High-aluminum-titanium-nickel-based high-temperature alloy composite powder as well as preparation method and application thereof

Through wet ball milling, the submicron-scale hafnium carbide powder is uniformly dispersed in high-aluminum titanium nickel-based high-temperature alloy powder, solving the problem that high-temperature alloys are prone to microcracks in additive manufacturing, and achieving improvement of material performance and reduction of crack density .

CN118910470APending Publication Date: 2024-11-08XI AN JIAOTONG UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410959642.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

High-aluminum titanium-nickel-based high-temperature alloys are prone to microcracks in additive manufacturing, and existing ceramic reinforced particles cannot be evenly dispersed, affecting material performance.

Method used

Wet ball mill is used to mix submicron-scale hafnium carbide powder with high aluminum titanium nickel-based high-temperature alloy powder. Through wet ball milling process, hafnium carbide particles are evenly dispersed on the nickel-based high-temperature alloy powder sphere to prevent the powder from overheating and deformation, and use hafnium rich The eutectic phase fills the thermal cracks caused by shrinkage.

Benefits of technology

It effectively suppresses cracks in laser selection melting technology of high-aluminum titanium nickel-based high-temperature alloys, improves the tensile strength and elongation of the material, reduces the crack density, and expands the process window.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910470A_ABST
    Figure CN118910470A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of high-temperature alloy and additive manufacturing, in particular to high-aluminum-titanium-nickel-based high-temperature alloy composite powder as well as a preparation method and application thereof. The composite powder is prepared by dispersing reinforced particles on the surface of a matrix in a wet ball milling manner; the strengthening particles are submicron hafnium carbide powder, and the matrix is high-aluminum titanium nickel-based high-temperature alloy powder; and the reinforced particles account for 1-3% of the mass of the composite powder. And the composite powder is placed on a forming cylinder base plate, and under the protective atmosphere, the nickel-based superalloy printing piece is obtained through the selective laser melting technology. According to the method disclosed by the invention, the submicron hafnium carbide powder is utilized to modify the high-aluminum-titanium-nickel-based superalloy powder in a wet ball milling manner, so that hafnium carbide particles are better dispersed on nickel-based superalloy powder spheres, and effective inhibition of cracks in a high-aluminum-titanium-nickel-based superalloy additive manufacturing process and improvement of material performance are realized; the problem that microcracks are prone to being generated in current additive manufacturing is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of high-temperature alloys and additive manufacturing, and specifically relates to a high-aluminum-titanium-nickel-based high-temperature alloy composite powder and a preparation method and application thereof. Background Art

[0002] High aluminum titanium nickel-based superalloys have excellent high temperature strength, creep resistance and oxidation resistance due to their high volume fraction of γˊ phase. The modern aerospace field has continuously improved the requirements for material technical indicators and service performance. Nickel-based superalloys are widely used in the preparation of hot end components of aerospace engines due to their excellent high temperature comprehensive performance.

[0003] In recent years, various technologies in the field of additive manufacturing have developed rapidly. Compared with traditional manufacturing technologies, laser selective melting technology can broaden the freedom of design of hot end components and further improve their service performance, such as forming turbine blades with complex air film cooling structures. However, due to the extremely high cooling rate, uneven solidification temperature distribution, complex stress state and difficult process control of laser selective melting technology, high aluminum titanium nickel-based high-temperature alloy formed components have many cracks and poor high-temperature performance, which restricts its wide application. Therefore, eliminating cracks in the laser selective melting process and improving the overall performance have become key issues that need to be urgently solved in the field of additive manufacturing.

[0004] Some researchers have modified high-temperature alloy powders by adding ceramic reinforcement particles to promote grain refinement of printed structures, thereby dispersing thermal stress and reducing cracks. However, the added particles are often not evenly dispersed in the alloy powder, and may even cause the negative effect of increasing cracks, seriously affecting the performance of parts. Summary of the invention

[0005] In order to solve the problem that microcracks are easily generated in the current additive manufacturing of high-aluminum-titanium-nickel-based high-temperature alloys, the purpose of the present invention is to provide a high-aluminum-titanium-nickel-based high-temperature alloy composite powder and a preparation method and application.

[0006] The present invention uses submicron hafnium carbide powder to modify high-aluminum-titanium-nickel-based high-temperature alloy powder by wet ball milling, so that the hafnium carbide particles can be better and more evenly dispersed on the nickel-based high-temperature alloy powder spheres, thereby effectively suppressing cracks in the additive manufacturing process of the high-aluminum-titanium-nickel-based high-temperature alloy and improving material properties.

[0007] To achieve the above objectives, the technical solution of the present invention is as follows.

[0008] The first aspect of the present invention provides a high-aluminum-titanium-nickel-based high-temperature alloy composite powder, wherein the composite powder is prepared by dispersing strengthening particles on the surface of a matrix by wet ball milling;

[0009] The strengthening particles are submicron hafnium carbide powder, and the matrix is ​​high-aluminum-titanium-nickel-based high-temperature alloy powder; the weight percentage of the strengthening particles in the composite powder is 1-3%.

[0010] The present invention mainly adds submicron hafnium carbide powder and utilizes the submicron hafnium carbide powder to perform thermal crack healing and grain boundary strengthening on the nickel-based high-temperature alloy. The wet ball milling process has the following functions: on the one hand, it prevents the powder from being overheated and deformed, and on the other hand, it can disperse the submicron hafnium carbide powder on the nickel-based high-temperature alloy powder sphere.

[0011] Because the particle surface of the high aluminum titanium nickel-based high temperature alloy powder before modification is not smooth, but full of tiny bumps and pores, showing complex microstructural characteristics. After wet ball milling modification, the modified particles are filled into the corresponding pore structure, so that after laser selective melting technology, a hafnium-rich eutectic phase is formed, and the fluidity of the hafnium-rich eutectic phase is used to fill the thermal cracks caused by shrinkage of the alloy powder.

[0012] In a preferred embodiment, the particle size of the submicron hafnium carbide powder is 0.8 to 1 μm. It was found through experiments that the composite powder prepared by modifying the micron hafnium carbide powder had many cracks in the sample prepared by the laser selective melting technology. It is speculated that this may be related to the micron hafnium carbide particles promoting the initiation and expansion of cracks. However, the sample formed by SLM using submicron hafnium carbide powder has no obvious cracks on the surface. Therefore, the present invention uses submicron hafnium carbide powder as the strengthening particle, and the strengthening particles with small particle size have a more obvious effect on suppressing cracks.

[0013] In a preferred embodiment, the wetting agent used in the wet ball milling is ethanol. Experimental verification shows that the addition of ethanol can prevent the agglomeration of submicron reinforcement particles and promote the uniform dispersion of reinforcement particles in high aluminum titanium nickel-based high temperature alloy powder.

[0014] In a preferred embodiment, in the high-aluminum-titanium-nickel-based high-temperature alloy powder, the sum of the mass percentages of aluminum and titanium elements is greater than 4.5%;

[0015] The particle size distribution of the high-aluminum-titanium-nickel-based high-temperature alloy powder is 15 to 53 μm.

[0016] In a preferred embodiment, the high aluminum titanium nickel-based high temperature alloy powder is CM247LC powder, and high aluminum titanium nickel-based high temperature alloys such as Mar M247, IN 738LC, and Rene 95 may also be used.

[0017] In a preferred embodiment, the purity of the submicron hafnium carbide powder is ≥98.5%.

[0018] The second aspect of the present invention provides a method for preparing the high aluminum titanium nickel-based high temperature alloy composite powder according to the first aspect, comprising the following steps:

[0019] Submicron hafnium carbide powder is mixed with high aluminum titanium nickel-based high temperature alloy powder, and then wet ball milled to disperse the submicron hafnium carbide powder on the surface of the high aluminum titanium nickel-based high temperature alloy powder to prepare a composite powder.

[0020] In a preferred embodiment, the wetting agent used in the wet ball milling is ethanol, and the amount of ethanol used is measured based on the amount of ethanol needed to immerse the mixed powder.

[0021] In a preferred embodiment, the conditions for the wet ball milling are: a ball-to-material ratio of 1:2, a ball milling time of 3 to 10 hours, and a ball milling speed of 300 to 350 rpm.

[0022] In a preferred embodiment, the wet ball milling further includes drying.

[0023] A third aspect of the present invention provides a method for additive manufacturing of high-aluminum-titanium-nickel-based high-temperature alloy composite powder, comprising the following steps:

[0024] The high-aluminum-titanium-nickel-based high-temperature alloy composite powder described in the first aspect is placed on a molding cylinder substrate, and molded and manufactured by a laser selective melting process under a protective atmosphere to obtain a nickel-based high-temperature alloy print.

[0025] In a preferred embodiment, the preset process parameters of the laser selective melting process are:

[0026] The laser power is 100-200 W, the scanning speed is 700-2500 mm / s, the layer thickness is 0.02 mm, and the scanning interval is 0.05 mm.

[0027] In a preferred embodiment, before the molding process is performed, the process further includes:

[0028] The molding cylinder substrate is preheated at a temperature of 100 to 200°C.

[0029] In a preferred embodiment, the protective atmosphere is argon.

[0030] Beneficial effects of the present invention:

[0031] 1. The present invention uses submicron hafnium carbide powder to modify high aluminum titanium nickel-based superalloy powder through a wet ball milling process, which can prevent the powder from overheating and deformation, and can make the submicron hafnium carbide particles more evenly dispersed on the nickel-based superalloy powder spheres. It can effectively suppress cracks in the additive manufacturing process of high aluminum titanium nickel-based superalloy and improve material performance.

[0032] 2. The present invention adopts a wet ball milling process to prevent the powder from overheating and deformation caused by high-speed planetary ball milling. Compared with other process operations, the original morphology of the nickel-based high-temperature alloy powder can be maintained; at the same time, high rotation speed and high ball-to-material ratio can reduce the ball milling time and improve the mixing efficiency. Compared with other process operations, it is simpler and easier, has lower cost and is universal to nickel-based high-temperature alloys of different compositions.

[0033] 3. The present invention uses laser selective melting technology to improve the fluidity of the hafnium-rich eutectic phase melted at the end of solidification, fill the thermal cracks caused by shrinkage, and improve the performance of the material. Compared with the unmodified powder, the average crack density of the formed sample obtained by the additive manufacturing method of the present invention is 0.013mm / mm 2 The tensile strength is increased to 1200MPa-1400MPa, while the elongation is maintained between 7% and 10%.

[0034] 4. The crack-resistant nickel-based high-temperature alloy printed parts prepared by the present invention have a significant crack reduction effect in a relatively large process parameter range, and the crack density is extremely low, which expands the process window. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a schematic flow chart of an additive manufacturing method for a high-aluminum-titanium-nickel-based high-temperature alloy composite powder provided in one embodiment of the present invention.

[0036] Figure 2 Figure (a) is an electron microscope scanning image of the unmodified CM247LC powder of comparative example 1; Figure (b) is an electron microscope scanning image of the CM247LC powder modified with submicron hafnium carbide particles of Example 1; Figure (c) is an electron microscope scanning image of the CM247LC powder modified with submicron hafnium carbide particles of comparative example 4.

[0037] Figure 3 Figure (a) is a macroscopic metallographic photograph of the nickel-based high-temperature alloy sample prepared in Comparative Example 1; Figure (b) is a macroscopic metallographic photograph of the nickel-based high-temperature alloy sample prepared in Example 1, Figure (c) is a macroscopic metallographic photograph of the nickel-based high-temperature alloy sample prepared in Example 4, and Figure (d) is a macroscopic metallographic photograph of the nickel-based high-temperature alloy sample prepared in Example 5.

[0038] Figure 4 This is the stress-strain curve of the nickel-based high-temperature alloy sample prepared in Example 1.

[0039] Figure 5 A crack density comparison bar graph is produced for the nickel-based high-temperature alloy samples prepared in Examples 1 to 2 and Comparative Examples 1 and 4.

[0040] Figure 6 This is the crack morphology of the nickel-based high-temperature alloy sample prepared in Comparative Example 5. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0042] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.

[0043] The first aspect of the present invention provides a high-aluminum-titanium-nickel-based high-temperature alloy composite powder, wherein the composite powder is prepared by dispersing strengthening particles on the surface of a matrix by wet ball milling;

[0044] The strengthening particles are submicron hafnium carbide powder, and the matrix is ​​high-aluminum titanium nickel-based high-temperature alloy powder; the strengthening particles account for 1-3% of the composite powder by mass. For example, 1%, 2%, and 3%. According to thermodynamic calculations, adding more than 3% of strengthening particles will seriously expand the solidification range of the alloy and cause a large number of thermal cracks. In addition, excessive submicron strengthening particles are prone to agglomeration, affecting the dispersion load of strengthening particles on the surface of the matrix.

[0045] The present invention mainly adds submicron hafnium carbide powder and utilizes the submicron hafnium carbide powder to perform thermal crack healing and grain boundary strengthening on the nickel-based high-temperature alloy. The wet ball milling process has the following functions: on the one hand, it prevents the powder from being overheated and deformed, and on the other hand, it can disperse the submicron hafnium carbide powder on the nickel-based high-temperature alloy powder sphere.

[0046] Because the particle surface of the high aluminum titanium nickel-based high temperature alloy powder before modification is not smooth, but full of tiny bumps and pores, showing complex microstructural characteristics. After wet ball milling modification, the modified particles are filled into the corresponding pore structure, so that after laser selective melting technology, a hafnium-rich eutectic phase is formed, and the fluidity of the hafnium-rich eutectic phase is used to fill the thermal cracks caused by shrinkage of the alloy powder.

[0047] In a preferred embodiment, the particle size of the submicron hafnium carbide powder is 0.8-1 μm.

[0048] In a preferred embodiment, the purity of the submicron hafnium carbide powder is ≥98.5%.

[0049] The experiment found that the composite powder prepared by modifying the micron-sized hafnium carbide powder had many cracks in the sample prepared by laser selective melting technology, which is speculated to be related to the micron-sized hafnium carbide particles promoting the initiation and expansion of cracks. However, the sample formed by SLM using submicron-sized hafnium carbide powder had no obvious cracks on the surface. Therefore, the present invention uses submicron-sized hafnium carbide powder as the strengthening particle, and the strengthening particle with a small particle size has a more obvious effect on suppressing cracks.

[0050] In a preferred embodiment, the wetting agent used in the wet ball milling is ethanol. Experimental verification shows that the addition of ethanol can prevent the agglomeration of submicron reinforcement particles and promote the uniform dispersion of reinforcement particles in high aluminum titanium nickel-based high temperature alloy powder.

[0051] In a preferred embodiment, in the high-aluminum-titanium-nickel-based high-temperature alloy powder, the sum of the mass percentages of aluminum and titanium elements is greater than 4.5%; and the particle size distribution of the high-aluminum-titanium-nickel-based high-temperature alloy powder is 15 to 53 μm.

[0052] In a preferred embodiment, the high aluminum titanium nickel-based high temperature alloy powder is CM247LC powder, and can also be Mar M247, IN 738LC, Rene 95 and other high aluminum titanium nickel-based high temperature alloys. These high aluminum titanium nickel-based high temperature alloys all meet the sum of the mass percentages of aluminum and titanium elements>4.5%.

[0053] The second aspect of the present invention provides a method for preparing the high aluminum titanium nickel-based high temperature alloy composite powder according to the first aspect, comprising the following steps:

[0054] Submicron hafnium carbide powder is mixed with high aluminum titanium nickel-based high temperature alloy powder, and then wet ball milled to disperse the submicron hafnium carbide powder on the surface of the high aluminum titanium nickel-based high temperature alloy powder to prepare a composite powder.

[0055] In a preferred embodiment, the wetting agent used in the wet ball milling is ethanol, and the amount of ethanol used is measured based on the amount of ethanol needed to immerse the mixed powder.

[0056] In a preferred embodiment, the conditions for the wet ball milling are: a ball-to-material ratio of 1:2, a ball milling time of 3 to 10 hours, and a ball milling speed of 300 to 350 rpm.

[0057] In a preferred embodiment, the wet ball milling further includes drying.

[0058] A third aspect of the present invention provides a method for additive manufacturing of high-aluminum-titanium-nickel-based high-temperature alloy composite powder, comprising the following steps:

[0059] The high-aluminum-titanium-nickel-based high-temperature alloy composite powder described in the first aspect is placed on a molding cylinder substrate, and molded and manufactured by a laser selective melting process under a protective atmosphere to obtain a nickel-based high-temperature alloy print.

[0060] In a preferred embodiment, the preset process parameters of the laser selective melting process are:

[0061] The laser power is 100-200 W, the scanning speed is 700-2500 mm / s, the layer thickness is 0.02 mm, and the scanning interval is 0.05 mm.

[0062] In a preferred embodiment, before the molding process is performed, the process further includes:

[0063] The molding cylinder substrate is preheated at a temperature of 100 to 200° C. For example, 100° C., 120° C., 140° C., 150° C., 160° C., 180° C., 200° C., etc.

[0064] In a preferred embodiment, the protective atmosphere is argon. Specific embodiments

[0066] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.

[0067] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0068] Unless otherwise specified, the methods described in the following embodiments are conventional methods; the reagents and materials, unless otherwise specified, can be purchased on the market. In the following embodiments, high aluminum titanium nickel-based high temperature alloy powder can be selected from CM247LC powder, Mar M247, IN 738LC, Rene 95 and other high aluminum titanium nickel-based high temperature alloys. Due to experimental conditions, the following embodiments only list CM247LC powder as high aluminum titanium nickel-based high temperature alloy powder, and use CM247LC powder as an example to illustrate the technical solution of the present invention. The submicron grade refers to materials with a scale of 100nm to 1μm. Therefore, the following embodiments of the present invention list a technical solution for modifying CM247LC powder with submicron hafnium carbide powder with a particle size of 0.8 to 1μm. SLM stands for selective laser melting technology, which is a type of additive manufacturing technology that can be applied to metal and plastic materials.

[0069] Example 1

[0070] A method for additive manufacturing of high-aluminum-titanium-nickel-based high-temperature alloy powder, comprising the following steps:

[0071] (1) According to the mass percentage of 99%:1%, 990 g of CM247LC powder and 10 g of submicron hafnium carbide powder (particle size 0.8-1 μm) were weighed.

[0072] (2) The two powders are mixed and placed in a ball mill, and 500 g of ceramic balls with a diameter of 1 to 10 mm are placed in the jar. Then, an appropriate amount of anhydrous ethanol is added to just cover the powder. The planetary ball mill speed is 350 rpm and the ball milling time is 3 h to obtain a high aluminum titanium nickel-based high temperature alloy powder modified with hafnium carbide, referred to as modified powder.

[0073] (3) The ball-milled modified powder is taken out, placed in a stainless steel basin, and dried in a vacuum drying oven for 6 h at a drying temperature of 100° C., and then the dried modified powder is vacuum-packaged.

[0074] (4) Take the dried modified powder and screen it, then put the screened modified powder into the powder cylinder of the SLM forming equipment, introduce argon as the protective gas, preheat the high-temperature alloy substrate to 200°C, and perform SLM forming. The process parameters P1 are: laser power 120W; scanning speed 1200mm / s; scanning spacing 0.05mm; powder layer thickness 0.02mm.

[0075] The scanning strategy is reciprocating for each layer, and the stack is rotated 67°. The printed samples are cut from the substrate by wire cutting process and surface polished to obtain crack-resistant SLM-formed nickel-based high-temperature alloy samples.

[0076] Example 2

[0077] A method for additive manufacturing of high-aluminum-titanium-nickel-based high-temperature alloy powder, comprising the following steps:

[0078] (1) According to the mass percentage of 99%:1%, 990 g of CM247LC powder and 10 g of submicron hafnium carbide powder (particle size 0.8-1 μm) were weighed.

[0079] (2) The two powders are mixed and placed in a ball mill, and 500 g of ceramic balls with a diameter of 1 to 10 mm are placed in the jar. Then, an appropriate amount of anhydrous ethanol is added to just cover the powder. The planetary ball mill speed is 350 rpm and the ball milling time is 3 h to obtain a high aluminum titanium nickel-based high temperature alloy powder modified with hafnium carbide, referred to as modified powder.

[0080] (3) The ball-milled modified powder is taken out, placed in a stainless steel basin, and dried in a vacuum drying oven for 6 h at a drying temperature of 100° C., and then the dried modified powder is vacuum-packaged.

[0081] (4) Take the dried modified powder and screen it, then put the screened modified powder into the powder cylinder of the SLM forming equipment, introduce argon as the protective gas, preheat the high-temperature alloy substrate to 200°C, and perform SLM forming. The process parameters P2 are: laser power 100W; scanning speed 700mm / s; scanning spacing 0.05mm; powder layer thickness 0.02mm.

[0082] The scanning strategy is reciprocating for each layer, and the stack is rotated 67°. The printed samples are cut from the substrate by wire cutting process and surface polished to obtain the crack-resistant SLM-formed nickel-based high-temperature alloy samples.

[0083] Example 3

[0084] A method for additive manufacturing of high-aluminum-titanium-nickel-based high-temperature alloy powder, comprising the following steps:

[0085] (1) According to the mass percentage of 99%:1%, 990 g of CM247LC powder and 10 g of submicron hafnium carbide powder (particle size 0.8-1 μm) were weighed.

[0086] (2) The two powders are mixed and placed in a ball mill, and 500 g of ceramic balls with a diameter of 1 to 10 mm are placed in the jar. Then, an appropriate amount of anhydrous ethanol is added to just cover the powder. The planetary ball mill speed is 350 rpm and the ball milling time is 3 h to obtain a high aluminum titanium nickel-based high temperature alloy powder modified with hafnium carbide, referred to as modified powder.

[0087] (3) The ball-milled modified powder is taken out, placed in a stainless steel basin, and dried in a vacuum drying oven for 6 h at a drying temperature of 100° C., and then the dried modified powder is vacuum-packaged.

[0088] (4) Take the dried modified powder and screen it, then put the screened modified powder into the powder cylinder of the SLM forming equipment, introduce argon as the protective gas, preheat the high-temperature alloy substrate to 200°C, and perform SLM forming. The process parameters P3 are: laser power 200W; scanning speed 2500mm / s; scanning spacing 0.05mm; powder layer thickness 0.02mm.

[0089] The scanning strategy is reciprocating for each layer, and the stack is rotated 67°. The printed samples are cut from the substrate by wire cutting process and surface polished to obtain the crack-resistant SLM-formed nickel-based high-temperature alloy samples.

[0090] Example 4

[0091] A method for additive manufacturing of high-aluminum-titanium-nickel-based high-temperature alloy powder, comprising the following steps:

[0092] (1) According to the mass percentage of 98%:2%, 980 g of CM247LC powder and 20 g of submicron hafnium carbide powder (particle size 0.8-1 μm) were weighed.

[0093] (2) The two powders are mixed and placed in a ball mill, and 500 g of ceramic balls with a diameter of 1 to 10 mm are placed in the jar. Then, an appropriate amount of anhydrous ethanol is added to just cover the powder. The planetary ball mill speed is 350 rpm and the ball milling time is 3 h to obtain a high aluminum titanium nickel-based high temperature alloy powder modified with hafnium carbide, referred to as modified powder.

[0094] (3) The ball-milled modified powder is taken out, placed in a stainless steel basin, and dried in a vacuum drying oven for 6 h at a drying temperature of 100° C., and then the dried modified powder is vacuum-packaged.

[0095] (4) Take the dried modified powder and screen it, then put the screened modified powder into the powder cylinder of the SLM forming equipment, introduce argon as the protective gas, preheat the high-temperature alloy substrate to 200°C, and perform SLM forming. The process parameters P1 are: laser power 120W; scanning speed 1200mm / s; scanning spacing 0.05mm; powder layer thickness 0.02mm.

[0096] The scanning strategy is reciprocating for each layer, and the stack is rotated 67°. The printed samples are cut from the substrate by wire cutting process and surface polished to obtain crack-resistant SLM-formed nickel-based high-temperature alloy samples.

[0097] Example 5

[0098] A method for additive manufacturing of high-aluminum-titanium-nickel-based high-temperature alloy powder, comprising the following steps:

[0099] (1) According to the mass percentage of 97%:3%, 970 g of CM247LC powder and 30 g of submicron hafnium carbide powder (particle size 0.8-1 μm) were weighed.

[0100] (2) The two powders are mixed and placed in a ball mill, and 500 g of ceramic balls with a diameter of 1 to 10 mm are placed in the jar. Then, an appropriate amount of anhydrous ethanol is added to just cover the powder. The planetary ball mill speed is 350 rpm and the ball milling time is 3 h to obtain a high aluminum titanium nickel-based high temperature alloy powder modified with hafnium carbide, referred to as modified powder.

[0101] (3) The ball-milled modified powder is taken out, placed in a stainless steel basin, and dried in a vacuum drying oven for 6 h at a drying temperature of 100° C., and then the dried modified powder is vacuum-packaged.

[0102] (4) Take the dried modified powder and screen it, then put the screened modified powder into the powder cylinder of the SLM forming equipment, introduce argon as the protective gas, preheat the high-temperature alloy substrate to 200°C, and perform SLM forming. The process parameters P1 are: laser power 120W; scanning speed 1200mm / s; scanning spacing 0.05mm; powder layer thickness 0.02mm.

[0103] The scanning strategy is reciprocating for each layer, and the stack is rotated 67°. The printed samples are cut from the substrate by wire cutting process and surface polished to obtain crack-resistant SLM-formed nickel-based high-temperature alloy samples.

[0104] Comparative Example 1

[0105] A method for additive manufacturing of high-aluminum-titanium-nickel-based high-temperature alloy powder, comprising the following steps:

[0106] Take 1000g of CM247LC powder, place it in the powder cylinder of the SLM forming equipment, introduce argon as protective gas, preheat the high-temperature alloy substrate to 200℃, and perform SLM forming. The process parameters P1 are: laser power is 120W; scanning speed is 1200mm / s; scanning spacing is 0.05mm; powder layer thickness is 0.02mm; scanning strategy is reciprocating per layer, and the stacking is rotated 67°. The printed sample is cut from the substrate by wire cutting process and the surface is polished to obtain the SLM-formed nickel-based high-temperature alloy sample.

[0107] Comparative Example 2

[0108] A method for additive manufacturing of high-aluminum-titanium-nickel-based high-temperature alloy powder, comprising the following steps:

[0109] The same CM247LC powder as in Comparative Example 1 was used as raw material, 1000 g was taken and placed in the SLM forming equipment, argon gas was introduced as the protective gas, the high temperature alloy substrate was preheated to 200°C, and SLM forming was performed. The process parameters P2 were: laser power of 100 W; scanning speed of 700 mm / s; scanning spacing of 0.05 mm; and powder layer thickness of 0.02 mm.

[0110] The scanning strategy is reciprocating for each layer, and the stack is rotated 67°. The printed sample is cut from the substrate by wire cutting process and the surface is polished to obtain the SLM-formed nickel-based high-temperature alloy sample.

[0111] Comparative Example 3

[0112] A method for additive manufacturing of high-aluminum-titanium-nickel-based high-temperature alloy powder, comprising the following steps:

[0113] The same CM247LC powder as in Comparative Example 1 was used as raw material, 1000 g was placed in the SLM forming equipment, argon was introduced as protective gas, the high temperature alloy substrate was preheated to 200°C, and SLM forming was performed. The process parameters P3 were: laser power 200 W; scanning speed 2500 mm / s; scanning spacing 0.05 mm; powder layer thickness 0.02 mm.

[0114] The scanning strategy is reciprocating for each layer, and the stack is rotated 67°. The printed sample is cut from the substrate by wire cutting process and the surface is polished to obtain the SLM-formed nickel-based high-temperature alloy sample.

[0115] Comparative Example 4

[0116] A modification method for high-aluminum-titanium-nickel-based high-temperature alloy powder comprises the following steps:

[0117] (1) According to the mass percentage of 99%:1%, 990 g of CM247LC powder and 10 g of submicron hafnium carbide powder (particle size 0.8-1 μm) were weighed;

[0118] (2) The two powders are mixed and placed in a ball mill, and 500 g of ceramic balls are placed in the ball mill. The diameter of the ceramic balls is 1 to 10 mm. The planetary ball mill rotates at 350 rpm and the ball milling time is 3 h. A high-aluminum-titanium-nickel-based high-temperature alloy powder modified with hafnium carbide is obtained, referred to as modified powder.

[0119] (3) The ball-milled modified powder is taken out, placed in a stainless steel basin, and dried in a vacuum drying oven for 6 h at a drying temperature of 100° C., and then the dried modified powder is vacuum-packaged.

[0120] Comparative Example 5

[0121] A method for additive manufacturing of high-aluminum-titanium-nickel-based high-temperature alloy powder, comprising the following steps:

[0122] (1) According to the mass percentage of 99%:1%, 990 g of CM247LC powder and 10 g of micron-sized hafnium carbide powder (particle size 2-10 μm) were weighed.

[0123] (2) The two powders are mixed and placed in a ball mill, and 500 g of ceramic balls with a diameter of 1 to 10 mm are placed in the jar. Then, an appropriate amount of anhydrous ethanol solution is added to just cover the powder. The planetary ball mill speed is 350 rpm and the ball milling time is 3 h to obtain a high-aluminum-titanium-nickel-based high-temperature alloy powder modified with hafnium carbide, referred to as modified powder.

[0124] (3) The ball-milled modified powder is taken out, placed in a stainless steel basin, and dried in a vacuum drying oven for 6 h at a drying temperature of 100° C., and then the dried modified powder is vacuum-packaged.

[0125] (4) The dried modified powder was sieved, and then the sieved modified powder was placed in the powder cylinder of the SLM forming equipment, and argon gas was introduced as the protective gas. The preheating temperature of the high-temperature alloy substrate was 200°C, and SLM forming was performed. The process parameters P1 were: laser power was 120 W; scanning speed was 1200 mm / s; scanning spacing was 0.05 mm; and powder layer thickness was 0.02 mm.

[0126] The scanning strategy is reciprocating for each layer, and the stack is rotated 67°. The printed samples are cut from the substrate by wire cutting process and the surface is polished to obtain SLM-formed nickel-based high-temperature alloy samples.

[0127] The performance tests were performed on the samples prepared in the above examples.

[0128] Test Example 1:

[0129] The unmodified CM247LC powder of Comparative Example 1, the CM247LC powder modified with submicron hafnium carbide particles of Example 1 (with ethanol added), and the CM247LC powder modified with submicron hafnium carbide particles of Comparative Example 4 (without ethanol added) were respectively subjected to scanning electron microscopy (SEM) tests to study the particle dispersion before and after modification of submicron chromium carbide, as well as the effects of wet grinding and dry grinding on the particle dispersion.

[0130] The experimental parameters and conditions are shown in Table 1, and the SEM test results are shown in Figure 2 . Figure 2Figure (a) is an electron microscope scanning image of the unmodified CM247LC powder of comparative example 1; Figure (b) is an electron microscope scanning image of the CM247LC powder modified with submicron hafnium carbide particles of Example 1; Figure (c) is an electron microscope scanning image of the CM247LC powder modified with submicron hafnium carbide particles of comparative example 4.

[0131] Table 1 Experimental parameters of grinding conditions

[0132]

[0133]

[0134] Note: “-” means no ethanol was added or the corresponding grinding operation was not performed.

[0135] Depend on Figure 2 The results show that the particle size distribution of the CM247LC powder before modification is relatively uniform, but there are also some larger particles scattered among them. Figure 2 As can be seen from Figure (a), the surface of the CM247LC powder particles is not smooth, has obvious dendrite morphology, and exhibits complex microstructural characteristics.

[0136] like Figure 2 Figure (b) shows that the modified powder obtained by modifying CM247LC powder with submicron hafnium carbide particles can obtain a powder morphology with uniform particle dispersion by wet ball milling under appropriate ball milling parameters; it can be seen from the SEM image that the submicron hafnium carbide particles can be well and evenly dispersed on the surface of the high aluminum titanium nickel-based high-temperature alloy powder sphere.

[0137] like Figure 2 Figure (c) shows that the modified powder obtained by ordinary mechanical mixing has a serious submicron reinforcement particle agglomeration effect, as can be seen from the SEM image. The submicron hafnium carbide reinforcement particles agglomerate and cannot be evenly dispersed on the surface of the high aluminum titanium nickel-based high-temperature alloy powder sphere.

[0138] This shows that the wet grinding method used in Example 1 of the present invention helps to evenly disperse the submicron hafnium carbide particles on the surface of the high aluminum titanium nickel-based high temperature alloy powder sphere. The addition of anhydrous ethanol can prevent the agglomeration of submicron reinforcement particles and promote the uniform dispersion of reinforcement particles in the high aluminum titanium nickel-based high temperature alloy powder.

[0139] Test Example 2:

[0140] The SLM-formed nickel-based high-temperature alloy samples prepared in Comparative Example 1, Example 1 and Examples 4-5 were subjected to macroscopic metallographic observation and photographed to explore the effect of different addition amounts of submicron hafnium carbide powder on the apparent properties of the nickel-based high-temperature alloy samples.

[0141] The experimental parameters of different addition amounts of hafnium carbide powder are shown in Table 2, and the macroscopic metallographic photos are shown in Figure 3 . Figure 3 Figure (a) is a macroscopic metallographic photograph of the nickel-based high-temperature alloy sample prepared in Comparative Example 1; Figure (b) is a macroscopic metallographic photograph of the nickel-based high-temperature alloy sample prepared in Example 1, Figure (c) is a macroscopic metallographic photograph of the nickel-based high-temperature alloy sample prepared in Example 4, and Figure (d) is a macroscopic metallographic photograph of the nickel-based high-temperature alloy sample prepared in Example 5.

[0142] Table 2 Experimental parameters and test results of different addition amounts of hafnium carbide powder

[0143]

[0144] Note: “-” indicates that no hafnium carbide powder was added; Examples 1, 4-5 and Comparative Example 1 were compared under the same process parameter P1.

[0145] Depend on Figure 3 It can be seen from the macroscopic metallographic photos that under the same process parameter P1, the nickel-based high-temperature alloy sample obtained by laser selective melting using submicron hafnium carbide modified high-aluminum-titanium nickel-based high-temperature alloy powder has an average crack density on the surface of the sample that gradually increases with the increase in the amount of submicron hafnium carbide powder added. Among them, there is no obvious crack on the surface of the sample in Example 1.

[0146] Compared with the nickel-based high-temperature alloy sample prepared from the unmodified CM247LC powder in comparative example 1, the cracks and pores of the sample obtained in Example 1 of the present invention are significantly reduced, and the average crack density is 0.013 mm / mm 2 .

[0147] It can be seen that Example 1 of the present invention uses 1% submicron hafnium carbide powder to modify the high aluminum titanium nickel-based high-temperature alloy powder. The submicron hafnium carbide powder can be better and more evenly dispersed on the nickel-based high-temperature alloy powder spheres by wet grinding. The fluidity of the melted hafnium-rich eutectic phase at the end of solidification is improved by the laser selective melting technology, which fills the thermal cracks caused by shrinkage, thereby improving the performance of the material.

[0148] Test Example 3:

[0149] The room temperature mechanical properties test of the SLM-formed nickel-based high-temperature alloy specimens prepared in Examples 1, 4 and 5 and Comparative Example 1 was carried out to explore the effect of different addition amounts of submicron hafnium carbide powder on the mechanical properties of the nickel-based high-temperature alloy specimens.

[0150] The room temperature mechanical properties test results of samples prepared with different amounts of hafnium carbide powder are shown in Tables 3 and Figure 4 . Figure 4 These are stress-strain curves of the nickel-based high-temperature alloy samples prepared in Example 1, Example 4 and Comparative Example 1. Each nickel-based high-temperature alloy sample was tested twice in parallel.

[0151] Table 3 Room temperature mechanical properties test results

[0152]

[0153] Note: "-" indicates that no addition was made, or the corresponding operation steps were not performed. Examples 1, 4-5 and Comparative Example 1 were compared under the same process parameter P1. Since the test result of the average crack density of Example 5 was lower than that of Example 4, it was inferred that the mechanical property results of Example 5 were lower than those of Example 4. Therefore, we did not record the mechanical property results of Example 5.

[0154] Depend on Figure 4 It can be seen from the results in Table 3 that with the increase in the amount of submicron hafnium carbide powder, the tensile strength and elongation show a trend of first increasing and then decreasing, and the tensile strength and elongation are the largest when the addition amount is 1%. Moreover, compared with the sample in Comparative Example 1, the sample formed by laser selective melting after the high aluminum titanium nickel-based high temperature alloy powder is modified by submicron hafnium carbide in Example 1 has a significant improvement in strength, with a tensile strength of 1247.7±6.83MPa and an elongation of 7.2±0.19%. This shows that by adding 1% of submicron hafnium carbide powder, the tensile strength and elongation of the nickel-based high temperature alloy sample can be significantly improved.

[0155] Test Example 4:

[0156] The crack morphology of the SLM-formed nickel-based high-temperature alloy sample prepared in Comparative Example 5 was observed and photographed, and compared with the test results of Example 1 to explore the effect of hafnium carbide powder of different particle sizes on the apparent performance of the nickel-based high-temperature alloy sample; the results are shown in Figure 6 and Figure 3 (b) Figure . Figure 6 This is the crack morphology of the nickel-based high-temperature alloy sample prepared in Comparative Example 5. Figure 3 Figure (b) is a macroscopic metallographic photograph of the nickel-based high-temperature alloy sample prepared in Example 1.

[0157] Table 4 Effect of different particle sizes of hafnium carbide powder on the apparent properties of the samples

[0158]

[0159] Comparative Example 5 ( Figure 6 ) and Example 1 ( Figure 3 (b)) is compared with the macroscopic metallographic photographs of the nickel-based high-temperature alloy samples. It can be seen that the nickel-based high-temperature alloy sample prepared by using micron-sized hafnium carbide to modify CM247LC in Comparative Example 5 has more cracks, and the average crack density of the sample in Comparative Example 5 is much greater than the average crack density of the sample in Example 1. It is speculated that this may be related to the micron-sized hafnium carbide particles promoting the initiation and expansion of cracks. The nickel-based high-temperature alloy sample in Example 1, such as Figure 3 As shown in (b), there are no obvious cracks on the sample surface. This shows that the use of submicron hafnium carbide strengthening particles has a better modification effect on high aluminum titanium nickel-based high-temperature alloys, and small-size strengthening particles have a more obvious effect on crack inhibition.

[0160] Test Example 5:

[0161] The crack density of the nickel-based high-temperature alloy samples prepared in Examples 1 to 3 and Comparative Examples 1 to 3 was compared. Figure 5 and Table 5. Figure 5 A comparative bar graph of crack density is made for the nickel-based high-temperature alloy samples prepared in Examples 1 to 2 and Comparative Examples 1 and 4. Process 1 represents process parameter P1; Process 2 represents process parameter P2; Process 3 represents process parameter P3; CM247LC-Pure represents unmodified CM247LC powder; CM247LC+1wt%HfC represents CM247LC powder modified with 1wt% of submicron hafnium carbide particles; Crack Density represents crack density.

[0162] Table 5 Comparison of crack density of different process parameters

[0163]

[0164] Note: Process parameters P1 are: laser power 120W; scanning speed 1200mm / s; scanning spacing 0.05mm; powder layer thickness 0.02mm. Process parameters P2 are: laser power 100W; scanning speed 700mm / s; scanning spacing 0.05mm; powder layer thickness 0.02mm. Process parameters P3 are: laser power 200W; scanning speed 2500mm / s; scanning spacing 0.05mm; powder layer thickness 0.02mm.

[0165] From the crack density comparison results, it can be seen that compared with the unmodified CM247LC powder, the submicron hafnium carbide modified particles have a significant crack inhibition effect on the process parameter range of different energy densities, greatly expanding the process window.

[0166] In summary, in view of the problem that microcracks are easily generated in the current additive manufacturing of high-aluminum-titanium-nickel-based high-temperature alloys, the present invention modifies the high-aluminum-titanium-nickel-based high-temperature alloy powder by adding a certain amount of submicron hafnium carbide powder to obtain modified particles, and uses the modified particles for SLM forming, which can heal the hot cracks and strengthen the grain boundaries of the nickel-based high-temperature alloy. Hafnium is widely used in the casting process of high-temperature alloys to improve the fluidity of molten metal liquid, prevent defects such as shrinkage, shrinkage and cracks, and thus extend a variety of alloys known on the market. In the additive manufacturing process, there is a large component segregation in the molten metal liquid at the end of solidification, especially hafnium, so the hafnium-rich metal liquid has good fluidity and will fill the solidification cracks caused by solidification shrinkage, thereby achieving the healing effect of cracks; on the other hand, the submicron hafnium carbide powder evenly distributed in the high-temperature alloy powder helps to achieve the effect of dispersion strengthening the grain boundaries, further prevent the initiation of intergranular cracks, and greatly improve the comprehensive mechanical properties of the additive manufacturing high-aluminum-titanium-nickel-based high-temperature alloy.

[0167] The method of the present invention is used to form and modify CM247LC high aluminum titanium nickel-based high temperature alloy without obvious cracks, and has a significant effect on a considerable range of process parameters, and can control the crack density within 0.009-0.013 mm / mm 2 The method of the present invention can also provide a certain reference basis for the technical expansion of microcrack suppression of other nickel-based high-temperature alloys.

[0168] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A high-aluminum-titanium-nickel-based high-temperature alloy composite powder, characterized in that: The composite powder is prepared by dispersing the strengthening particles on the surface of the matrix by wet ball milling; The strengthening particles are submicron hafnium carbide powder, and the matrix is ​​high-aluminum-titanium-nickel-based high-temperature alloy powder; the weight percentage of the strengthening particles in the composite powder is 1-3%.

2. The high aluminum titanium nickel-based high temperature alloy composite powder according to claim 1, characterized in that: The particle size of the submicron hafnium carbide powder is 0.8-1 μm.

3. The high aluminum titanium nickel-based high temperature alloy composite powder according to claim 1, characterized in that: The wetting agent used in the wet ball milling is ethanol.

4. The high aluminum titanium nickel-based high temperature alloy composite powder according to claim 1, characterized in that: In the high-aluminum-titanium-nickel-based high-temperature alloy powder, the sum of the mass percentages of aluminum and titanium elements is greater than 4.5%; The particle size distribution of the high-aluminum-titanium-nickel-based high-temperature alloy powder is 15 to 53 μm.

5. A method for preparing the high aluminum titanium nickel-based high temperature alloy composite powder according to claim 1, characterized in that: The following steps are involved: Submicron hafnium carbide powder is mixed with high aluminum titanium nickel-based high temperature alloy powder, and then wet ball milled to disperse the submicron hafnium carbide powder on the surface of the high aluminum titanium nickel-based high temperature alloy powder to prepare a composite powder.

6. The method for preparing high aluminum titanium nickel-based high temperature alloy composite powder according to claim 5, characterized in that: The wetting agent used in wet ball milling is ethanol, and the amount of ethanol used is measured based on the amount of ethanol needed to immerse the mixed powder.

7. The method for preparing high aluminum titanium nickel-based high temperature alloy composite powder according to claim 5, characterized in that: The conditions of the wet ball milling are: a ball-to-material ratio of 1:2, a ball milling time of 3 to 10 hours, and a ball milling speed of 300 to 350 rpm.

8. A method for additive manufacturing using high-aluminum-titanium-nickel-based high-temperature alloy composite powder, characterized in that: The following steps are involved: The high-aluminum-titanium-nickel-based high-temperature alloy composite powder described in claim 1 is placed on a molding cylinder substrate, and is molded and manufactured by a laser selective melting process under a protective atmosphere to obtain a nickel-based high-temperature alloy print.

9. The method for additive manufacturing using high aluminum titanium nickel-based high temperature alloy composite powder according to claim 8, characterized in that: The preset process parameters of the laser selective melting process are: The laser power is 100-200 W, the scanning speed is 700-2500 mm / s, the layer thickness is 0.02 mm, and the scanning interval is 0.05 mm.

10. The method for additive manufacturing using high aluminum titanium nickel-based high temperature alloy composite powder according to claim 8, characterized in that: Before molding and manufacturing, it also includes: The molding cylinder substrate is preheated at a temperature of 100 to 200°C.