High-strength rare earth doped aluminum alloy and preparation method thereof
By doping rare earth elements and other alloy elements in aluminum alloys, and using vacuum smelting and solid solution treatment processes, the problem of insufficient strength of aluminum alloys is solved, significantly improving its strength and hardness, and meeting high-performance needs.
Patent Information
- Application Number
- CN202410990205.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional aluminum alloys are prone to wear and breakage during long-term use in external environments, and are insufficient in strength and cannot meet the growing performance needs.
By doping rare earth elements cerium, lanthanum, neodymium and scandium, combined with magnesium, copper, lithium, silicon, titanium and other elements, vacuum smelting and solid solution treatment are used to prepare high-strength rare earth doped aluminum alloys to improve their strength and hardness.
It significantly improves the strength and hardness of aluminum alloys, meets high performance needs, improves the mechanical properties and toughness of the materials, and is suitable for applications in multiple fields.
Smart Images

Figure CN118910473A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum alloys, and in particular to a high-strength rare earth-doped aluminum alloy and a preparation method thereof. Background Art
[0002] Aluminum is the second largest metal material in terms of output after steel. It is known as the "universal metal" due to its good performance, wide range of uses, large demand and low recycling cost. With the continuous advancement of science and technology and the continuous growth of social needs, aluminum alloys are increasingly used in industry, such as aerospace, automobiles, ships, construction, electronics and other fields. Aluminum alloys are made of pure aluminum by adding some alloying elements, such as Al-Mn alloys developed by adding manganese elements to pure aluminum, Al-Cu alloys developed by adding copper elements to pure aluminum, Al-Cu-Mg hard aluminum alloys developed by adding copper and magnesium elements to pure aluminum, and Al-Zn-Mg-Cu super-hard aluminum alloys developed by adding zinc, magnesium and copper elements to pure aluminum.
[0003] However, with the increasing demand in application fields, more and more attention is paid to the strength performance of aluminum alloys, and the performance requirements are getting higher and higher. However, traditional aluminum alloys have low strength and are prone to wear and breakage under long-term use conditions in the external environment. Therefore, the present invention proposes a high-strength rare earth-doped aluminum alloy and a preparation method thereof to solve the problems existing in the prior art. Summary of the invention
[0004] In view of the above problems, the purpose of the present invention is to propose a high-strength rare earth doped aluminum alloy and a preparation method thereof. The high-strength rare earth doped aluminum alloy and the preparation method thereof can solve the problems existing in the prior art by doping rare earth elements to improve the strength of the aluminum alloy.
[0005] To achieve the purpose of the present invention, the present invention is implemented through the following technical scheme: a high-strength rare-earth-doped aluminum alloy and a preparation method thereof, comprising an alloy material and a rare-earth material, wherein the alloy material comprises the following raw materials in weight percentage: 0.3-0.6% magnesium, 0.3-0.5% silicon, 0.05-0.15% lithium, 0.1-0.2% zirconium, 0.4-0.5% copper and 0.05-0.10% titanium, and the rare-earth material comprises the following raw materials in weight percentage: 1.0-1.5% cerium, 0.1-0.2% lanthanum, 0.6-1.1% neodymium and 0.1-0.3% scandium, and the remainder is aluminum and inevitable impurities, the alloy material and the rare-earth material are both in powder form, and the sum of the alloy material, the rare-earth material, the aluminum and the inevitable impurities is 100%.
[0006] A further improvement is that it includes alloy materials and rare earth materials, the alloy material includes the following raw materials in weight percentage: 0.6% magnesium, 0.5% silicon, 0.15% lithium, 0.2% zirconium, 0.5% copper and 0.10% titanium, the rare earth material includes the following raw materials in weight percentage: 1.5% cerium, 0.2% lanthanum, 1.1% neodymium and 0.3% scandium, the remainder being aluminum and inevitable impurities, the sum of the alloy material, rare earth material, aluminum and inevitable impurities being 100%.
[0007] A further improvement is that it includes alloy materials and rare earth materials, the alloy material includes the following raw materials in weight percentage: 0.3% magnesium, 0.3% silicon, 0.05% lithium, 0.1% zirconium, 0.4% copper and 0.05% titanium, the rare earth material includes the following raw materials in weight percentage: 1.0% cerium, 0.1% lanthanum, 0.6% neodymium and 0.1% scandium, and the remainder is aluminum and inevitable impurities, and the sum of the alloy material, rare earth material, aluminum and inevitable impurities is 100%.
[0008] A method for preparing a high-strength rare earth-doped aluminum alloy comprises the following steps:
[0009] Step 1: Material preparation and processing
[0010] Accurately weigh the corresponding alloy materials, rare earth materials and aluminum materials according to the formula, and place the weighed materials in a drying oven for drying, and then mix them for standby use after drying;
[0011] Step 2: Initial Melting
[0012] First, the aluminum material in step 1 is placed in a vacuum melting furnace and heated for the first time to make the aluminum material molten, then the alloy material is added and heated for the second time. During the second heating, the material is stirred. After heating for 20 to 30 minutes, the rare earth material is added and heated for the third time. After completion, an aluminum alloy solution is obtained;
[0013] Step 3: Rare earth doped aluminum alloy casting
[0014] In step 2, after obtaining the aluminum alloy solution, the temperature is lowered to 650-680° C., and the solution is allowed to stand for 30-40 minutes. After the solution is allowed to stand, slag is removed. After the slag is removed, the composition of the aluminum alloy solution is analyzed to ensure that it meets the raw material formula. The temperature is then lowered to 550-600° C., and mold assembly is performed to obtain a rare earth-doped aluminum alloy.
[0015] Step 4: Post-processing
[0016] The obtained rare earth doped aluminum alloy is heat treated by solution treatment and aging treatment to improve the performance of the rare earth doped aluminum alloy, thereby obtaining a high-strength rare earth doped aluminum alloy and completing the preparation.
[0017] A further improvement is that in step 1, the temperature in the drying box is 80-100° C. and the drying time is 3-4 hours.
[0018] A further improvement is that in step 1, the mixing treatment is performed by mixing the dried alloy material for the first time to obtain a mixture A, and then mixing the dried rare earth material for the second time to obtain a mixture B.
[0019] A further improvement is that in step 2, the first heating temperature is 720-750°C, the second heating temperature is 740-770°C, and the third heating temperature is 760-790°C.
[0020] A further improvement is that in step 4, the specific steps of solution treatment and aging treatment are:
[0021] S1: heating the rare earth doped aluminum alloy to 250-350°C and keeping the temperature for 0.5-1h;
[0022] S2: Raise the temperature to 450-500°C and keep warm for 10-20 minutes;
[0023] S2: After keeping warm, lower the temperature to 350-400℃, keep warm for 20-30 minutes, and then quickly quench.
[0024] S4: After quenching, natural aging treatment is carried out at room temperature for 12 to 72 hours.
[0025] The beneficial effects of the present invention are as follows: the high-strength rare earth-doped aluminum alloy provided by the present invention is prepared by doping rare earth elements cerium, lanthanum, neodymium and scandium on the basis of aluminum alloy materials, and the performance of the aluminum alloy is improved by using rare earth elements. At the same time, the strength and hardness of the aluminum alloy matrix material are improved by adding copper, magnesium and lithium elements to the aluminum alloy material, and the performance of the aluminum alloy matrix material is further improved by adding silicon and titanium elements, thereby comprehensively improving the strength of the rare earth-doped aluminum alloy, thereby meeting the growing performance requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic diagram of the preparation method steps of the present invention. DETAILED DESCRIPTION
[0027] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.
[0028] The raw materials used in the following examples were all obtained through conventional commercial routes.
[0029] Embodiment 1
[0030] according to Figure 1 As shown, this embodiment proposes a high-strength rare earth-doped aluminum alloy, including an alloy material and a rare earth material, including an alloy material and a rare earth material, the alloy material includes the following raw materials in weight percentage: 0.6% magnesium, 0.5% silicon, 0.15% lithium, 0.2% zirconium, 0.5% copper and 0.10% titanium, the rare earth material includes the following raw materials in weight percentage: 1.5% cerium, 0.2% lanthanum, 1.1% neodymium and 0.3% scandium, the remainder is aluminum and inevitable impurities, the alloy material and the rare earth material are both in the form of single substance powder, and the sum of the alloy material, rare earth material, aluminum and inevitable impurities is 100%.
[0031] A method for preparing a high-strength rare earth-doped aluminum alloy comprises the following steps:
[0032] Step 1: Material preparation and processing
[0033] Accurately weigh the corresponding alloy materials, rare earth materials and aluminum materials according to the formula, wherein the alloy materials include the following raw materials in weight percentage: 0.3% magnesium, 0.3% silicon, 0.05% lithium, 0.1% zirconium, 0.4% copper and 0.05% titanium, and the rare earth materials include the following raw materials in weight percentage: 1.0% cerium, 0.1% lanthanum, 0.6% neodymium and 0.1% scandium, and the balance is aluminum, and the weighed materials are placed in a drying oven for drying, and then mixed for standby use, the temperature in the drying oven is 80° C., the drying time is 4 hours, and the mixing method is: the dried alloy materials are mixed for the first time to obtain a mixture A, and then the dried rare earth materials are mixed for the second time to obtain a mixture B;
[0034] Step 2: Initial Melting
[0035] First, the aluminum material in step 1 is placed in a vacuum melting furnace for the first heating. After the aluminum material is in a molten state, the alloy material is added and heated for the second time. During the second heating process, the material is stirred. After heating for 30 minutes, the rare earth material is added and heated for the third time. After completion, an aluminum alloy solution is obtained. The first heating temperature is 720°C, the second heating temperature is 740°C, and the third heating temperature is 760°C.
[0036] Step 3: Rare earth doped aluminum alloy casting
[0037] In step 2, after obtaining the aluminum alloy solution, the temperature is lowered to 650° C. and allowed to stand for 40 minutes. After standing, slag is removed. After slag removal, the composition of the aluminum alloy solution is analyzed to ensure that it meets the raw material formula. Then, the temperature is lowered to 550° C. and molded to obtain the rare earth doped aluminum alloy.
[0038] Step 4: Post-processing
[0039] The obtained rare earth doped aluminum alloy is heat treated by solution treatment and aging treatment to improve the performance of the rare earth doped aluminum alloy, thereby obtaining a high-strength rare earth doped aluminum alloy to complete the preparation, wherein the specific steps of the solution treatment and aging treatment are:
[0040] S1: heating the rare earth doped aluminum alloy to 250°C and keeping it at this temperature for 1h;
[0041] S2: Raise the temperature to 450°C and keep warm for 20 minutes;
[0042] S2: After keeping warm, lower the temperature to 350℃, keep warm for 30 minutes, and then quickly quench
[0043] S4: After quenching, natural aging treatment is carried out at room temperature for 72 hours.
[0044] Embodiment 2
[0045] according to Figure 1 As shown, this embodiment proposes a high-strength rare earth-doped aluminum alloy, including an alloy material and a rare earth material, the alloy material includes the following raw materials in weight percentage: 0.3% magnesium, 0.3% silicon, 0.05% lithium, 0.1% zirconium, 0.4% copper and 0.05% titanium, the rare earth material includes the following raw materials in weight percentage: 1.0% cerium, 0.1% lanthanum, 0.6% neodymium and 0.1% scandium, the remainder being aluminum and inevitable impurities, the alloy material and the rare earth material are both in the form of single substance powder, and the sum of the alloy material, the rare earth material, aluminum and the inevitable impurities is 100%.
[0046] A method for preparing a high-strength rare earth-doped aluminum alloy comprises the following steps:
[0047] Step 1: Material preparation and processing
[0048] Accurately weigh the corresponding alloy materials, rare earth materials and aluminum materials according to the formula, wherein the alloy materials include the following raw materials in weight percentage: 0.3% magnesium, 0.3% silicon, 0.05% lithium, 0.1% zirconium, 0.4% copper and 0.05% titanium, and the rare earth materials include the following raw materials in weight percentage: 1.0% cerium, 0.1% lanthanum, 0.6% neodymium and 0.1% scandium, and the balance is aluminum, and the weighed materials are placed in a drying oven for drying, and then mixed for standby use, the temperature in the drying oven is 100° C., the drying time is 3 hours, and the mixing method is: the dried alloy materials are mixed for the first time to obtain a mixture A, and then the dried rare earth materials are mixed for the second time to obtain a mixture B;
[0049] Step 2: Initial Melting
[0050] First, the aluminum material in step 1 is placed in a vacuum melting furnace for the first heating. After the aluminum material is in a molten state, the alloy material is added and heated for the second time. During the second heating process, the material is stirred. After heating for 20 minutes, the rare earth material is added and heated for the third time. After completion, an aluminum alloy solution is obtained. The first heating temperature is 750°C, the second heating temperature is 770°C, and the third heating temperature is 790°C.
[0051] Step 3: Rare earth doped aluminum alloy casting
[0052] In step 2, after obtaining the aluminum alloy solution, the temperature is lowered to 680° C. and allowed to stand for 30 minutes. After standing, slag is removed. After slag removal, the composition of the aluminum alloy solution is analyzed to ensure that it meets the raw material formula. Then, the temperature is lowered to 600° C. and molded to obtain a rare earth-doped aluminum alloy.
[0053] Step 4: Post-processing
[0054] The obtained rare earth doped aluminum alloy is heat treated by solution treatment and aging treatment to improve the performance of the rare earth doped aluminum alloy, thereby obtaining a high-strength rare earth doped aluminum alloy. The specific steps of preparation, solution treatment and aging treatment are as follows:
[0055] S1: heating the rare earth doped aluminum alloy to 350°C and keeping it at this temperature for 0.5h;
[0056] S2: Raise the temperature to 500°C and keep warm for 10 minutes;
[0057] S2: After keeping warm, lower the temperature to 400℃, keep warm for 20 minutes, and then quickly quench
[0058] S4: After quenching, natural aging treatment is carried out at room temperature for 12 hours.
[0059] Embodiment 3
[0060] according to Figure 1 As shown, this embodiment proposes a high-strength rare earth-doped aluminum alloy, including an alloy material and a rare earth material, the alloy material includes the following raw materials in weight percentage: 0.45% magnesium, 0.4% silicon, 0.10% lithium, 0.15% zirconium, 0.45% copper and 0.07% titanium, the rare earth material includes the following raw materials in weight percentage: 1.3% cerium, 0.15% lanthanum, 0.8% neodymium and 0.2% scandium, the remainder is aluminum and inevitable impurities, the alloy material and the rare earth material are both in powder form, the alloy material and the rare earth material are both in single substance powder form, and the sum of the alloy material, rare earth material, aluminum and inevitable impurities is 100%.
[0061] A method for preparing a high-strength rare earth-doped aluminum alloy comprises the following steps:
[0062] Step 1: Material preparation and processing
[0063] According to the formula proposed in this embodiment, the corresponding alloy material, rare earth material and aluminum material are weighed, wherein the alloy material includes the following raw materials in weight percentage: 0.3% magnesium, 0.3% silicon, 0.05% lithium, 0.1% zirconium, 0.4% copper and 0.05% titanium, and the rare earth material includes the following raw materials in weight percentage: 1.0% cerium, 0.1% lanthanum, 0.6% neodymium and 0.1% scandium, and the balance is aluminum. After weighing, drying is performed, that is, drying is performed in a drying oven, the temperature in the drying oven is 100°C, and the drying time is 4h. After drying, the dried alloy material is subjected to The first mixing is performed to obtain a mixture A, and then the dried rare earth materials are mixed for the second time to obtain a mixture B, which is used for subsequent smelting. In this embodiment, the raw materials are dried for the purpose of performing preliminary pretreatment. The drying process can effectively remove moisture from the raw materials, prevent bubbles and oxidation caused by evaporation of moisture during the smelting process, and reduce the oxide layer on the surface of the raw materials. For easily oxidized metal elements, the oxidation loss during the subsequent smelting process can be reduced by drying, thereby ensuring the accuracy of the alloy composition.
[0064] Step 2: Initial Melting
[0065] After the raw materials are prepared and processed in step 1, aluminum is first melted to obtain aluminum liquid, and then the aluminum material in step 1 is placed in a vacuum melting furnace, smelted in a vacuum environment, and heated for the first time at a temperature of 740° C. After the aluminum material is in a molten state, an alloy material, namely, mixture A, is added, and heated for the second time at a temperature of 755° C., and stirred at the same time. After heating for 30 minutes, a rare earth material, namely, mixture B, is added, and heated for the third time at a temperature of 780° C. After heating and stirring for 25 minutes, an aluminum alloy solution is obtained. In this embodiment, the vacuum melting method can prevent the occurrence of oxidation and nitridation, and at the same time contributes to the uniform distribution of alloy elements, because it reduces the reaction between the melt and the crucible wall, and also reduces the formation of an oxide film on the surface of the melt, which is conducive to the uniform mixing of the components, and then the mechanical properties of the rare earth-doped aluminum alloy can be improved;
[0066] Step 3: Rare earth doped aluminum alloy casting
[0067] On the basis of step 2, after obtaining the aluminum alloy solution, the temperature is lowered to 660°C, and the solution is allowed to stand for 35 minutes. After the solution is allowed to stand, the slag is removed, and then the composition of the aluminum alloy solution is analyzed by photoelectron spectroscopy to ensure that it meets the raw material formula. When the analysis result is different from the raw material formula, the temperature is lowered to 580°C after adding materials for adjustment, and then molded to obtain the rare earth doped aluminum alloy;
[0068] Step 4: Post-processing
[0069] The obtained rare earth doped aluminum alloy is heat treated by solution treatment and aging treatment to improve the performance of the rare earth doped aluminum alloy, thereby obtaining a high-strength rare earth doped aluminum alloy. The specific steps of preparation, solution treatment and aging treatment are as follows:
[0070] S1: heating the rare earth doped aluminum alloy to 300°C and keeping it at this temperature for 0.7h;
[0071] S2: Raise the temperature to 460°C and keep warm for 15 minutes;
[0072] S2: After keeping warm, lower the temperature to 380℃, keep warm for 25 minutes, and then quickly quench
[0073] S4: After quenching, natural aging treatment is carried out at room temperature for 48 hours.
[0074] In combination with Example 1, Example 2 and Example 3, the strength of the high-strength rare earth-doped aluminum alloy provided in Example 1, Example 2 and Example 3 was tested, and a control group was set up. The control group was an aluminum alloy that was not doped with rare earth elements (6% silicon, 1.4% magnesium, 0.35% iron, 0.04% cobalt, 0.04% calcium, 0.02% molybdenum, 0.04% samarium, and the balance was aluminum), which was purchased on the market. The test results are as follows:
[0075] Embodiment 1 Embodiment 2 Embodiment 3 Control group Tensile strength(Mpa) 765 789 810 545 Yield Strength(Mpa) 586 597 608 503 Hardness (HB) 87 89 92 80
[0076] As shown in the above table, the high-strength rare earth-doped aluminum alloys prepared in Example 1, Example 2, and Example 3 have good strength. Specifically, in the present invention, trace rare earth elements cerium, lanthanum, neodymium, and scandium are doped. The trace rare earth elements cerium and lanthanum can refine the grains, promote the refinement of the grains in the aluminum alloy, and improve the mechanical properties of the material. Neodymium can play a strengthening role in the aluminum alloy, improve the strength and hardness of the material, and scandium and zirconium are combined to have a significant strengthening effect in the aluminum alloy.
[0077] Furthermore, magnesium and copper elements can improve the strength and hardness of aluminum alloys, silicon element can improve the casting properties of aluminum alloys and reduce casting defects, lithium element can improve the strength of aluminum alloys, and titanium element promotes grain refinement in aluminum alloys and improves the mechanical properties of materials, thereby improving the strength, hardness and toughness of aluminum alloys.
[0078] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the framework and scope of application of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A high-strength rare earth-doped aluminum alloy, characterized in that: It includes alloy materials and rare earth materials. The alloy material includes the following raw materials in weight percentage: 0.3-0.6% magnesium, 0.3-0.5% silicon, 0.05-0.15% lithium, 0.1-0.2% zirconium, 0.4-0.5% copper and 0.05-0.10% titanium. The rare earth material includes the following raw materials in weight percentage: 1.0-1.5% cerium, 0.1-0.2% lanthanum, 0.6-1.1% neodymium and 0.1-0.3% scandium, and the balance is aluminum and inevitable impurities. The alloy material and rare earth material are both in powder form, and the sum of the alloy material, rare earth material, aluminum and inevitable impurities is 100%.
2. The high-strength rare earth-doped aluminum alloy according to claim 1, characterized in that: It includes alloy materials and rare earth materials, the alloy material includes the following raw materials in weight percentage: 0.6% magnesium, 0.5% silicon, 0.15% lithium, 0.2% zirconium, 0.5% copper and 0.10% titanium, the rare earth material includes the following raw materials in weight percentage: 1.5% cerium, 0.2% lanthanum, 1.1% neodymium and 0.3% scandium, the remainder is aluminum and inevitable impurities, and the sum of the alloy material, rare earth material, aluminum and inevitable impurities is 100%.
3. The high-strength rare earth-doped aluminum alloy according to claim 1, characterized in that: It includes alloy materials and rare earth materials, the alloy material includes the following raw materials in weight percentage: 0.3% magnesium, 0.3% silicon, 0.05% lithium, 0.1% zirconium, 0.4% copper and 0.05% titanium, the rare earth material includes the following raw materials in weight percentage: 1.0% cerium, 0.1% lanthanum, 0.6% neodymium and 0.1% scandium, and the balance is aluminum and inevitable impurities, and the sum of the alloy material, rare earth material, aluminum and inevitable impurities is 100%.
4. A method for preparing a high-strength rare earth-doped aluminum alloy as claimed in claim 1, characterized in that: The following steps are involved: Step 1: Material preparation and processing Accurately weigh the corresponding alloy materials, rare earth materials and aluminum materials according to the formula, and place the weighed materials in a drying oven for drying, and then mix them for standby use after drying; Step 2: Initial Melting First, the aluminum material in step 1 is placed in a vacuum melting furnace and heated for the first time to make the aluminum material molten, then the alloy material is added and heated for the second time. During the second heating, the material is stirred. After heating for 20 to 30 minutes, the rare earth material is added and heated for the third time. After completion, an aluminum alloy solution is obtained; Step 3: Rare earth doped aluminum alloy casting In step 2, after obtaining the aluminum alloy solution, the temperature is lowered to 650-680° C., and the solution is allowed to stand for 30-40 minutes. After the solution is allowed to stand, slag is removed. After the slag is removed, the composition of the aluminum alloy solution is analyzed to ensure that it meets the raw material formula. The temperature is then lowered to 550-600° C., and mold assembly is performed to obtain a rare earth-doped aluminum alloy. Step 4: Post-processing The obtained rare earth doped aluminum alloy is heat treated by solution treatment and aging treatment to improve the performance of the rare earth doped aluminum alloy, thereby obtaining a high-strength rare earth doped aluminum alloy and completing the preparation.
5. The method for preparing a high-strength rare earth-doped aluminum alloy according to claim 4, characterized in that: In the step 1, the temperature in the drying oven is 80-100° C., and the drying time is 3-4 hours.
6. The method for preparing a high-strength rare earth-doped aluminum alloy according to claim 4, characterized in that: In the step 1, the mixing treatment is carried out in the following manner: the dried alloy material is mixed for the first time to obtain a mixture A, and then the dried rare earth material is mixed for the second time to obtain a mixture B.
7. The method for preparing a high-strength rare earth-doped aluminum alloy according to claim 4, characterized in that: In the step 2, the first heating temperature is 720-750°C, the second heating temperature is 740-770°C, and the third heating temperature is 760-790°C.
8. The method for preparing a high-strength rare earth-doped aluminum alloy according to claim 4, characterized in that: In step 4, the specific steps of solution treatment and aging treatment are: S1: heating the rare earth doped aluminum alloy to 250-350°C and keeping the temperature for 0.5-1h; S2: Raise the temperature to 450-500°C and keep warm for 10-20 minutes; S2: After keeping warm, lower the temperature to 350-400℃, keep warm for 20-30 minutes, and then quickly quench. S4: After quenching, natural aging treatment is carried out at room temperature for 12 to 72 hours.
Citation Information
Cited By
A rare earth doped aluminum alloy that can be compression cast and a method of making the same
CN122811574A