, coarsely crushing the low-grade ore and grinding it to a particle size of 10-50 mesh, and using a gravity separation process to separate the low-density sediment and the high-density platinum group metal pyrite to obtain the coarsely ground low-grade ore and the coarse-grained platinum group metal sulfide after gravity separation; Step S2, fine grinding and ultrafine grinding are performed on the low-grade ore after coarse grinding and the coarse particles of platinum group metal sulfide after gravity separation to obtain powder with a particle size of 200-800 mesh, and then flotation is performed to obtain a pyrite enriched material rich in platinum group metals; Step S3, adding the pyrite enriched material rich in platinum group metals obtained by flotation into the inorganic salt solution of the MBR and compounding with other energy substrates; Step S4, when the concentration of platinum group metals in the regenerated active leachate no longer increases, it indicates that the direct leaching of platinum group metals in the pyrite as the energy substrate has been completed, and the solid energy substrate in the MBR needs to be replaced; Step S5, slowly adding hydrogen peroxide and one or more of potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate and ammonia water to the high-concentration platinum group metal enriched leachate produced by biological circulation leaching, stirring at 80° C.-90° C. until the pH value of the enriched liquid rises to 2.5-4.0 and keeping warm for 15-45 minutes, then centrifuging, filtering and filtering to remove iron-based precipitates and collecting low-iron platinum group metal enriched liquid; Step S6, extracting and separating the platinum group metals in the low-iron platinum group metal enriched solution by using anion targeted adsorption resin.
[0006] Optionally, in step S1, the slurry concentration in the gravity separation process is 20%-50% (w / v), the centrifugal speed is 800-1500 rpm, the residence time is 2-6 seconds, the temperature is 20°C-50°C, and a pyrite material with a density of 4.5-5.0 and a platinum group metal content of 2.0-10 g / ton is obtained, and the platinum group metal recovery rate is 50%-85%.
[0007] Optionally, in step S2, the flotation process is carried out at room temperature, with a solid-liquid ratio of 10%-35% and a residence time of 0.5-4 hours; wherein the activator is copper nitrate, copper chloride or copper sulfate, and the addition amount is 200-1000 g / ton; the frother is No. 2 oil, No. 4 oil or eucalyptus oil, and the addition amount is 200-1000 g / ton; the dispersant is water glass, sodium tripolyphosphate or sodium dodecyl sulfate, and the addition amount is 500-2500 g / ton; butyric acid 200-800 g / ton, ethyl thiocyanate 200-1000 g / ton, and the collector (Y89) 200-800 g / ton; the density of the pyrite enriched material of platinum group metals is 5.0-6.0, and the recovery rate of platinum group metals is 60%-90%.
[0008] Optionally, in step S3, the membrane pore size of the MBR is 0.1-0.5 microns, and the pyrite enriched material is compounded with thiosulfate, ferrous sulfate, sulfur, and waste sulfur paste.
[0009] Optionally, in step S3, the pyrite concentration is 2%-15% (w / v), the ratio of pyrite to the composite energy substrate is 1-10; the culture temperature is 20-40°C, the stirring speed is 30-150 rpm, the aeration volume is 0.10-1.0 reactor volume / min, and the sulfide iron oxidizing bacteria inoculation concentration is 3%-15%. Under the conditions, 0.5-2.0 reactor volumes of active leachate are extracted through the membrane every day, and the active leachate characteristics are: pH 0.5-2.0, Fe 2+ Concentration 200-1000mg / L, Fe 3+ Concentration 500-2500 mg / L, amino acid concentration 100-500 mg / L, extracellular polymer concentration 200-1000 mg / L, gold and other platinum group metals concentration 1-5 mg / L.
[0010] Optionally, in step S3, the oxide-enriched material rich in platinum group metals obtained by flotation is added to the leaching tank, and reacts with the active leachate to achieve indirect leaching of the oxide-enriched material; the indirect leaching temperature is 20-40°C, the leaching time is 1-4 hours, the solid-liquid ratio is 10%-50%, the stirring speed is 25-100 rpm, and the concentration of gold and other platinum group metals in the leachate is 5-50 mg / L.
[0011] Optionally, in step S4, when the solid energy substrate in the MBR is replaced, membrane pumping is suspended, and the mud-water mixture in the MBR is subjected to low-speed centrifugation and macroporous membrane filtration to separate the solid energy substrate and the bacterial solution, and the bacterial solution is returned to the MBR, and the pyrite after direct leaching of platinum group metals is discharged, and new pyrite rich in platinum group metals and composite energy substrates are added to the MBR for new batches of direct leaching and production of active leachate; the regenerated active leachate is used for indirect bioleaching of new batches of oxide materials; the pyrite for direct leaching to extract platinum group metals is replaced 2-4 times, and after 4-8 batches of platinum group metals in the oxide are extracted by indirect leaching, the enriched leachate containing high concentrations of platinum group metals is opened for separation and purification of platinum group metals.
[0012] Optionally, in step S5, the effective concentration of hydrogen peroxide is 30%, the added amount is 1%-5%; and the stirring speed is 30-120 rpm.
[0013] Optionally, in step S6, a gold-absorbing resin is used to specifically adsorb and separate gold in the enriched solution, and a resin that absorbs platinum group metals is used to specifically adsorb and separate platinum group metals in the enriched solution.
[0014] Optionally, the dosage of the targeted adsorption resin is 20%-40%, the adsorption temperature is 20°C-50°C, the adsorption time is 6-12 hours, and the saturated gold loading of the resin is 50-150 g / L.
[0015] The advantages of this application are: 1. In the MBR regeneration tank, direct leaching and enrichment of platinum group metals in sulfides is achieved by replacing sulfide materials, and indirect leaching and enrichment of platinum group metals in oxides is achieved by indirect leaching and enrichment of oxides. The direct leaching and enrichment of sulfides and the indirect leaching and enrichment of oxides are coupled to achieve the coordinated leaching and efficient liquid phase enrichment of platinum group metals in low-content solid waste and low-grade ores.
[0016] 2. With the coupling of direct bioleaching enrichment of sulfides and indirect bioleaching enrichment of oxides as the core, ball milling, gravity separation and flotation as pre-treatment, impurity removal, adsorption and electrolysis as post-treatment, the green extraction and recovery of low-content platinum group metals in metal-based solid waste and low-grade ores is achieved through the series connection of multiple processes such as gravity separation, flotation, bioleaching-cyclic enrichment, adsorption and electrolysis. DETAILED DESCRIPTION
[0017] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0018] The present application provides a method for green extraction and recovery of platinum group metals from solid waste and low-grade ores, which specifically comprises the following steps: Step S1, after rough crushing, the low-grade ore is coarsely ground to a particle size of 10-50 mesh, and the coarse-grained mixed tailings are separated by a gravity separation process from the low-density mud and the high-density platinum group metal pyrite to obtain the coarsely ground low-grade ore and the coarse-grained platinum group metal sulfide after gravity separation.
[0019] Among them, the slurry concentration of the gravity separation process is 20%-50% (w / v), the centrifugal speed is 800-1500 rpm, the residence time is 2-6 seconds, the temperature is 20℃-50℃, and the pyrite material with a density of 4.5-5.0 and a platinum group metal content of 2.0-10 g / ton is obtained, and the platinum group metal recovery rate is 50%-85%.
[0020] Step S2, the low-grade ore after coarse grinding and the coarse particles of platinum group metal sulfide after gravity separation are finely ground and ultrafinely ground to obtain a powder with a particle size of 200-800 mesh; for solid waste materials such as fine powder tailings, fly ash and smoke, there is no need to grind them again, and they can be directly floated to obtain a pyrite enriched material rich in platinum group metals.
[0021] The flotation process is carried out at room temperature, with a solid-liquid ratio of 10%-35% and a residence time of 0.5-4 hours. The activator is copper nitrate, copper chloride or copper sulfate, and the addition amount is 200-1000 g / ton; the frother is No. 2 oil, No. 4 oil or eucalyptus oil, and the addition amount is 200-1000 g / ton; the dispersant is water glass, sodium tripolyphosphate or sodium dodecyl sulfate, and the addition amount is 500-2500 g / ton; butyl xanthate 200-800 g / ton, ethyl thiocyanate 200-1000 g / ton, and collector (Y89) 200-800 g / ton. The platinum group metal enriched material is harvested, the platinum group metal enrichment multiple is 3-10 times, the enriched material density is 5.0-6.0, and the platinum group metal recovery rate is 60%-90%.
[0022] Step S3, adding the pyrite enriched material rich in platinum group metals obtained by flotation into the inorganic salt solution of MBR (membrane pore size 01-0.5 micron) and compounding with other energy substrates; The energy substrates include thiosulfate, ferrous sulfate, sulfur, waste sulfur paste and the like.
[0023] The concentration of pyrite is 2%-15% (w / v), and the ratio of pyrite to compound energy substrate is 1-10. The culture temperature is 20-40°C, the stirring speed is 30-150 rpm, the aeration volume is 0.10-1.0 reactor volume / minute, and the inoculation concentration of sulfide-oxidizing bacteria is 3%-15%. 0.5-2.0 reactor volumes of active leachate are extracted through the membrane every day. The characteristics of the active leachate are: pH 0.5-2.0, Fe 2+ Concentration 200-1000mg / L, Fe 3+ The concentration is 500-2500 mg / L, the amino acid concentration is 100-500 mg / L, the extracellular polymer concentration is 200-1000 mg / L, and the gold and other platinum group metal concentrations are 1-5 mg / L. The oxide enriched material rich in platinum group metals obtained by flotation is added to the leaching tank and reacts with the active leachate to achieve indirect leaching of the oxide enriched material. The indirect leaching temperature is 20-40°C, the leaching time is 1-4 hours, the solid-liquid ratio is 10%-50%, the stirring speed is 25-100 rpm, and the concentration of gold and other platinum group metals in the leaching solution is 5-50 mg / L.
[0024] Step S4, when the concentration of platinum group metals in the regenerated active leachate no longer increases, it means that the direct leaching of platinum group metals in the pyrite as the energy substrate has been completed, and the solid energy substrate in the MBR needs to be replaced.
[0025] When replacing the solid energy substrate, the membrane pumping is suspended, and the solid energy substrate and bacterial solution are separated by low-speed centrifugation and macroporous membrane filtration in the MBR. The bacterial solution is returned to the MBR, and the pyrite after direct leaching of platinum group metals is discharged. New pyrite rich in platinum group metals and composite energy substrates are added to the MBR for new (multiple) batches of direct leaching and production (regeneration) of active leachate. The regenerated active leachate is used for indirect bioleaching of new (multiple) batches of oxide materials. After the pyrite for direct leaching and extraction of platinum group metals is replaced 2-4 times and 4-8 batches of platinum group metals in oxides are extracted by indirect leaching, the enriched leachate containing high concentrations of platinum group metals (100-500 mg / L) is opened for separation and purification of platinum group metals. The entire bioleaching-circulation enrichment process is restarted.
[0026] Step S5, slowly add hydrogen peroxide (effective concentration 30%, added amount 1%-5%) and one or more of potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate, and ammonia water (concentration 0.5-2.0M) to the high-concentration platinum group metal enriched leaching solution produced by biological circulation leaching, stir (30-120 rpm) at 80°C-90°C until the pH value of the enriched solution rises to 2.5-4.0 and keep warm for 15-45 minutes, then centrifuge, filter, and filter press to remove iron-based precipitates and collect low-iron platinum group metal enriched solution (total iron concentration 0.2-1.0 g / L).
[0027] Among them, the low-iron enriched liquid is further removed by cationic resin ion exchange 3+ 、Al 3+ , Pb 2+ , Ca 2+ Mg 2+ Impurity metal ions. Resin impurity removal process: resin concentration 15%-30% (v / v), adsorption temperature 20℃-50℃, adsorption time 0.5-2.5 hours, stirring speed 20-80 rpm, residual concentration of iron and aluminum 20-100 mg / L, residual concentration of calcium and magnesium 40-200 mg / L. Use centrifugation, filtration, and filter press to separate the resin and collect the purified enriched liquid. The saturated resin that adsorbs impurities is regenerated by concentrated acid and washed with clean water and then reused for impurity removal of low-iron enriched liquid.
[0028] Step S6, extracting and separating the platinum group metals in the low-iron platinum group metal enriched solution by using anion targeted adsorption resin.
[0029] Among them, gold-absorbing resin is used to specifically adsorb and separate gold in the enriched solution, and platinum group metal-absorbing resin is used to specifically adsorb and separate platinum group metals in the enriched solution. The dosage of targeted adsorption resin is 20%-40%, the adsorption temperature is 20℃-50℃, the adsorption time is 6-12 hours, and the saturated gold (platinum group metal) loading of the resin is 50-150 g / L. Desorption process: sulfuric acid concentration is 2%-10%, thiourea concentration is 2%-10%, desorption temperature is 20℃-50℃, desorption time is 2-6 hours, the average desorption rate of platinum group metals is 80%-95%, and the concentration of platinum group metals in precious liquid is 15-60 g / L. The precious liquid is electrolyzed to produce single-substance platinum group metals or alloys with a purity of ≥90%. The desorbed targeted resin is regenerated in alkaline solution and washed with clean water to neutrality before reuse.
[0030] The following specific examples 1-3 are used to describe in detail the method for green extraction and recovery of platinum group metals from solid waste and low-grade ores provided in the present application. Example 1
[0031] Example 1 provides a method for green extraction and recovery of platinum group metals from solid waste and low-grade ores, which specifically comprises the following steps: Step S1, zinc-lead beneficiation tailings are separated from sediment and platinum group metal-containing pyrite by gravity separation process. The gravity separation process has a slurry concentration of 20% (w / v), a centrifugal speed of 1500 rpm, a residence time of 2 seconds, a temperature of 20°C, and a pyrite material with a density of 4.5 and a platinum group metal content of 10g / ton, and a platinum group metal recovery rate of 81%.
[0032] Step S2, the sulfide containing platinum group metals is subjected to flotation enrichment by ultrafine grinding to obtain a powder with a particle size of 600 mesh. The flotation process is carried out at room temperature, with a solid-liquid ratio of 25% and a residence time of 4 hours. The activator is a mixture of copper nitrate and copper chloride, and the addition amount is 1000 g / ton; the frother is a mixture of No. 2 oil and No. 4 oil, and the addition amount is 500 g / ton; the dispersant is water glass, and the addition amount is 1000 g / ton; 400 g / ton of butyl xanthate, 500 g / ton of ethyl thiocyanate, and 350 g / ton of collector (Y89). The platinum group metal enriched material is harvested, the platinum group metal enrichment multiple is 3.6 times, the enriched material density is 5.5, and the platinum group metal recovery rate is 84%.
[0033] Step S3, add the pyrite enriched material rich in platinum group metals obtained by flotation into the inorganic salt solution of MBR (membrane pore size 0.25 micron) and compound with sodium thiosulfate (1.5%) and sulfur (1.5%). Wherein, the pyrite concentration is 15% (w / v), the culture temperature is 30°C, the stirring speed is 50 rpm, the aeration volume is 0.2 reactor volume / min, and the inoculation concentration of sulfide iron oxidizing bacteria is 10%. 1.0 reactor volume of active leachate is extracted through the membrane every day. The characteristics of the active leachate are: pH 0.8, Fe 2+ Concentration 500 mg / L, Fe 3+ The concentration is 1000 mg / L, the amino acid concentration is 210 mg / L, the extracellular polymer concentration is 270 mg / L, and the gold and other platinum group metal concentrations are 2.4 mg / L. The zinc-lead smelting ash oxide enriched material rich in platinum group metals obtained by flotation is added to the leaching tank, and reacts with the active leachate to achieve indirect leaching of the oxide enriched material. The indirect leaching temperature is 30°C, the leaching time is 3 hours, the solid-liquid ratio is 15%, the stirring speed is 60 rpm, and the concentration of gold and other platinum group metals in the leachate is 22 mg / L.
[0034] Step S4, when the concentration of platinum group metals in the regenerated active leachate no longer increases, it indicates that the direct leaching of platinum group metals in pyrite as an energy substrate has been completed, and the solid energy substrate in the MBR needs to be replaced. In this case, membrane pumping is suspended, and the mud-water mixture in the MBR is separated from the solid energy substrate and the bacterial solution by low-speed centrifugation, macroporous membrane filtration, etc. The bacterial solution is returned to the MBR, and the pyrite after direct leaching of platinum group metals is discharged. New pyrite rich in platinum group metals and composite energy substrates are added to the MBR for new (multiple) batches of direct leaching and production (regeneration) of active leachate. The regenerated active leachate is used for indirect bioleaching of new (multiple) batches of oxide materials. After the pyrite for direct leaching of platinum group metals was replaced 3 times, and after 6 batches of indirect leaching of platinum group metals in oxides, the enriched leachate containing high concentrations of platinum group metals (260 mg / L) was opened for separation and purification of platinum group metals.
[0035] Step S5, slowly add hydrogen peroxide (effective concentration 30%, addition amount 5%) and sodium hydroxide (concentration 0.5M) to the enriched leaching solution containing high concentration of platinum group metals produced by biological circulation leaching, stir (100 rpm) at 90°C until the pH value of the enriched solution rises to 3.0 and keep warm for 30 minutes, then centrifuge, filter, and filter press to remove iron-based precipitates and collect low-iron platinum group metal enriched solution (total iron concentration 0.6 g / L). Among them, the low-iron enriched solution is further removed by cationic resin ion exchange 3+ 、Al 3+ , Pb 2+ , Ca 2+ Mg 2+Impurity metal ions. Resin impurity removal process: resin concentration 10% (v / v), adsorption temperature 25℃, adsorption time 1.0 hour, stirring speed 60 rpm, residual concentration of iron and aluminum 80 mg / L, residual concentration of calcium and magnesium 110 mg / L. Use centrifugation, filtration, and filter press to separate the resin and collect the purified enriched liquid.
[0036] Step S6, extract and separate the platinum group metals in the low-iron platinum group metal enriched solution by anion targeted adsorption resin. Among them, the dosage of targeted adsorption resin is 30%, the adsorption temperature is 30°C, the adsorption time is 8 hours, and the resin saturated gold (platinum group metal) loading is 120 g / L. Desorption process: sulfuric acid concentration is 5%, thiourea concentration is 5%, desorption temperature is 30°C, desorption time is 6 hours, average desorption rate of platinum group metals is 87%, and the concentration of platinum group metals in precious liquid is 32 g / L. The precious liquid is electrolyzed to produce single-substance platinum group metals or alloys with a purity of 92%. Example 2
[0037] Example 2 provides a method for green extraction and recovery of platinum group metals from solid waste and low-grade ores, which specifically comprises the following steps: Step S1, the copper beneficiation tailings are separated from the silt and the platinum group metal-containing pyrite by a gravity separation process. The gravity separation process has a slurry concentration of 25% (w / v), a centrifugal speed of 1200 rpm, a residence time of 2 seconds, a temperature of 30°C, and a pyrite material with a density of 4.6 and a platinum group metal content of 11g / ton, and a platinum group metal recovery rate of 82%.
[0038] Step S2, the sulfide containing platinum group metals is subjected to flotation enrichment by ultrafine grinding to obtain a powder with a particle size of 400 mesh. The flotation process is carried out at room temperature, with a solid-liquid ratio of 20% and a residence time of 5 hours. The activator is a mixture of copper sulfate and copper chloride, with an addition amount of 800 g / ton; the frother is No. 2 oil, with an addition amount of 600 g / ton; the dispersant is water glass, with an addition amount of 600 g / ton; butyl xanthate 500 g / ton, ethyl thiocyanate 400 g / ton, and collector (Y89) 400 g / ton. The platinum group metal enriched material is harvested, with a platinum group metal enrichment multiple of 3.5 times, an enriched material density of 5.7, and a platinum group metal recovery rate of 82%.
[0039] Step S3, add the pyrite enriched material rich in platinum group metals obtained by flotation into the inorganic salt solution of MBR (membrane pore size 0.25 micron) and compound with waste sulfur paste (1.5%) and sulfur (1.5%). Among them, the pyrite concentration is 12% (w / v), the culture temperature is 32°C, the stirring speed is 60 rpm, the aeration volume is 0.15 reactor volume / minute, and the sulfide iron oxidizing bacteria inoculation concentration is 15%. 1.0 reactor volume of active leachate is extracted through the membrane every day. The characteristics of the active leachate are: pH 0.8, Fe 2+Concentration 600 mg / L, Fe 3+ The concentration is 1100 mg / L, the amino acid concentration is 230 mg / L, the extracellular polymer concentration is 260 mg / L, and the gold and other platinum group metal concentrations are 3.4 mg / L. The oxide enriched material of copper smelting ash rich in platinum group metals obtained by flotation is added to the leaching tank, and reacts with the active leachate to achieve indirect leaching of the oxide enriched material. The indirect leaching temperature is 35°C, the leaching time is 3.5 hours, the solid-liquid ratio is 16%, the stirring speed is 80 rpm, and the concentration of gold and other platinum group metals in the leachate is 25 mg / L.
[0040] Step S4, when the concentration of platinum group metals in the regenerated active leachate no longer increases, it indicates that the direct leaching of platinum group metals in pyrite as an energy substrate has been completed, and the solid energy substrate in the MBR needs to be replaced. In this case, membrane pumping is suspended, and the mud-water mixture in the MBR is separated from the solid energy substrate and the bacterial solution by low-speed centrifugation, macroporous membrane filtration, etc. The bacterial solution is returned to the MBR, and the pyrite after direct leaching of platinum group metals is discharged. New pyrite rich in platinum group metals and composite energy substrates are added to the MBR for new (multiple) batches of direct leaching and production (regeneration) of active leachate. The regenerated active leachate is used for indirect bioleaching of new (multiple) batches of oxide materials. After the pyrite for direct leaching of platinum group metals was replaced 4 times and 5 batches of platinum group metals in oxides were extracted by indirect leaching, the enriched leachate containing high concentrations of platinum group metals (220 mg / L) was opened for separation and purification of platinum group metals.
[0041] Step S5, slowly add hydrogen peroxide (effective concentration 30%, addition amount 5%) and sodium hydroxide (concentration 0.5M) to the enriched leaching solution containing high concentration of platinum group metals produced by biological circulation leaching, stir (100 rpm) at 85°C until the pH value of the enriched solution rises to 3.3 and keep warm for 25 minutes, then centrifuge, filter, and filter press to remove iron-based precipitates and collect low-iron platinum group metal enriched solution (total iron concentration 0.65g / L). Among them, the low-iron enriched solution is further removed by cationic resin ion exchange 3+ 、Al 3+ , Pb 2+ , Ca 2+ Mg 2+ Impurity metal ions. Resin impurity removal process: resin concentration 12% (v / v), adsorption temperature 30℃, adsorption time 1.5 hours, stirring speed 60 rpm, residual concentration of iron and aluminum 85mg / L, residual concentration of calcium and magnesium 120mg / L. Use centrifugation, filtration, and filter press to separate the resin and collect the purified enriched liquid.
[0042] Step S6, extract and separate the platinum group metals in the low-iron platinum group metal enriched solution by anion targeted adsorption resin. Among them, the dosage of targeted adsorption resin is 35%, the adsorption temperature is 35°C, the adsorption time is 6 hours, and the resin saturated gold (platinum group metal) loading is 150 g / L. Desorption process: sulfuric acid concentration is 6%, thiourea concentration is 6%, desorption temperature is 40°C, desorption time is 8 hours, average desorption rate of platinum group metals is 89%, and the concentration of platinum group metals in precious liquid is 42 g / L. The precious liquid is electrolyzed to produce single-substance platinum group metals or alloys with a purity of 91%. Example 3
[0043] Example 3 provides a method for green extraction and recovery of platinum group metals from solid waste and low-grade ores, which specifically comprises the following steps: Step S1, the pyrite acid-making waste residue is separated from the material containing platinum group metals by a gravity separation process. The gravity separation process has a slurry concentration of 30% (w / v), a centrifugal speed of 1000 rpm, a residence time of 2 seconds, a temperature of 35°C, a collection density of 4.2, a platinum group metal content of 14.3 g / ton, and a platinum group metal recovery rate of 65%.
[0044] Step S2, the high-value material containing platinum group metals is subjected to flotation enrichment by ultrafine grinding to obtain a powder with a particle size of 600 mesh. The flotation process is carried out at room temperature, with a solid-liquid ratio of 25%, a residence time of 4 hours, an activator of a mixture of copper sulfate and copper nitrate, and an addition amount of 850 g / ton; a frother is No. 2 oil, and an addition amount of 500 g / ton; a dispersant is water glass, and an addition amount of 500 g / ton; butyl xanthate 500 g / ton, ethyl thiocyanate 400 g / ton, and a collector (Y89) 400 g / ton. The platinum group metal enriched material is harvested, with a platinum group metal enrichment multiple of 3.0 times, an enriched material density of 5.6, and a platinum group metal recovery rate of 74%.
[0045] Step S3, add the sulfide gold tailings to the inorganic salt solution of the MBR (membrane pore size 0.55 microns) and compound with the waste sulfur paste (5.0%). Among them, the concentration of pyrite gold tailings is 10% (w / v), the culture temperature is 35°C, the stirring speed is 40 rpm, the aeration volume is 0.25 reactor volume / minute, and the sulfide iron oxidizing bacteria inoculation concentration is 10%. 1.0 reactor volume of active leachate is extracted through the membrane every day. The characteristics of the active leachate are: pH 0.7, Fe 2+ Concentration 500 mg / L, Fe 3+The concentration is 1300 mg / L, the amino acid concentration is 260 mg / L, the extracellular polymer concentration is 280 mg / L, and the gold ion concentration is 1.2 mg / L. Add the oxide gold tailings to the leaching tank and react with the active leachate to achieve indirect leaching of the oxidized tailings. The indirect leaching temperature is 50°C, the leaching time is 4.5 hours, the solid-liquid ratio is 25%, the stirring speed is 60 rpm, and the gold ion concentration in the leaching solution is 9.8 mg / L.
[0046] Step S4, when the gold ion concentration in the regenerated active leachate no longer increases, replace the sulfide gold tailings in the MBR. In which, membrane pumping is suspended, the mud-water mixture in the MBR is separated from the solid energy substrate and the bacterial solution by low-speed centrifugation, macroporous membrane filtration, etc., the bacterial solution is returned to the MBR, the pyrite after direct leaching is discharged, and new sulfide gold tailings and composite energy substrates are added to the MBR for new (multiple) batches of direct leaching and production (regeneration) of active leachate. The regenerated active leachate is used for indirect bioleaching of new (multiple) batches of oxide materials. After the direct leaching of pyrite gold tailings was replaced 4 times and the indirect leaching of oxide gold tailings was extracted for 5 batches, the enriched leaching solution containing high concentration of gold ions (54 mg / L) was opened for separation and purification of gold.
[0047] Step S5, slowly add hydrogen peroxide (effective concentration 30%, addition amount 4%) and sodium hydroxide (concentration 0.4M) to the gold-containing enriched leaching solution produced by biological circulation leaching, stir (100 rpm) at 90°C until the pH value of the enriched solution rises to 3.3 and keep warm for 25 minutes, then centrifuge, filter, and filter press to remove iron-based precipitates and collect low-iron platinum group metal enriched solution (total iron concentration 0.55g / L). The low-iron enriched solution is further removed by cationic resin ion exchange 3+ 、Al 3+ , Pb 2+ , Ca 2+ Mg 2+ Impurity metal ions. Resin impurity removal process: resin concentration 15% (v / v), adsorption temperature 30℃, adsorption time 2.5 hours, stirring speed 80 rpm, residual concentration of iron and aluminum 95mg / L, residual concentration of calcium and magnesium 110mg / L. Use centrifugation, filtration, and filter press to separate the resin and collect the purified enriched liquid.
[0048] Step S6, extract and separate the platinum group metals in the low-iron platinum group metal enriched solution by anion targeted adsorption resin. Among them, the dosage of targeted adsorption resin is 35%, the adsorption temperature is 35°C, the adsorption time is 6 hours, and the saturated gold loading of the resin is 120 g / L. Desorption process: sulfuric acid concentration is 6%, thiourea concentration is 6%, desorption temperature is 40°C, desorption time is 8 hours, average gold desorption rate is 92%, and gold concentration in precious liquid is 19 g / L. Elemental gold is produced by electrolysis of precious liquid with a purity of 93%.
[0049] The embodiments of the present application are described above, but the present application is not limited to the above-mentioned specific implementation modes. The above-mentioned specific implementation modes are merely illustrative and not restrictive. Under the guidance of the present application, ordinary technicians in this field can also make many forms without departing from the purpose of the present application and the scope of protection of the claims, all of which are within the protection of the present application.
Claims
1. A method for green extraction and recovery of platinum group metals from solid waste and low-grade ores, It is characterized in that The steps include: Step S1, coarsely crushing the low-grade ore and grinding it to a particle size of 10-50 mesh, and using a gravity separation process to separate the low-density sediment and the high-density platinum group metal pyrite to obtain the coarsely ground low-grade ore and the coarse-grained platinum group metal sulfide after gravity separation; Step S2, fine grinding and ultrafine grinding are performed on the low-grade ore after rough grinding and the coarse particles of platinum group metal sulfide after gravity separation to obtain a powder with a particle size of 200-800 mesh, and then flotation is performed to obtain a pyrite enriched material rich in platinum group metals; Step S3, adding the pyrite enriched material rich in platinum group metals obtained by flotation into the inorganic salt solution of the MBR and compounding with other energy substrates; Step S4, when the concentration of platinum group metals in the regenerated active leachate no longer increases, it indicates that the direct leaching of platinum group metals in the pyrite as the energy substrate has been completed, and the solid energy substrate in the MBR needs to be replaced; Step S5, slowly adding hydrogen peroxide and one or more of potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate and ammonia water to the high-concentration platinum group metal enriched leachate produced by biological circulation leaching, stirring at 80° C.-90° C. until the pH value of the enriched liquid rises to 2.5-4.0 and keeping warm for 15-45 minutes, then centrifuging, filtering and filtering to remove iron-based precipitates and collecting low-iron platinum group metal enriched liquid; Step S6, extracting and separating the platinum group metals in the low-iron platinum group metal enriched solution by using anion targeted adsorption resin.
2. The method according to claim 1, It is characterized in that In step S1, the ore pulp concentration in the gravity separation process is 20%-50% (w / v), the centrifugal speed is 800-1500 rpm, the residence time is 2-6 seconds, the temperature is 20°C-50°C, and a pyrite material with a density of 4.5-5.0 and a platinum group metal content of 2.0-10 g / ton is obtained, and the platinum group metal recovery rate is 50%-85%.
3. The method according to claim 1 or 2, It is characterized in that In step S2, the flotation process is carried out at room temperature, with a solid-liquid ratio of 10%-35% and a residence time of 0.5-4 hours; wherein the activator is copper nitrate, copper chloride or copper sulfate, and the addition amount is 200-1000 g / ton; the frother is No. 2 oil, No. 4 oil or eucalyptus oil, and the addition amount is 200-1000 g / ton; the dispersant is water glass, sodium tripolyphosphate or sodium dodecyl sulfate, and the addition amount is 500-2500 g / ton; butyl xanthate 200-800 g / ton, ethyl thiocyanate 200-1000 g / ton, and the collector (Y89) 200-800 g / ton; the density of the pyrite enriched material of the platinum group metal is 5.0-6.0, and the recovery rate of the platinum group metal is 60%-90%.
4. The method according to claim 1, It is characterized in that In step S3, the pore size of the MBR membrane is 0.1-0.5 micrometers, and other energy substrates include thiosulfate, ferrous sulfate, sulfur, and waste sulfur paste.
5. The method according to claim 4, It is characterized in that In step S3, the pyrite concentration is 2%-15% (w / v), the ratio of pyrite to the composite energy substrate is 1-10; the culture temperature is 20-40°C, the stirring speed is 30-150 rpm, the aeration volume is 0.10-1.0 reactor volume / min, and the sulfide iron oxidizing bacteria inoculation concentration is 3%-15%. 0.5-2.0 reactor volumes of active leachate are extracted through the membrane every day. The active leachate has the following characteristics: pH value 0.5-2.0, Fe 2+ Concentration 200-1000mg / L, Fe 3+ Concentration 500-2500 mg / L, amino acid concentration 100-500 mg / L, extracellular polymer concentration 200-1000 mg / L, gold and other platinum group metals concentration 1-5 mg / L.
6. The method according to claim 5, It is characterized in that In step S3, the oxide-enriched material rich in platinum group metals obtained by flotation is added to the leaching tank, and reacts with the active leachate to achieve indirect leaching of the oxide-enriched material; the indirect leaching temperature is 20-40° C., the leaching time is 1-4 hours, the solid-liquid ratio is 10%-50%, the stirring speed is 25-100 rpm, and the concentration of gold and other platinum group metals in the leachate is 5-50 mg / L.
7. The method according to claim 5, It is characterized in that In step S4, when the solid energy substrate in the MBR is replaced, the membrane pumping is suspended, and the mud-water mixture in the MBR is subjected to low-speed centrifugation and macroporous membrane filtration to separate the solid energy substrate and the bacterial solution, and the bacterial solution is returned to the MBR, and the pyrite after direct leaching of platinum group metals is discharged, and new pyrite rich in platinum group metals and the composite energy substrate are added to the MBR to carry out direct leaching of a new batch and produce active leachate; Regenerated active leachate is used for indirect bioleaching of new batches of oxide materials; the pyrite used for direct leaching to extract platinum group metals is replaced 2-4 times, and after 4-8 batches of indirect leaching to extract platinum group metals from oxides, the enriched leachate containing high concentrations of platinum group metals is opened for separation and purification of platinum group metals.
8. The method according to claim 5, It is characterized in that In step S5, the effective concentration of hydrogen peroxide is 30%, the added amount is 1%-5%; and the stirring speed is 30-120 rpm.
9. The method according to claim 5, It is characterized in that In step S6, a gold-absorbing resin is used to specifically adsorb and separate gold in the enriched solution, and a resin that absorbs platinum group metals is used to specifically adsorb and separate platinum group metals in the enriched solution.
10. The method according to claim 9, It is characterized in that The dosage of targeted adsorption resin is 20%-40%, the adsorption temperature is 20℃-50℃, the adsorption time is 6-12 hours, and the saturated gold loading of the resin is 50-150 g / L.
Citation Information
Patent Citations
Harmless treatment and high value utilization method for copper-containing sludge
CN106834699A
Method for separating nonferrous metals based on hydrometallurgy
CN112941335A
Precious metal recovery using thiocyanate lixiviant
US20040197249A1
Integrated, tank / heap biooxidation process
US5873927A