Composite refining modifier and preparation method thereof, high-iron-aluminum-silicon alloy and composite refining modification method of high-iron-aluminum-silicon alloy
By using a composite refining agent composed of Mn, Y and Ba, the α-Al grains, eutectic Si and iron-rich phases in high-ferrometer aluminum-silicon alloys are coordinated to solve the existing refining agents in the treatment of high-ferrometer aluminum-silicon alloys. The problem of poor refinement effect has achieved improvement in the mechanical properties of the materials and expansion of application scope.
Patent Information
- Application Number
- CN202410922331.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-08
AI Technical Summary
When the existing refining agents treat high-iron aluminum-silicon alloys, there are coarse dendritic α-Al grains, needle-flake eutectic Si and β-iron-rich phase refinement effects, and there is 'Si poisoning' phenomenon and aspiration. tendency limits the application range of materials.
Using composite refinement agents, including Mn, Y and Ba, the α-Al grains, eutectic Si and iron-rich phases in metamorphic high-ferrome aluminum-silicon alloy are synergistically refined by forming a uniform melt of Al-Mn-Y-Ba. , the reaction between Ti element and Si and the inspiration of Sr element are avoided, and the uniform distribution of grains and the improvement of mechanical properties are achieved.
Effectively eliminate coarse dendritic α-Al grains, needle-shaped eutectic Si and iron-rich phases, improve the strength and plasticity of high-iron aluminum-silicon alloys, broaden its application range, and does not have the phenomenon of 'Si poisoning' and tendency to inspire. , with high efficiency and stability.
Smart Images

Figure CN118910441A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of molten cast aluminum-silicon alloy modification, and in particular to a composite refining modifier and a preparation method thereof, a high-iron aluminum-silicon alloy and a composite refining modifier method thereof. Background Art
[0002] Aluminum-silicon alloy materials are considered to be an ideal lightweight material due to their light weight, good casting performance, heat and corrosion resistance, and high strength. However, recycled aluminum waste materials usually contain a large amount of impurity elements, especially the iron content will increase sharply, resulting in a high iron content in the recycled aluminum-silicon alloy, forming a high-iron aluminum-silicon alloy. These high-iron aluminum-silicon alloys will produce coarse dendritic α-Al grains, coarse needle-like eutectic Si and β-iron-rich phases during the solidification process, which seriously affect their strength, plasticity and corrosion resistance, limiting their application in various fields, especially in high-end manufacturing.
[0003] In order to solve the problems existing in high iron aluminum silicon alloys, the method of refining and modification is currently widely used. However, there are many problems with existing refiners, such as single function, easy decay, and difficulty in preparation and molding. For example, traditional Al-Ti refiners may cause "Si poisoning phenomenon", while Al-3B and Al-4.5Nb-0.5B refiners have single functions and the refining effect is easy to decay. In addition, although Al-10Sr intermediate alloy has excellent refining and modification effects on coarse needle-like eutectic silicon, its strong air absorption tendency easily leads to the generation of pore defects. Therefore, how to effectively refine and modify the above-mentioned coarse dendritic α-Al grains, needle-like eutectic Si and β-iron-rich phase is the key to solving the application problems of high iron aluminum silicon alloys. Summary of the invention
[0004] The problem solved by the invention is how to effectively refine and modify the coarse dendritic α-Al grains, needle-shaped eutectic Si and β-iron-rich phase.
[0005] In order to solve the above problems, the present invention provides a composite refining modifier and a preparation method thereof, a high iron aluminum silicon alloy and a composite refining modifier method thereof.
[0006] In a first aspect, the present invention provides a composite refining modifier, which comprises, by mass percentage, 5-9% Mn, 1-4% Y, 0.2-0.6% Ba, and the balance being Al and unavoidable impurity elements.
[0007] Optionally, the alloy comprises, by mass percentage, 7% Mn, 3% Y, 0.4% Ba, and the balance being Al and inevitable impurity elements.
[0008] In a second aspect, the present invention provides a method for preparing a composite refinement modifier, comprising:
[0009] According to the composition ratio of the composite refining modifier as described above, aluminum ingots, Al-Mn master alloy, Al-Ba master alloy and Al-Y master alloy are weighed respectively;
[0010] heating and melting the aluminum ingot to obtain an Al melt;
[0011] Adding the Al-Mn master alloy, the Al-Ba master alloy and the Al-Y master alloy to the Al melt in sequence to obtain an Al-Mn-Y-Ba uniform melt;
[0012] A refining agent is added to the Al-Mn-Y-Ba uniform melt, and the melt is cast into an ingot to obtain a composite refining modifier.
[0013] Optionally, the Al-Mn master alloy, the Al-Ba master alloy and the Al-Y master alloy are sequentially added to the Al melt to obtain an Al-Mn-Y-Ba uniform melt, comprising:
[0014] The Al melt is controlled at a first temperature, the Al-Mn master alloy is added to the Al melt, the Al-Mn master alloy is stirred and kept at the first temperature, and scum is removed to obtain a uniform Al-Mn melt;
[0015] Adding the Al-Ba master alloy to the Al-Mn homogeneous melt, and stirring the mixture under the first temperature to obtain an Al-Mn-Ba homogeneous melt;
[0016] The Al-Mn-Ba homogeneous melt is cooled to a second temperature, scum is removed, the Al-Y master alloy is added to the Al-Mn-Ba homogeneous melt, the mixture is kept warm and stirred at the second temperature, scum is removed, and the Al-Mn-Y-Ba homogeneous melt is obtained.
[0017] Optionally, a refining agent is added to the Al-Mn-Y-Ba uniform melt and cast into an ingot to obtain a composite refining modifier, comprising:
[0018] A refining agent is added to the Al-Mn-Y-Ba uniform melt, and the mixture is stirred and kept warm at the second temperature. After standing, the scum is removed, and the mixture is cooled to a third temperature, cast into an ingot, and cooled to room temperature to obtain the composite refining modifier.
[0019] Optionally, the Al-Mn master alloy, the Al-Ba master alloy and the Al-Y master alloy are all preheated before being added into the Al melt.
[0020] Optionally, the content of Mn in the Al-Mn master alloy is 5wt.%-20wt.%, the content of Y in the Al-Y master alloy is 5wt.%-10wt.%, and the content of Ba in the Al-Ba master alloy is 5wt.%-10wt.%.
[0021] In a third aspect, the present invention provides a composite refinement and modification method for a high iron aluminum silicon alloy, comprising:
[0022] The high iron aluminum silicon alloy raw material is heated and melted, and the scum is removed to obtain the high iron aluminum silicon alloy liquid;
[0023] Adding a composite refining modifier to the high iron aluminum silicon alloy liquid, keeping it warm and stirring it, to obtain a mixed metal melt; wherein the composite refining modifier is the composite refining modifier as described above, or is obtained by the preparation method of the composite refining modifier as described above;
[0024] A refining agent is added to the mixed metal melt, and nitrogen is introduced into the mixed metal melt at the same time. After standing, the temperature of the mixed metal melt is lowered to a fourth temperature, and a solidification molding process is performed after removing the slag to obtain a high iron aluminum silicon alloy after composite refinement and modification.
[0025] Optionally, the high iron aluminum silicon alloy raw material is heated and melted at 800°C-850°C.
[0026] In a fourth aspect, the present invention provides a high iron aluminum silicon alloy, wherein the high iron aluminum silicon alloy uses the composite refining modifier as described above during the refining and modification process, or the high iron aluminum silicon alloy is made by the composite refining and modification method of the high iron aluminum silicon alloy as described in any one of the above items.
[0027] The beneficial effects of the composite refinement modifier of the present invention are:
[0028] The composite refining modifier of the present invention can simultaneously achieve the refinement and modification of the α-Al grains, eutectic silicon and iron-rich phase of the high-iron aluminum-silicon alloy, effectively eliminate the harm of coarse dendritic α-Al grains, needle-shaped eutectic silicon and iron-rich phase to its mechanical properties, improve the strength and plasticity of the high-iron aluminum-silicon alloy, and has the advantages of high efficiency and stability, no "Si poisoning" phenomenon, no air absorption tendency, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The flowchart of the preparation method of the composite refinement modifier in the embodiment of the present invention;
[0030] Figure 2 A comparison chart of the statistical data of the metallographic structure characteristics of the high iron aluminum silicon alloy obtained in Examples 1 to 4 of the present invention and Comparative Examples 1 to 4;
[0031] Figure 3It is a comparison chart of the tensile stress-strain curves of the high iron aluminum silicon alloy obtained by Examples 1 to 4 of the present invention and Comparative Examples 1 to 4. DETAILED DESCRIPTION
[0032] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.
[0033] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by those skilled in the art to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific implementation methods and are not intended to limit this application;
[0034] The term "including" and its variations used in this document are open inclusions, i.e., "including but not limited to"; the term "based on" means "based at least in part on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments"; the term "optionally" means "optional embodiments".
[0035] In the related art, when refining and modifying the coarse dendritic α-Al grains, needle-shaped eutectic Si and β-iron-rich phase, the traditional Al-Ti series refiner is usually used. However, due to the strong affinity between Si and Ti, Si atoms cover the surface of Ti-containing particles, causing them to lose the non-uniform nucleation core of α-Al, resulting in "Si poisoning phenomenon"; in addition, when the Si content is greater than 4wt.%, Si reacts with Ti to form Ti5Si2 phase, consuming Ti element, and the non-uniform nucleation core of TiB2 or TiC particles formed is naturally reduced, which cannot effectively refine the aluminum-silicon alloy and eliminate the coarse dendritic α-Al grains. Although the refining effects of Al-3B, Al-4.5Nb-0.5B, etc. are better than those of the traditional Al-Ti series refiners, their refining effects are easy to decline, and the preparation and molding are difficult. Moreover, these refiners only have the function of refining α-Al, and do not have the function of modifying eutectic silicon and iron-rich phases, and their functions are relatively single. In addition, Al-10Sr master alloy can be used as a modifier for eutectic silicon in aluminum-silicon alloy. However, the Sr in Al-10Sr is relatively active and has a strong tendency to absorb air, which can easily lead to air absorption in the aluminum-silicon alloy and produce pore defects, thereby reducing the mechanical properties of the aluminum-silicon alloy. In addition, it only has the effect of modifying eutectic silicon.
[0036] In view of the problems existing in the above-mentioned related technologies, the present embodiment provides a composite refining modifier and a preparation method thereof, a high iron aluminum silicon alloy and a composite refining modifier method thereof.
[0037] A composite refining modifier provided by an embodiment of the present invention comprises, by mass percentage, 5-9% Mn, 1-4% Y, 0.2-0.6% Ba, and the remainder Al and unavoidable impurity elements, wherein the content of a single impurity element is ≤0.05%, and the total amount of impurity elements is ≤0.15%.
[0038] The composite refining modifier of this embodiment uses Mn, Y, and Ba as refining elements. Among them, Mn atoms can replace Fe atoms in the iron-rich phase, change the crystal structure and growth direction of the iron-rich phase, and transform the coarse needle-shaped β-iron-rich phase into a fine Chinese character-shaped α-iron-rich phase, greatly reducing the harm of the iron-rich phase to the alloy plasticity. In addition, Mn atoms can also increase the melting point of the iron-rich phase, from between the formation temperature of α-Fe and eutectic silicon to higher than the formation temperature of α-Al. Therefore, a large number of iron-rich phase particles formed become heterogeneous nucleation cores of α-Al, which plays a role in refining α-Al grains.
[0039] Y is a rare earth element, which will form Al3Y intermediate phase in the alloy. The dispersed Al3Y is a non-uniform nucleation point of α-Al, which transforms the coarse dendritic α-Al grains into fine equiaxed grains. At the same time, Y, as an active element, will be adsorbed on the growth interface of needle-shaped eutectic silicon and iron-rich phase, hindering the preferential growth of eutectic silicon and iron-rich phase, playing a role in modification, and Y can absorb gas in the melt, and has a certain degassing function. In addition, among the rare earth elements, Y is the lightest rare earth element among the 17 rare earth elements except Sc. The density of Al3Y formed with aluminum is much lower than that of the intermediate phase formed by lanthanide rare earth elements and aluminum, so it is not easy to sink and aggregate, and can be more stably and evenly distributed in the aluminum alloy melt, playing a better role in refining grains. In addition, Y has a low price, which is conducive to cost control. Compared with the very expensive Sc, it is more conducive to cost control and promotion and application. Therefore, the composite refining modifier component of this embodiment contains only Y, a rare earth element.
[0040] Ba has a very good refining and modifying effect on eutectic silicon in aluminum-silicon alloy. Adding a trace amount of Ba can transform coarse needle-like eutectic silicon into fine particles and short rods and evenly distribute them in the aluminum-silicon alloy, eliminating the harm of coarse needle-like eutectic silicon to the mechanical properties of high-iron aluminum-silicon alloy.
[0041] The inventors found in their research that the composite refining modifier Al-Mn-Y-Ba can synergistically refine and modify α-Al grains, eutectic silicon and iron-rich phases in high-iron aluminum-silicon alloys. Specifically, on the one hand, Mn atoms can transform the coarse needle-shaped β-iron-rich phase into a fine Chinese character-shaped α-iron-rich phase, greatly weakening the splitting effect of the β-iron-rich phase on the aluminum matrix, while Y will be adsorbed on the growth interface of the iron-rich phase, hindering the preferential growth of the iron-rich phase, thereby coordinating with Mn atoms to modify and refine the β-iron-rich phase. On the other hand, Y will form an Al3Y intermediate phase in the alloy, transforming the coarse dendritic α-Al grains into fine equiaxed grains, while Mn atoms can increase the melting point of the iron-rich phase, forming a large number of iron-rich phase particles and becoming the heterogeneous nucleation core of α-Al, and coordinating with Y to refine and modify the coarse dendritic α-Al grains. On the other hand, Ba can transform the coarse needle-shaped eutectic silicon into fine particles and short rod-shaped eutectic silicon, and evenly distribute it in the aluminum-silicon alloy. At the same time, Y is adsorbed on the growth interface of the needle-shaped eutectic silicon, hindering the preferential growth of eutectic silicon. The two elements jointly modify and refine the eutectic silicon. Moreover, any one of the three elements Mn, Y, and Ba (and the intermediate phase formed in the high-iron aluminum-silicon alloy) in the high-iron aluminum-silicon alloy will not have an adverse effect on the refinement and modification of the other two elements (and the intermediate phase formed in the high-iron aluminum-silicon alloy), nor will it interact with other elements in the high-iron aluminum-silicon alloy to produce an adverse effect on the refinement and modification of the other two elements.
[0042] The inventors also found in the study that when a composition range of 5%-9% by mass of Mn, 1%-4% by mass of Y, and 0.2%-0.6% by mass of Ba is used, the composite refining modifier has the most significant comprehensive effect on the synergistic refining and modification of α-Al, eutectic silicon, and iron-rich phases in the high-iron aluminum-silicon alloy.
[0043] In addition, the composite refining and modifying agent provided in this embodiment does not contain Ti element in the refining and modifying elements, thereby avoiding the problem of "Si poisoning" between Ti element and Si atoms in the high-iron aluminum-silicon alloy and the inability to effectively refine the α-Al grains; in addition, the refining and modifying elements also do not contain Sr element which can be used as a eutectic silicon modifier, thereby avoiding the pore defects caused by Sr element absorption.
[0044] In summary, the composite refining modifier of the present embodiment can simultaneously achieve the refinement and modification of the α-Al grains, eutectic silicon and iron-rich phase of the high-iron aluminum-silicon alloy, effectively eliminate the harm of coarse dendritic α-Al grains, needle-like eutectic silicon and iron-rich phase to its mechanical properties, improve the strength and plasticity of the high-iron aluminum-silicon alloy, broaden the application range of the high-iron aluminum-silicon alloy, and is particularly suitable for the composite refining and modification treatment of aluminum-silicon alloys with high iron content, and has the advantages of high efficiency and stability, no "Si poisoning" phenomenon, and no air absorption tendency.
[0045] Optionally, the composite refining modifier consists of an α-Al matrix and Al6Mn, Al3Y and Al4Ba intermediate phase particles uniformly distributed in the α-Al matrix.
[0046] Among them, the α-Al matrix, as the main component, provides basic structural support, while the Al6Mn, Al3Y and Al4Ba intermediate phase particles are evenly distributed in the matrix, which plays a role in refining the modified α-Al, eutectic silicon and β-iron-rich phase. By forming a more uniform microstructure in the alloy, it helps to refine the grains and eutectic phases and improve the mechanical properties and comprehensive properties of the alloy.
[0047] Optionally, the composite refining modifier includes, by mass percentage: Mn 7%, Y 3%, Ba 0.4%, and the balance is Al and unavoidable impurity elements. That is, the chemical composition of the composite refining modifier is: Al-7Mn-3Y-0.4Ba.
[0048] In this optional embodiment, when the mass fractions of Mn, Y, and Ba are further determined to be the above-mentioned values, the synergistic refining and metamorphic effect of these components on the α-Al, eutectic silicon, and iron-rich phases in the high iron aluminum silicon alloy is most obvious, which has the effects of further refining the metamorphic microstructure, improving strength and wear resistance, improving thermal stability, and improving processing performance, so that the alloy has better comprehensive performance and application potential.
[0049] See also Figure 1 As shown, a method for preparing a composite fine modifier provided by an embodiment of the present invention comprises:
[0050] According to the composition ratio of the composite refining modifier as described above, aluminum ingots, Al-Mn master alloys, Al-Ba master alloys and Al-Y master alloys are weighed respectively;
[0051] heating and melting the aluminum ingot to obtain an Al melt;
[0052] Adding the Al-Mn master alloy, the Al-Ba master alloy and the Al-Y master alloy to the Al melt in sequence to obtain an Al-Mn-Y-Ba uniform melt;
[0053] A refining agent is added to the Al-Mn-Y-Ba uniform melt, and the melt is cast into an ingot to obtain a composite refining modifier.
[0054] In this embodiment, various master alloys are weighed according to the above ratio to achieve accurate control of various elemental components of the composite refining modifier, ensure that the content of each element in the alloy meets the design requirements, and the alloy raw materials used to provide each elemental component are highly safe and non-toxic. Then, after the aluminum ingot is heated and melted, Al-Mn, Al-Ba, and Al-Y master alloys are added to the melt in sequence to fully mix the various elements to form a uniform Al-Mn-Y-Ba melt, which is conducive to stabilizing the distribution of alloy components and improving the stability and consistency of the alloy. Finally, by adding a refining agent during the preparation process, it plays a role in degassing and slag removal, purifying the aluminum melt, and avoiding the harm to the performance of the high-iron aluminum-silicon alloy by carrying gas and slag into the high-iron aluminum-silicon alloy through the composite refining modifier. In addition, the composite refining modifier of this embodiment has a simple preparation process, low production cost, and safe and pollution-free production and use process, which is very conducive to industrial application.
[0055] Optionally, the Al-Mn master alloy, the Al-Ba master alloy and the Al-Y master alloy are sequentially added to the Al melt to obtain an Al-Mn-Y-Ba uniform melt, comprising:
[0056] The Al melt is controlled at a first temperature, and the Al-Mn master alloy is added to the Al melt, and the mixture is stirred and kept warm at the first temperature, and scum is removed to obtain a uniform Al-Mn melt;
[0057] Adding the Al-Ba master alloy to the Al-Mn homogeneous melt, and stirring the mixture under the first temperature to obtain an Al-Mn-Ba homogeneous melt;
[0058] The Al-Mn-Ba homogeneous melt is cooled to a second temperature, scum is removed, the Al-Y master alloy is added to the Al-Mn-Ba homogeneous melt, the mixture is kept warm and stirred at the second temperature, scum is removed, and the Al-Mn-Y-Ba homogeneous melt is obtained.
[0059] Since the melting points of Al-Mn master alloy and Al-Ba master alloy are higher than those of Al-Y master alloy, in this embodiment, the high melting point Al-Mn master alloy and Al-Ba master alloy are first added at a higher first temperature, and then the temperature of the melt is lowered to a second temperature, and then the Al-Y master alloy with a lower melting point is added to ensure that each raw material is completely melted and evenly distributed in the melt. In addition, when adding materials, the scum on the surface of the melt may be brought into the melt, increasing the content of oxidized slag in the melt. In order to solve this problem, in this embodiment, after each raw material is added, the scum is removed after being kept warm and stirred evenly, thus avoiding the problem of bringing the scum on the surface of the melt into the melt after each raw material is added, thereby reducing the content of oxidized slag in the melt. At the same time, since the temperature gradually decreases with the melting process, the gas content of the melt will also gradually decrease, shortening the melting time, improving efficiency, and reducing energy consumption, which is convenient for the final casting and molding. In addition, the preparation process is simple, easy to operate, and has a low preparation cost, which is conducive to industrial large-scale production.
[0060] Optionally, the first temperature is 830°C-860°C.
[0061] Within this temperature range, the aluminum-manganese master alloy used can be quickly and evenly melted in the aluminum melt, while the temperature will not be too high to cause a sharp increase in the gas and slag content of the melt, thus saving energy.
[0062] Optionally, the second temperature is 730°C-760°C.
[0063] In this optional embodiment, the temperature of the Al-Mn-Ba uniform melt is lowered to 730°C-760°C before adding the Al-Y master alloy, which is slightly higher than the melting point of the aluminum-yttrium master alloy added later, thereby ensuring that the aluminum-yttrium master alloy can be melted uniformly. In addition, since the gas content decreases with temperature, lowering the temperature to this level also further reduces the gas content of the melt, saving energy.
[0064] Optionally, a refining agent is added to the Al-Mn-Y-Ba uniform melt and cast into an ingot to obtain a composite refining modifier, comprising:
[0065] A refining agent is added to the Al-Mn-Y-Ba uniform melt, and the mixture is stirred and kept warm at the second temperature. After standing, the scum is removed, and the mixture is cooled to a third temperature, cast into an ingot, and cooled to room temperature to obtain the composite refining modifier.
[0066] After adding the refining agent, the melt is maintained at the second temperature and stirred evenly, and then allowed to stand (e.g., 10-15 minutes) to allow the gas and slag in the melt sufficient time to float and sink to the maximum extent, thereby reducing the gas content and slag inclusion amount in the melt.
[0067] Optionally, the third temperature is 700°C-720°C.
[0068] The Al-Mn-Y-Ba melt is poured into an ingot at this temperature, which not only ensures good flow and filling properties, but also makes the structure uniform and fine after solidification. Due to the inheritance of the structure (that is, the microstructure and morphological characteristics in the alloy will maintain a certain stability and consistency after the alloy solidifies), adding it to the high-iron aluminum-silicon alloy melt will make the high-iron aluminum-silicon alloy structure after solidification more uniform and fine. At the same time, adding a refining modifier with uniform and fine structure to the melt helps to distribute it more quickly and evenly in the aluminum alloy melt.
[0069] Optionally, the time of heat preservation and stirring at the first temperature and the second temperature is 15 min-30 min.
[0070] The stirring time is designed to be within the above range to ensure uniform mixing of the ingredients while also avoiding too long a time.
[0071] Optionally, the aluminum ingot is heated and melted at a temperature of 680°C-710°C.
[0072] Within the above temperature range, the melting of the aluminum ingot can be ensured, while also shortening the time for subsequently heating the melt from the melting temperature to a high temperature of 830°C-860°C, thereby reducing the amount of slag produced by the aluminum melt during air absorption.
[0073] Optionally, the Al-Mn master alloy, the Al-Ba master alloy and the Al-Y master alloy are all preheated before being added into the Al melt. Preferably, the preheating temperature is 300° C.-400° C., and the preheating time is 1 h-1.5 h.
[0074] The above three kinds of master alloy raw materials are all preheated before being added into the melt. On the one hand, the surface moisture can be removed to prevent the moisture from forming gas inclusions in the melt. On the other hand, the time for uniform melting can be greatly shortened, that is, the time for the aluminum melt to absorb gas and produce slag can be shortened, while avoiding a sharp drop in the temperature of the aluminum melt.
[0075] Optionally, the content of Mn in the Al-Mn master alloy is 5wt.%-20wt.%, the content of Y in the Al-Y master alloy is 5wt.%-10wt.%, and the content of Ba in the Al-Ba master alloy is 5wt.%-10wt.%.
[0076] The Al-Mn master alloy containing the above-mentioned Mn content can improve the strength and hardness of the aluminum alloy, and can also improve the casting properties of the aluminum alloy, such as fluidity and solidification, and the appropriate Mn content can also improve the wear resistance and corrosion resistance of the alloy. The Al-Y master alloy containing the above-mentioned Y content can effectively refine the grains of the aluminum alloy, improve the strength and plasticity of the alloy, and improve the performance of the aluminum alloy at high temperatures, so that it has better thermal stability and thermal expansion properties. The Al-Ba master alloy containing the above-mentioned Ba content can improve the casting properties of the aluminum alloy, reduce the formation of pores and inclusions, improve the surface quality of the casting, and promote the dispersion and dissolution of other elements in the alloy, so that the alloy composition is more uniform, and the stability and consistency of the alloy are improved. In addition, the above-mentioned intermediate alloy raw materials (such as Al-20wt.% Mn alloy, Al-10wt.% Y alloy, Al-10wt.% Ba alloy) have a low melting point and can be melted evenly at a lower temperature, avoiding excessively high temperature melting to increase energy consumption and air absorption; and these raw materials are easy to obtain and relatively low in price, ensuring that the designed composite refining modifier composition can be melted out.
[0077] Optionally, the refining agent is C2Cl6, and the amount of the refining agent added is 0.2%-0.5% of the mass of the Al-Mn-Y-Ba uniform melt.
[0078] C2Cl6 is added to the melt as a refining agent to promote grain refinement, improve the grain structure of aluminum alloy and enhance its mechanical properties. C2Cl6 can remove oxides and other impurities in the aluminum alloy melt, reduce oxidizing gases, reduce the generation of gas and pores, and help improve the purity and density of aluminum alloys, improve quality and reduce defects. In addition, this refining agent does not produce harmful gases during the production process, has weak corrosion to equipment, and is easy to store and use.
[0079] The embodiment of the present invention provides a composite refinement and modification method of a high iron aluminum silicon alloy, comprising:
[0080] The high iron aluminum silicon alloy raw material is heated and melted, and the scum is removed to obtain the high iron aluminum silicon alloy liquid;
[0081] Adding the composite refining modifier as described above into the high iron aluminum silicon alloy liquid, keeping the temperature and stirring, to obtain a mixed metal melt;
[0082] A refining agent is added to the mixed metal melt, and nitrogen is introduced into the mixed metal melt at the same time. After standing, the temperature of the mixed metal melt is lowered to a fourth temperature, and a solidification molding process is performed after removing the slag to obtain a high iron aluminum silicon alloy after composite refinement and modification.
[0083] In this embodiment, after the high iron aluminum silicon alloy is melted and the scum is removed, a high iron aluminum silicon alloy liquid is obtained, and then a composite refining modifier is added to improve the grain refining effect of the alloy. During the process of adding the refining agent, nitrogen is introduced into the mixed metal melt to blow away the gas in the melt, effectively reducing the pores, bubbles and gas inclusions in the melt, which is beneficial to improving the density and uniformity of the alloy. At the same time, the introduced nitrogen can also cause the slag inclusions in the melt to float on the surface of the melt, which is convenient for subsequent scum treatment and is beneficial to improving the purity and quality of the alloy. In addition, the method is simple in process, easy to operate, has a good refining and modification effect, optimizes the organization and performance of the high iron aluminum silicon alloy, has a low production cost, and is suitable for industrial large-scale production.
[0084] Optionally, the heating and melting process of the high iron aluminum silicon alloy raw material specifically includes: melting the high iron aluminum silicon alloy raw material at 800℃-850℃, keeping warm for 30min-60min after being completely melted, cooling to 720℃-740℃, removing slag, and obtaining high iron aluminum silicon alloy liquid.
[0085] In this embodiment, the high iron aluminum silicon alloy raw material is melted at 800℃-850℃. Under this temperature condition, the hereditary characteristics of the bad organization of the high iron aluminum silicon alloy can be eliminated, the microstructure of the high iron aluminum silicon alloy can be made more uniform, and the defects and unevenness in the organization can be reduced. When the high iron aluminum silicon alloy raw material is completely melted, it is kept warm for 30min-60min under the above temperature conditions to eliminate the bad organization hereditary characteristics of the high iron aluminum silicon alloy to the greatest extent. Thereafter, the melt after insulation is cooled to 720℃-740℃, and the high iron aluminum silicon alloy liquid is obtained after removing the scum. It can be understood that 720℃-740℃ is the lowest temperature range to ensure that the composite refining modifier added later can be quickly melted and evenly.
[0086] Optionally, the added amount of the composite refining modifier is 0.2%-0.8% of the mass of the high iron aluminum silicon alloy liquid.
[0087] Controlling the amount of the composite refining and modifying agent added within the above range not only ensures a significant refining and modifying effect, but also avoids the problem of increased costs due to excessive addition.
[0088] Optionally, nitrogen is introduced into the mixed metal melt for 10 min to 15 min, and then the mixed metal melt is allowed to stand for 10 min to 15 min.
[0089] In this optional embodiment, the nitrogen introduction time is controlled to be 10-15 minutes, so that the nitrogen can fully contact with the aluminum melt, contact with the gas and slag in the melt to the greatest extent and adsorb the gas and slag. In addition, after the nitrogen is introduced for a certain period of time, it is also left to stand for 10-15 minutes. This period of time allows the nitrogen bubbles that adsorb the gas and slag to fully float and escape to the surface of the melt, which is conducive to removing the gas and slag.
[0090] Optionally, the nitrogen gas has an inlet flow rate of 1 L / min-2 L / min.
[0091] In this optional embodiment, the nitrogen flow rate is controlled within this range to generate finely dispersed nitrogen bubbles, which are in full contact with the aluminum alloy melt. While fully adsorbing gas and slag inclusions to purify the aluminum melt, the surface of the aluminum liquid will not be violently fluctuated and introduced into the melt due to the introduction of gas and slag inclusions.
[0092] Optionally, the fourth temperature is 690°C-710°C.
[0093] The high iron aluminum silicon alloy melt after adding the composite refining modifier is poured within this temperature range, which not only ensures good flow and filling properties, but also makes the structure after solidification more uniform and fine, further improving the mechanical properties of the alloy.
[0094] Optionally, the solidification molding process is to pour the melt into a metal mold, and obtain a high iron aluminum silicon alloy after composite refinement and modification after cooling.
[0095] An embodiment of the present invention further provides a high iron aluminum silicon alloy, wherein the high iron aluminum silicon alloy uses the composite refining modifier as described above during the refining and modification process, or the high iron aluminum silicon alloy is made by the composite refining and modification method of the high iron aluminum silicon alloy as described above.
[0096] Adding a small amount of the Al-Mn-Y-Ba composite refining modifier prepared above to the high iron aluminum silicon alloy can simultaneously refine and modify the α-Al grains, eutectic silicon and iron-rich phase in the high iron aluminum silicon alloy, effectively eliminate the hazards of coarse dendritic α-Al grains, needle-shaped eutectic silicon and iron-rich phase, and there is no "Si poisoning phenomenon" and no gas absorption tendency, which can synergistically improve the strength and plastic toughness of the high iron aluminum silicon alloy. In addition, the production process of the high iron aluminum silicon alloy does not emit toxic and harmful substances, which is conducive to the recycling and high-value application of the recycled high iron aluminum silicon alloy, and has high value for industrial promotion and application.
[0097] The present invention is further described below in conjunction with specific examples. If no specific conditions are specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0098] Example 1
[0099] This embodiment first provides a composite refining modifier, whose mass percentage composition is: Mn 8%, Y 4%, Ba 0.3%, and the balance is Al and unavoidable impurity elements, wherein the single content of the impurity element is ≤0.05%, and the total content is ≤0.15%.
[0100] This embodiment also provides a method for preparing the above-mentioned composite refinement modifier, which comprises the following steps:
[0101] (1) According to the above-mentioned composition ratio, aluminum ingots, Al-Mn master alloys, Al-Ba master alloys and Al-Y master alloys are weighed respectively. The purity of the aluminum ingots is ≥99.8wt.%, the Al-Mn master alloy is an Al-20wt.%Mn alloy, the Al-Y master alloy is an Al-10wt.%Y alloy, and the Al-Ba master alloy is an Al-10wt.%Ba alloy;
[0102] (2) The weighed aluminum ingot is put into a smelting furnace to melt to obtain an Al melt, the melting temperature of the smelting furnace is 680°C, then the temperature is raised to 850°C, Al-Mn master alloy is added to the Al melt, the mixture is kept warm and stirred evenly for 20 minutes, and the scum is removed to obtain an Al-Mn uniform melt, then Al-Ba master alloy is added to the Al-Mn uniform melt, the mixture is kept warm and stirred evenly for 20 minutes, and the Al-Mn-Ba uniform melt is obtained, the mixture is left to cool to 740°C, the scum is removed, and Al-Y master alloy is added to the Al-Mn-Ba uniform melt, the mixture is kept warm and stirred evenly for 20 minutes, and the scum is removed to obtain an Al-Mn-Y-Ba uniform melt. Wherein, the Al-Mn master alloy, the Al-Y master alloy and the Al-Ba master alloy are all preheated in a resistance furnace before being added to the melt, and the preheating temperature is 350°C and the preheating time is 1 hour.
[0103] (3) Adding a refining agent C2Cl6 to the Al-Mn-Y-Ba uniform melt in an amount of 0.3% of the mass of the Al-Mn-Y-Ba uniform melt, stirring the melt for 20 minutes to mix the melt evenly, letting it stand for 10 minutes, removing the scum, cooling the melt to 720°C, casting the melt into an ingot, and demolding the melt after cooling to room temperature to obtain a composite refining modifier.
[0104] This embodiment also provides an application of the above-mentioned composite refining modifier, where the composite refining modifier is added to a high iron aluminum silicon alloy. The chemical composition of the selected high iron aluminum silicon alloy is shown in Table 1.
[0105] Table 1: Chemical composition of high iron aluminum silicon alloy (wt.%)
[0106] element Si Fe Cu Mn Mg Ti other Al Element 11.13 1.36 0.36 0.02 0.29 0.16 ≤0.15 margin
[0107] A composite refinement and modification method for a high iron aluminum silicon alloy comprises the following steps:
[0108] The high iron aluminum silicon alloy raw material is melted at 840°C, kept warm for 40 minutes after being completely melted, cooled to 725°C, and the scum is removed to obtain a high iron aluminum silicon alloy liquid;
[0109] Add the composite refining modifier to the high iron aluminum silicon alloy liquid, keep warm and stir evenly to obtain a mixed metal melt, wherein the amount of the composite refining modifier added is 0.5% of the mass of the high iron aluminum silicon alloy liquid;
[0110] A refining agent was added to the above-mentioned mixed metal melt, and nitrogen was introduced into the mixed metal melt for 10 minutes at a nitrogen flow rate of 1 L / min. The mixed metal melt was then allowed to stand for 15 minutes, the temperature was reduced to 700°C, the slag was removed, the melt was poured into a metal mold, and it was cooled to room temperature to obtain a high iron aluminum silicon alloy after composite refinement and modification.
[0111] Example 2
[0112] This embodiment first provides a composite refining modifier, whose mass percentage composition is: Mn 5%, Y 1%, Ba 0.2%, and the balance is Al and unavoidable impurity elements, wherein the single content of the impurity element is ≤0.05%, and the total content is ≤0.15%.
[0113] This embodiment also provides a method for preparing the above-mentioned composite refinement modifier, which comprises the following steps:
[0114] (1) According to the above-mentioned composition ratio, aluminum ingots, Al-Mn master alloys, Al-Ba master alloys and Al-Y master alloys are weighed respectively. The purity of the aluminum ingots is ≥99.8wt.%, the Al-Mn master alloy is an Al-20wt.%Mn alloy, the Al-Y master alloy is an Al-10wt.%Y alloy, and the Al-Ba master alloy is an Al-10wt.%Ba alloy;
[0115] (2) The weighed aluminum ingot is put into a smelting furnace to melt to obtain an Al melt, the melting temperature of the smelting furnace is 690°C, and then the temperature is raised to 830°C, and Al-Mn master alloy is added to the Al melt, and the mixture is stirred evenly at the temperature for 25 minutes, and scum is removed to obtain an Al-Mn uniform melt, and then Al-Ba master alloy is added to the Al-Mn uniform melt, and the mixture is stirred evenly at the temperature for 25 minutes, and Al-Mn-Ba uniform melt is obtained, and the mixture is allowed to stand and cool to 730°C, and scum is removed, and Al-Y master alloy is added to the Al-Mn-Ba uniform melt, and the mixture is stirred evenly at the temperature for 25 minutes, and scum is removed to obtain an Al-Mn-Y-Ba uniform melt, and the Al-Mn master alloy, Al-Y master alloy and Al-Ba master alloy are all preheated in a resistance furnace before being added to the melt, and the preheating temperature is 300°C and the preheating time is 1.5 hours.
[0116] (3) Adding a refining agent C2Cl6 to the Al-Mn-Y-Ba uniform melt in an amount of 0.5% of the mass of the Al-Mn-Y-Ba uniform melt, stirring the melt for 25 minutes to mix the melt evenly, standing the melt for 12 minutes, removing the scum, cooling the melt to 710°C, casting the melt into an ingot, and demolding the melt after cooling to room temperature to obtain a composite refining modifier.
[0117] This embodiment also provides an application of the above-mentioned composite refining modifier, which is added to the high iron aluminum silicon alloy shown in Table 1. The composite refining modifier method of the high iron aluminum silicon alloy specifically includes the following steps:
[0118] The high iron aluminum silicon alloy raw material is melted at 810°C, kept warm for 60 minutes after being completely melted, cooled to 740°C, and the scum is removed to obtain a high iron aluminum silicon alloy liquid;
[0119] Add the composite refining modifier to the high iron aluminum silicon alloy liquid, keep warm and stir evenly to obtain a mixed metal melt, wherein the amount of the composite refining modifier added is 0.7% of the mass of the high iron aluminum silicon alloy liquid;
[0120] A refining agent was added to the above-mentioned mixed metal melt, and nitrogen was introduced into the mixed metal melt for 13 minutes at a nitrogen flow rate of 1.5 L / min. The mixed metal melt was then allowed to stand for 11 minutes, the temperature was reduced to 690°C, the slag was removed, the melt was poured into a metal mold, and the mixture was cooled to room temperature to obtain a high-iron aluminum-silicon alloy after composite refinement and metamorphism.
[0121] Example 3
[0122] This embodiment first provides a composite refining modifier, whose mass percentage composition is: Mn 7%, Y 3%, Ba 0.4%, and the balance is Al and unavoidable impurity elements, wherein the single content of the impurity elements is ≤0.05%, and the total content is ≤0.15%.
[0123] This embodiment also provides a method for preparing the above-mentioned composite refinement modifier, which comprises the following steps:
[0124] (1) According to the above-mentioned composition ratio, aluminum ingot, Al-Mn master alloy, Al-Ba master alloy and Al-Y master alloy are weighed respectively. The purity of the aluminum ingot is ≥99.8wt.%, the Al-Mn master alloy is Al-20wt.%Mn alloy, the Al-Y master alloy is Al-10wt.%Y alloy, and the Al-Ba master alloy is Al-10wt.%Ba alloy;
[0125] (2) The weighed aluminum ingot is put into a smelting furnace to melt to obtain an Al melt. The melting temperature of the smelting furnace is 710°C. Then, the temperature is raised to 860°C. Al-Mn master alloy is added to the Al melt. The mixture is kept warm and stirred for 30 minutes. The scum is removed to obtain an Al-Mn uniform melt. Al-Ba master alloy is added to the Al-Mn uniform melt. The mixture is kept warm and stirred for 30 minutes. The Al-Mn-Ba uniform melt is obtained. The mixture is allowed to stand and cooled to 740°C. The scum is removed. Al-Y master alloy is added to the Al-Mn-Ba uniform melt. The mixture is kept warm and stirred for 30 minutes. The scum is removed to obtain an Al-Mn-Y-Ba uniform melt. The Al-Mn master alloy, the Al-Y master alloy and the Al-Ba master alloy are all preheated in a resistance furnace before being added to the melt. The preheating temperature is 400°C and the preheating time is 1 hour.
[0126] (3) Adding a refining agent C2Cl6 to the Al-Mn-Y-Ba uniform melt in an amount of 0.4% of the mass of the Al-Mn-Y-Ba uniform melt, stirring the melt for 30 minutes to mix the melt evenly, standing the melt for 14 minutes, removing the scum, cooling the melt to 720°C, casting the melt into an ingot, and demolding the melt after cooling to room temperature to obtain a composite refining modifier.
[0127] This embodiment also provides the application of the above-mentioned composite refining modifier, and the composite refining modifier is added to the high iron aluminum silicon alloy shown in Table 1. The composite refining modifier method of the high iron aluminum silicon alloy specifically includes the following steps:
[0128] The high iron aluminum silicon alloy raw material is melted at 830°C, kept warm for 60 minutes after being completely melted, cooled to 730°C, and the scum is removed to obtain a high iron aluminum silicon alloy liquid;
[0129] Add the composite refining modifier to the high iron aluminum silicon alloy liquid, keep warm and stir evenly to obtain a mixed metal melt, wherein the amount of the composite refining modifier added is 0.8% of the mass of the high iron aluminum silicon alloy liquid;
[0130] A refining agent was added to the above-mentioned mixed metal melt, and nitrogen was introduced into the mixed metal melt for 15 minutes at a nitrogen flow rate of 1.5 L / min. The mixed metal melt was then allowed to stand for 13 minutes, the temperature was reduced to 700°C, the slag was removed, the melt was poured into a metal mold, and cooled to room temperature to obtain a high-iron aluminum-silicon alloy after composite refinement and modification.
[0131] Example 4
[0132] This embodiment first provides a composite refining modifier, whose mass percentage composition is: Mn 9%, Y 3%, Ba 0.6%, and the balance is Al and unavoidable impurity elements, wherein the single content of the impurity element is ≤0.05%, and the total content is ≤0.15%.
[0133] This embodiment also provides a method for preparing the above-mentioned composite refinement modifier, which comprises the following steps:
[0134] (1) According to the above-mentioned composition ratio, aluminum ingot, Al-Mn master alloy, Al-Ba master alloy and Al-Y master alloy are weighed respectively. The purity of the aluminum ingot is ≥99.8wt.%, the Al-Mn master alloy is Al-20wt.%Mn alloy, the Al-Y master alloy is Al-10wt.%Y alloy, and the Al-Ba master alloy is Al-10wt.%Ba alloy;
[0135] (2) The weighed aluminum ingot is put into a smelting furnace to melt to obtain an Al melt. The melting temperature of the smelting furnace is 710°C. Then, the temperature is raised to 860°C. Al-Mn master alloy is added to the Al melt. The mixture is kept warm and stirred for 30 minutes. The scum is removed to obtain an Al-Mn uniform melt. Al-Ba master alloy is added to the Al-Mn uniform melt. The mixture is kept warm and stirred for 30 minutes. The Al-Mn-Ba uniform melt is obtained. The mixture is allowed to stand and cooled to 740°C. The scum is removed. Al-Y master alloy is added to the Al-Mn-Ba uniform melt. The mixture is kept warm and stirred for 30 minutes. The scum is removed to obtain an Al-Mn-Y-Ba uniform melt. The Al-Mn master alloy, the Al-Y master alloy and the Al-Ba master alloy are all preheated in a resistance furnace before being added to the melt. The preheating temperature is 400°C and the preheating time is 1 hour.
[0136] (3) Adding a refining agent C2Cl6 to the Al-Mn-Y-Ba uniform melt in an amount of 0.4% of the mass of the Al-Mn-Y-Ba uniform melt, stirring the melt for 30 minutes to mix the melt evenly, standing the melt for 14 minutes, removing the scum, cooling the melt to 720°C, casting the melt into an ingot, and demolding the melt after cooling to room temperature to obtain a composite refining modifier.
[0137] This embodiment also provides the application of the above-mentioned composite refining modifier, and the composite refining modifier is added to the high iron aluminum silicon alloy shown in Table 1. The composite refining modifier method of the high iron aluminum silicon alloy specifically includes the following steps:
[0138] The high iron aluminum silicon alloy raw material is melted at 830°C, kept warm for 60 minutes after being completely melted, cooled to 730°C, and the scum is removed to obtain a high iron aluminum silicon alloy liquid;
[0139] Add the composite refining modifier to the high iron aluminum silicon alloy liquid, keep warm and stir evenly to obtain a mixed metal melt, wherein the amount of the composite refining modifier added is 0.8% of the mass of the high iron aluminum silicon alloy liquid;
[0140] A refining agent was added to the above-mentioned mixed metal melt, and nitrogen was introduced into the mixed metal melt for 15 minutes at a nitrogen flow rate of 1.5 L / min. The mixed metal melt was then allowed to stand for 13 minutes, the temperature was reduced to 700°C, the slag was removed, the melt was poured into a metal mold, and cooled to room temperature to obtain a high-iron aluminum-silicon alloy after composite refinement and modification.
[0141] Comparative Example 1
[0142] This comparative example first provides a composite refining modifier, whose mass percentage composition is: Mn 7%, Y 3%, and the balance is Al and unavoidable impurity elements, wherein the single content of the impurity elements is ≤0.05%, and the total content is ≤0.15%.
[0143] This comparative example also provides a method for preparing the above-mentioned composite refinement modifier, which comprises the following steps:
[0144] (1) According to the above-mentioned composition ratio, aluminum ingot, Al-Mn master alloy and Al-Y master alloy are weighed respectively. The purity of the aluminum ingot is ≥99.8wt.%, the Al-Mn master alloy is Al-20wt.%Mn alloy, and the Al-Y master alloy is Al-10wt.%Y alloy;
[0145] (2) The weighed aluminum ingot is put into a smelting furnace to melt to obtain an Al melt, the melting temperature of the smelting furnace is 710°C, and then the temperature is raised to 860°C, and Al-Mn master alloy is added to the Al melt, and the mixture is stirred evenly at the temperature for 30 minutes. The mixture is allowed to stand and cooled to 740°C, and scum is removed to obtain an Al-Mn uniform melt. Al-Y master alloy is then added to the Al-Mn uniform melt, and the mixture is stirred evenly at the temperature for 30 minutes. Scum is removed to obtain an Al-Mn-Y uniform melt. Before being added to the melt, the Al-Mn master alloy and the Al-Y master alloy are preheated in a resistance furnace at a preheating temperature of 400°C for 1 hour.
[0146] (3) Adding a refining agent C2Cl6 to the Al-Mn-Y uniform melt in an amount of 0.4% of the mass of the Al-Mn-Y uniform melt, stirring the melt for 30 minutes to mix the melt evenly, standing the melt for 14 minutes, removing the scum, cooling the melt to 720°C, casting the melt into an ingot, and demolding the melt after cooling to room temperature to obtain a composite refining modifier.
[0147] This comparative example also provides the application of the above-mentioned composite refining modifier, and the composite refining modifier is added to the high iron aluminum silicon alloy shown in Table 1. The composite refining modifier method of the high iron aluminum silicon alloy specifically includes the following steps:
[0148] The high iron aluminum silicon alloy raw material is melted at 830°C, kept warm for 60 minutes after being completely melted, cooled to 730°C, and the scum is removed to obtain a high iron aluminum silicon alloy liquid;
[0149] Add the composite refining modifier to the high iron aluminum silicon alloy liquid, keep warm and stir evenly to obtain a mixed metal melt, wherein the amount of the composite refining modifier added is 0.8% of the mass of the high iron aluminum silicon alloy liquid;
[0150] A refining agent was added to the above-mentioned mixed metal melt, and nitrogen was introduced into the mixed metal melt for 15 minutes at a nitrogen flow rate of 1.5 L / min. The mixed metal melt was then allowed to stand for 13 minutes, the temperature was reduced to 700°C, the slag was removed, the melt was poured into a metal mold, and cooled to room temperature to obtain a high-iron aluminum-silicon alloy after composite refinement and modification.
[0151] Comparative Example 2
[0152] This comparative example first provides a composite refining modifier, whose mass percentage composition is: Mn 7%, Ba 0.4%, and the balance is Al and inevitable impurity elements, wherein the single content of the impurity elements is ≤0.05%, and the total content is ≤0.15%.
[0153] This comparative example also provides a method for preparing the above-mentioned composite refinement modifier, which comprises the following steps:
[0154] (1) According to the above-mentioned composition ratio, aluminum ingot, Al-Mn master alloy and Al-Ba master alloy are weighed respectively. The purity of the aluminum ingot is ≥99.8wt.%, the Al-Mn master alloy is Al-20wt.%Mn alloy, and the Al-Ba master alloy is Al-10wt.%Ba alloy;
[0155] (2) The weighed aluminum ingot is put into a smelting furnace to melt to obtain an Al melt, the melting temperature of the smelting furnace is 710°C, then the temperature is raised to 860°C, Al-Mn master alloy is added to the Al melt, the mixture is kept warm and stirred evenly for 30 minutes, and the scum is removed to obtain an Al-Mn uniform melt, then Al-Ba master alloy is added to the Al-Mn uniform melt, the mixture is kept warm and stirred evenly for 30 minutes, and the Al-Mn-Ba uniform melt is obtained, the mixture is left to cool to 740°C, and the scum is removed. Before adding the Al-Mn master alloy and the Al-Ba master alloy to the melt, they are both preheated in a resistance furnace at a preheating temperature of 400°C and a preheating time of 1 hour.
[0156] (3) Adding a refining agent C2Cl6 to the Al-Mn-Ba uniform melt in an amount of 0.4% of the mass of the Al-Mn-Ba uniform melt, stirring the melt for 30 minutes to mix the melt evenly, standing the melt for 14 minutes, removing the scum, cooling the melt to 720°C, casting the melt into an ingot, and demolding the melt after cooling to room temperature to obtain a composite refining modifier.
[0157] This comparative example also provides the application of the above-mentioned composite refining modifier, and the composite refining modifier is added to the high iron aluminum silicon alloy shown in Table 1. The composite refining modifier method of the high iron aluminum silicon alloy specifically includes the following steps:
[0158] The high iron aluminum silicon alloy raw material is melted at 830°C, kept warm for 60 minutes after being completely melted, cooled to 730°C, and the scum is removed to obtain a high iron aluminum silicon alloy liquid;
[0159] Add the composite refining modifier to the high iron aluminum silicon alloy liquid, keep warm and stir evenly to obtain a mixed metal melt, wherein the amount of the composite refining modifier added is 0.8% of the mass of the high iron aluminum silicon alloy liquid;
[0160] A refining agent was added to the above-mentioned mixed metal melt, and nitrogen was introduced into the mixed metal melt for 15 minutes at a nitrogen flow rate of 1.5 L / min. The mixed metal melt was then allowed to stand for 13 minutes, the temperature was reduced to 700°C, the slag was removed, the melt was poured into a metal mold, and cooled to room temperature to obtain a high-iron aluminum-silicon alloy after composite refinement and modification.
[0161] Comparative Example 3
[0162] This comparative example first provides a composite refining modifier, whose mass percentage composition is: Y 3%, Ba 0.4%, and the balance is Al and unavoidable impurity elements, wherein the single content of the impurity elements is ≤0.05%, and the total content is ≤0.15%.
[0163] This comparative example also provides a method for preparing the above-mentioned composite refinement modifier, which comprises the following steps:
[0164] (1) According to the above-mentioned composition ratio, weigh aluminum ingot, Al-Y master alloy and Al-Ba master alloy respectively. The purity of the aluminum ingot is ≥99.8wt.%, the Al-Y master alloy is Al-10wt.%Y alloy, and the Al-Ba master alloy is Al-10wt.%Ba alloy;
[0165] (2) The weighed aluminum ingot is put into a smelting furnace to melt to obtain an Al melt. The melting temperature of the smelting furnace is 710°C. Then, the temperature is raised to 860°C. Al-Ba master alloy is added to the Al melt. The mixture is kept warm and stirred for 30 minutes to obtain an Al-Ba uniform melt. The mixture is allowed to stand and cool to 740°C. The scum is removed. Al-Y master alloy is added to the Al-Ba uniform melt. The mixture is kept warm and stirred for 30 minutes. The scum is removed to obtain an Al-Y-Ba uniform melt. The Al-Y master alloy and the Al-Ba master alloy are preheated in a resistance furnace before being added to the melt. The preheating temperature is 400°C and the preheating time is 1 hour.
[0166] (3) Adding a refining agent C2Cl6 to the Al-Y-Ba uniform melt in an amount of 0.4% of the mass of the Al-Y-Ba uniform melt, stirring the melt for 30 minutes to mix the melt evenly, standing the melt for 14 minutes, removing the scum, cooling the melt to 720°C, casting the melt into an ingot, and demolding the melt after cooling to room temperature to obtain a composite refining modifier.
[0167] This comparative example also provides the application of the above-mentioned composite refining modifier, and the composite refining modifier is added to the high iron aluminum silicon alloy shown in Table 1. The composite refining modifier method of the high iron aluminum silicon alloy specifically includes the following steps:
[0168] The high iron aluminum silicon alloy raw material is melted at 830°C, kept warm for 60 minutes after being completely melted, cooled to 730°C, and the scum is removed to obtain a high iron aluminum silicon alloy liquid;
[0169] Add the composite refining modifier to the high iron aluminum silicon alloy liquid, keep warm and stir evenly to obtain a mixed metal melt, wherein the amount of the composite refining modifier added is 0.8% of the mass of the high iron aluminum silicon alloy liquid;
[0170] A refining agent was added to the above-mentioned mixed metal melt, and nitrogen was introduced into the mixed metal melt for 15 minutes at a nitrogen flow rate of 1.5 L / min. The mixed metal melt was then allowed to stand for 13 minutes, the temperature was reduced to 700°C, the slag was removed, the melt was poured into a metal mold, and cooled to room temperature to obtain a high-iron aluminum-silicon alloy after composite refinement and modification.
[0171] Comparative Example 4
[0172] The difference between this comparative example and Example 3 is that no composite refinement modifier is used. The specific steps are as follows:
[0173] The high iron aluminum silicon alloy raw materials shown in Table 1 were melted at 830°C, kept warm for 60 minutes after being completely melted, cooled to 730°C, and the scum was removed to obtain a high iron aluminum silicon alloy melt, which was kept warm and stirred uniformly to obtain a high iron aluminum silicon alloy uniform melt;
[0174] A refining agent was added to the above-mentioned high iron aluminum silicon alloy uniform melt, and nitrogen was introduced into the high iron aluminum silicon alloy uniform melt for 15 minutes at a nitrogen flow rate of 1.5L / min. The melt was then allowed to stand for 13 minutes, the temperature was reduced to 700°C, the slag was removed, the melt was poured into a metal mold, and the mold was cooled to room temperature to obtain a high iron aluminum silicon alloy for comparison.
[0175] Effect Example
[0176] Metallographic samples were taken from the high iron aluminum silicon alloy after composite refinement and modification obtained in Example 1 to Example 4 and the high iron aluminum silicon alloy for comparison obtained in Comparative Example 1 to Comparative Example 4, and the statistical data of the metallographic structure characteristics of the alloy were determined by microscope. The ingots were sampled and processed into standard specimens, and the tensile stress-strain curve of the alloy was tested by a universal mechanical testing machine.
[0177] The statistical data of metallographic structure characteristics of high iron aluminum silicon alloys of comparative examples 1 to 4 and examples 1 to 4 are compared as shown in Figure 2 .Depend on Figure 2 It can be seen that the secondary dendrite spacing of the high iron aluminum silicon alloy obtained in comparative example 4 is larger, indicating that the grains are relatively coarse, while the secondary dendrite spacing of examples 1 to 4 is significantly reduced, indicating that the high iron aluminum silicon alloy obtained after the addition of the composite refining modifier has its grains refined. Figure 2 It can also be seen that the eutectic silicon area of comparative example 4 is the largest, and the eutectic silicon roundness is low, indicating that the eutectic silicon phase is large and the eutectic silicon particles are irregular in shape, while the eutectic silicon area of examples 1 to 4 is small, and the eutectic silicon particles are more regular and rounded, indicating that the eutectic silicon phase has been significantly modified and refined. Figure 2It can also be seen that the length and width of the iron-rich phase in Comparative Example 4 are the largest, while the length and width of the iron-rich phase in Examples 1 to 4 are significantly reduced, indicating that the iron-rich phase particles have also been significantly modified and refined. Figure 2 It can be seen that the composite refining modifier provided in this embodiment can simultaneously and significantly refine the three metallographic structures of α-Al grains, eutectic silicon and iron-rich phase in the modified high-iron aluminum-silicon alloy. Figure 2 It can also be seen that compared with Example 1, Example 2 and Example 4, the secondary dendrite spacing, the length and width of the iron-rich phase and the roundness of eutectic silicon in Example 3 are all smaller, indicating that the high iron aluminum-silicon alloy obtained in Example 3 has the best degree of refinement and modification.
[0178] Comparison of the tensile stress-strain curves of high iron aluminum silicon alloys of Comparative Examples 1-4 and Examples 1-4 is shown in Figure 3 .Depend on Figure 3 It can be seen that the tensile strength of the high iron aluminum silicon alloy obtained in Comparative Example 4 is relatively low, about 250 MPa, while the tensile strengths of Examples 1 to 4 are significantly improved, all exceeding 300 MPa. In addition, the strain rate of the high iron aluminum silicon alloy obtained in Comparative Example 4 is significantly lower than that of Examples 1 to 4.
[0179] In addition, from Figure 2 It can be seen that although the secondary dendrite spacing, eutectic silicon area, eutectic silicon rounding and iron-rich phase length and width of Comparative Examples 1 to 3 are all lower than those of Comparative Example 4 to varying degrees, at least one of the secondary dendrite spacing, eutectic silicon area, eutectic silicon rounding and iron-rich phase length and width is much higher than that of Examples 1 to 4. Figure 3 It can be seen that although the strength and elongation of Comparative Examples 1 to 3 are higher than those of Comparative Example 4, they are much lower than those of Examples 1 to 4 and cannot reach the level of Examples 1 to 4. This shows that the three elements of Mn, Y and Ba have a synergistic metamorphic and refining effect, and none of them can be missing. Only when the three elements work together can the three metallographic structures of α-Al grains, eutectic silicon and iron-rich phase in the high-iron aluminum-silicon alloy be significantly modified and refined at the same time, thereby significantly improving the strength and elongation of the high-iron aluminum-silicon alloy at the same time.
[0180] In summary, through Figure 2 and Figure 3 It can be seen that the composite refining modifier provided in this embodiment can simultaneously and significantly refine the three metallographic structures of α-Al grains, eutectic silicon and iron-rich phase in the modified high-iron aluminum-silicon alloy, thereby simultaneously and significantly improving the tensile strength and elongation of the high-iron aluminum-silicon alloy. Among them, the tensile strength can be increased by more than 20%, and the elongation can be increased by more than 170%.
[0181] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.
Claims
1. A composite refinement modifier, characterized in that: Calculated by mass percentage, it comprises: Mn 5-9%, Y 1-4%, Ba0.2-0.6%, and the balance is Al and inevitable impurity elements.
2. The composite refinement modifier according to claim 1, characterized in that: Calculated by mass percentage, it comprises: Mn 7%, Y 3%, Ba 0.4%, and the balance is Al and inevitable impurity elements.
3. A method for preparing a composite refinement modifier, characterized in that: include: According to the composition ratio of the composite refining modifier according to claim 1 or 2, aluminum ingot, Al-Mn master alloy, Al-Ba master alloy and Al-Y master alloy are weighed respectively; heating and melting the aluminum ingot to obtain an Al melt; Adding the Al-Mn master alloy, the Al-Ba master alloy and the Al-Y master alloy to the Al melt in sequence to obtain an Al-Mn-Y-Ba uniform melt; A refining agent is added to the Al-Mn-Y-Ba uniform melt, and the melt is cast into an ingot to obtain a composite refining modifier.
4. The method for preparing the composite refinement modifier according to claim 3, characterized in that: The Al-Mn master alloy, the Al-Ba master alloy and the Al-Y master alloy are sequentially added into the Al melt to obtain an Al-Mn-Y-Ba uniform melt, comprising: The Al melt is controlled at a first temperature, the Al-Mn master alloy is added to the Al melt, the Al-Mn master alloy is stirred and kept at the first temperature, and scum is removed to obtain a uniform Al-Mn melt; Adding the Al-Ba master alloy to the Al-Mn homogeneous melt, and stirring the mixture under the first temperature to obtain an Al-Mn-Ba homogeneous melt; The Al-Mn-Ba homogeneous melt is cooled to a second temperature, scum is removed, the Al-Y master alloy is added to the Al-Mn-Ba homogeneous melt, the mixture is kept warm and stirred at the second temperature, scum is removed, and the Al-Mn-Y-Ba homogeneous melt is obtained.
5. The method for preparing the composite refinement modifier according to claim 4, characterized in that: Adding a refining agent to the Al-Mn-Y-Ba uniform melt and casting it into an ingot to obtain a composite refining modifier, comprising: A refining agent is added to the Al-Mn-Y-Ba uniform melt, and the mixture is stirred and kept warm at the second temperature. After standing, the scum is removed, and the mixture is cooled to a third temperature, cast into an ingot, and cooled to room temperature to obtain the composite refining modifier.
6. The method for preparing the composite refinement modifier according to claim 3, characterized in that: The Al-Mn master alloy, the Al-Ba master alloy and the Al-Y master alloy are all preheated before being added into the Al melt.
7. The method for preparing the composite refinement modifier according to claim 3, characterized in that: The content of Mn in the Al-Mn master alloy is 5wt.%-20wt.%, the content of Y in the Al-Y master alloy is 5wt.%-10wt.%, and the content of Ba in the Al-Ba master alloy is 5wt.%-10wt.%.
8. A composite refinement and modification method for high iron aluminum silicon alloy, characterized in that: include: The high iron aluminum silicon alloy raw material is heated and melted, and the scum is removed to obtain the high iron aluminum silicon alloy liquid; Adding a composite refining modifier to the high iron aluminum silicon alloy liquid, stirring while keeping warm, to obtain a mixed metal melt; wherein the composite refining modifier is the composite refining modifier according to claim 1 or 2, or is obtained by the preparation method of the composite refining modifier according to any one of claims 3 to 7; A refining agent is added to the mixed metal melt, and nitrogen is introduced into the mixed metal melt at the same time. After standing, the temperature of the mixed metal melt is lowered to a fourth temperature, and a solidification molding process is performed after removing the slag to obtain a high iron aluminum silicon alloy after composite refinement and modification.
9. The composite refinement and modification method of high iron aluminum silicon alloy according to claim 8, characterized in that: The high iron aluminum silicon alloy raw material is heated and melted at 800° C.-850° C.
10. A high iron aluminum silicon alloy, characterized in that: The high iron aluminum silicon alloy uses the composite refining modifier described in claim 1 or 2 during the refining and modification process, or the high iron aluminum silicon alloy is made by the composite refining and modification method of the high iron aluminum silicon alloy described in claim 8 or 9.
Citation Information
Cited By
Aluminum alloy comprehensive alterant and preparation method thereof
CN121294928A