High-strength and high-toughness steel suitable for extremely cold areas and production method

By optimizing chemical composition and production process, the problem of difficult balance of strong plastic toughness in extremely cold areas is solved, and high-strength, high-strength and low-cost high-strength toughness steel is achieved, which meets the improvement of low-temperature impact work of -60℃ need.

CN118910498AActive Publication Date: 2024-11-08武汉钢铁有限公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410969800.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

In the application of existing high-strength steel in extremely cold areas, the strong plastic toughness of the material is difficult to balance, resulting in high production costs and insufficient low-temperature impact power of -60℃. The existing technology processes are complex, resulting in high costs.

Method used

By optimizing chemical composition and production process, it includes C: 0.10-0.18%, Si: 0.10-0.25%, Mn: 1.2-1.5%, P: ≤0.015%, S: ≤0.005%, Cr: 0.10-0.30%, Ti: 0.01~0.03%, Nb: 0.02~0.05%, B: 0.001~0.003%, Al: 0.02~0.05%, N≤0.006%, high-pressure water descaling, finishing rolling, quenching and tempering technology are adopted. Control rolling temperature and cooling speed to improve material strength and toughness.

Benefits of technology

A high-strength tough steel with a yield strength ≥750MPa, tensile strength ≥800MPa, and an elongation after break of ≥18%, and a low temperature impact work ≥100J was achieved, reducing production cost by at least 5%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004952818770000061
    Figure BDA0004952818770000061
  • Figure BDA0004952818770000071
    Figure BDA0004952818770000071
  • Figure BDA0004952818770000072
    Figure BDA0004952818770000072
Patent Text Reader

Abstract

The invention discloses high-strength and high-toughness steel suitable for an extremely cold region. The high-strength and high-toughness steel comprises the following components in percentage by weight: 0.10-0.18% of C, 0.10-0.25% of Si, 1.2-1.5% of Mn, less than or equal to 0.015% of P, less than or equal to 0.005% of S, 0.10-0.30% of Cr and the balance of Fe. The alloy comprises the following components in percentage by weight: 0.01 to 0.03 percent of Ti, 0.02 to 0.05 percent of Nb and 0.001 to 0.003 percent of B; 0.02-0.05% of Als and less than or equal to 0.006% of N; the production method comprises the following steps: desulfurizing molten iron, and conventionally smelting to set components; heating the plate blank; descaling with high-pressure water; performing finish rolling after conventional rough rolling; cooling to a coiling temperature and coiling; carrying out pretreatment after transverse cutting; quenching is conducted; tempering is conducted; and standing for later use. Under the conditions that the yield strength is larger than or equal to 750 MPa, the tensile strength is larger than or equal to 800 MPa, the percentage elongation after fracture is larger than or equal to 18%, the-60 DEG C low-temperature impact energy is larger than or equal to 100 J, and the production cost can be reduced by at least 5%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a hot-rolled steel and a production method, and in particular to a high-strength and toughness steel suitable for extremely cold regions and a production method. Background Art

[0002] With the continuous advancement of technology and scientific and technological progress in various industries, the market demand for high-strength steel applications continues to increase. At the same time, the service environment of materials is becoming increasingly severe, so more stringent requirements are put forward for the comprehensive performance of materials, such as high-temperature resistant building structure steel, high-strength steel resistant to various corrosion environments, and low-temperature resistant high-strength steel. However, as the strength of materials continues to increase, the plasticity and toughness of materials will be reduced accordingly. How to balance the strength, plasticity and toughness of materials has become a technical bottleneck for the development of high-strength steel in extremely cold regions.

[0003] Yield strength 700MPa grade high strength steel has been researched and manufactured in domestic and foreign institutions and enterprises. For example, after searching: China Patent Publication No. CN96190123.3 discloses a "high strength steel with excellent low temperature toughness and weldability", whose composition and production process are: C: 0.05-0.10%, Si: ≤0.6%, Mn: 1.7-2.5%, P: ≤0.015%, S: ≤0.003%, Ni: 0.1-1.0%, Mo: 0.15-0.60%, Nb: 0.01-0.10%, Ti: 0.005-0.030%, Al: ≤0.06%, N: 0.001-0.006%, and the rest is iron Fe. This design uses more precious alloys, which greatly increases the overall production cost.

[0004] The Chinese patent publication number is CN98812439.4, which discloses an "ultra-high strength steel with excellent low-temperature toughness", whose composition and production process are: C: 0.04-0.12%, Mn: 0.5-2.5%, Ni: ≥1%, Cu: 0.1-1.50%, Mo: 0.10-0.80%, Nb: 0.02-0.10%, Ti: 0.008-0.030%, Al: 0.001-0.050%, N: 0.002-0.005%, and the rest is iron Fe. The process is to produce the steel billet by offline quenching + tempering process after hot rolling. This design uses a large number of precious alloys, and the cost is high.

[0005] The Chinese patent publication number is CN1757783A, which discloses "A method for manufacturing 700MPa grade F / B high-strength strip steel". Its component composition and production process are: C 0.12-0.18, Si≤0.1, Mn 1.60-2.20, Ti 0.15-0.22, P<0.01, S<0.01, and the rest is iron Fe. The continuous casting billet heating temperature is 1200℃, the rough rolling start temperature is 1150℃, the rough rolling final rolling temperature is 1050℃, the intermediate billet thickness is 32-45mm, the finishing rolling start temperature is 1000-950℃, the finishing rolling final rolling temperature is 790-850℃, and the finishing rolling mill is water-cooled; the cooling rate after rolling is 30-50℃ / s, and the coiling is at 450-600℃, and the product thickness is 3-8mm. This design is mainly aimed at CSP production lines. The thickness specifications are limited and only thin-specification products can be produced. At the same time, the products designed do not show excellent low-temperature toughness characteristics. Summary of the invention

[0006] The present invention aims to overcome the shortcomings of the prior art that the process is complicated, resulting in high cost, and the low-temperature impact energy of -60°C does not exceed 80J, and to provide a high-strength and toughness steel suitable for extremely cold areas and a production method that can reduce the production cost by at least 5% while ensuring the yield strength ≥750MPa, the tensile strength ≥800MPa, the elongation after fracture ≥18%, and the low-temperature impact energy of -60°C ≥100J.

[0007] Measures to achieve the above objectives:

[0008] A high-strength and toughness steel suitable for extremely cold regions, the components and weight percentage contents of which are: C: 0.10-0.18%, Si: 0.10-0.25%, Mn: 1.2-1.5%, P: ≤0.015%, S: ≤0.005%, Cr: 0.10-0.30%, Ti: 0.01-0.03%, Nb: 0.02-0.05%, B: 0.001-0.003%, Als: 0.02-0.05%, N≤0.006%, and the balance is Fe and unavoidable impurities.

[0009] Preferably, the weight percentage of Cr is 0.19-0.26%.

[0010] Preferably, the weight percentage content of B is 0.001-0.0025%.

[0011] A method for producing high-strength and toughness steel suitable for extremely cold regions, comprising the following steps:

[0012] 1) After desulfurization of molten iron, conventional smelting is performed to the set composition;

[0013] 2) After being cast into a slab, the slab is heated, and the heating temperature of the slab is controlled at 1250-1300°C, and the insulation time is 150-170 minutes;

[0014] 3) Perform high-pressure water descaling before rolling, and control the descaling water pressure at 280-420 bar;

[0015] 4) After conventional rough rolling, finishing rolling is carried out, and the reduction ratio of the first two passes is controlled to be greater than 20%, and the cumulative reduction ratio of the first three passes is not less than 50%, and the final rolling temperature is controlled at 810-870°C; the thickness of the finished steel plate is 3-8mm;

[0016] 5) Cooling to a temperature not exceeding 400°C at a cooling rate of not less than 30°C / s and then coiling;

[0017] 6) Pretreatment after cross-cutting: heat the steel plate to 770-800°C in a quenching furnace and keep it at this temperature for 9-11 minutes;

[0018] 7) quenching, cooling to no more than 400°C at a cooling rate greater than 30°C / s;

[0019] 8) Tempering, control the tempering temperature at 500-580°C, and keep warm at this temperature. The holding time is as follows:

[0020] Steel plate thickness t+10min;

[0021] Where: t is the steel plate thickness data in mm;

[0022] 9) Set aside.

[0023] Preferably, the pretreatment heating temperature is between 776°C and 793°C.

[0024] Preferably, the quenching is performed at a cooling rate greater than 35°C / s to a temperature not exceeding 350°C.

[0025] Preferably, the tempering temperature is between 535°C and 568°C.

[0026] Functions and mechanisms of the components and main processes in the present invention

[0027] C: Carbon is a cheap solid solution strengthening element. If its content is less than 0.10%, it cannot meet the hardenability requirements well; if its content is greater than 0.18%, it is easy to precipitate too many carbides during the subsequent tempering process, affecting the toughness of the material. At the same time, too high C content will also affect the welding performance of the material. Therefore, its content is limited to 0.10-0.18%.

[0028] Si: Silicon can purify ferrite and avoid the formation of coarse carbides during cooling, but it is also easy to form Fe2SiO4 and form a eutectic product with FeO on the surface of the steel billet, and solidify into an anchor-like structure, making it difficult to remove FeO and affecting the final surface quality. Therefore, the silicon content is limited to ≤0.25%.

[0029] Mn: Manganese is the most effective element for improving strength and toughness, and can effectively delay pearlite transformation. If its content is less than 1.2%, the material's hardenability and strength requirements cannot be met; manganese also affects the material's welding performance; on the basis of meeting the strength requirements and having good weldability, the manganese content is limited to 1.2-1.5%.

[0030] P: Phosphorus is prone to central segregation, affecting the formability; an appropriate P content can reduce steelmaking costs; after comprehensive consideration, the phosphorus content is controlled to ≤0.015% in the present invention.

[0031] S, N: They are easy to combine with Ti in steel, and high content will lead to sulfide inclusions, affecting the toughness and plasticity of steel; stricter sulfur and nitrogen requirements will increase steelmaking costs. In the present invention, sulfur is controlled at ≤0.005% and nitrogen is controlled at ≤0.006%.

[0032] Cr: Chromium is a carbide-forming element with a strong affinity for carbon, which can hinder the diffusion of carbon atoms. Together with the combined effect of manganese, it significantly delays the transformation of pearlite and bainite, thereby improving the hardenability of the material. In the present invention, the chromium content is controlled to 0.10-0.30%.

[0033] Nb: Niobium is a kind of grain refinement and precipitation strengthening element, which can refine austenite grains and provide a certain precipitation strengthening effect. In the present invention, the niobium content is controlled to be 0.02-0.05%.

[0034] Ti: Titanium is a relatively economical strengthening element. By adding a small amount of Ti, the grains can be refined and the strength and toughness of the material can be improved. In the present invention, the chromium content is controlled to be 0.01-0.03%.

[0035] B: Boron is a strong hardenability element. The addition of B element can greatly improve the hardenability of the material, so that the material has a uniform and refined structure. In the present invention, the chromium content is controlled to 0.001-0.003%.

[0036] Als: Aluminum is an effective deoxidizer in the smelting process and has a certain grain refinement effect, which improves the strength of steel, but it is also easy to form Al2O3 inclusions. In the present invention, the chromium content is controlled at 0.02-0.05%.

[0037] The reason why the reduction rates of the first two passes of the finishing rolling are controlled to be greater than 20%, the cumulative reduction rate of the first three passes is greater than or equal to 50%, and the final rolling temperature is controlled at 810-870°C, is that the austenite grains are fully refined by large reduction in the first three passes, and then the material is rolled at a low final rolling temperature so that a large deformation energy is accumulated in the austenite non-recrystallization zone, which can provide more nucleation points in the subsequent phase transformation process and fully refine the grain size.

[0038] The reason why the coiling temperature is controlled at ≤400° C. in the present invention is to obtain a fine and uniform martensitic matrix structure.

[0039] The reason why the present invention controls the pretreatment after cross-cutting, that is, heating the steel plate to 770-800°C in a quenching furnace and keeping it at this temperature for 9-11 minutes and then quenching, is to precipitate a part of ferrite structure on the martensite matrix and improve the strength, plasticity and toughness of the material.

[0040] The present invention controls the tempering temperature at 500-580°C and performs heat preservation at this temperature. The heat preservation time is based on the thickness of the steel plate t+10min. Tempering in this temperature range can obtain the best performance of strength and toughness matching under this component system.

[0041] Compared with the prior art, the present invention has the advantages of ensuring yield strength ≥ 750MPa and tensile strength

[0042] ≥800MPa, elongation after break ≥18%, and -60℃ low-temperature impact energy ≥100J, the production cost can be reduced by at least 5%. DETAILED DESCRIPTION

[0043] The present invention is described in detail below:

[0044] Table 1 is a list of chemical components of various embodiments and comparative examples of the present invention;

[0045] Table 2 is a list of main process parameters of various embodiments and comparative examples of the present invention;

[0046] Table 3 is a table of performance test results of various embodiments and comparative examples of the present invention.

[0047] Each embodiment of the present invention is produced according to the following steps

[0048] 1) After desulfurization of molten iron, conventional smelting is performed to the set composition;

[0049] 2) After being cast into a slab, the slab is heated, and the heating temperature of the slab is controlled at 1250-1300°C, and the insulation time is 150-170 minutes;

[0050] 3) Perform high-pressure water descaling before rolling, and control the descaling water pressure at 280-420 bar;

[0051] 4) After conventional rough rolling, finishing rolling is carried out, and the reduction ratio of the first two passes is controlled to be greater than 20%, and the cumulative reduction ratio of the first three passes is not less than 50%, and the final rolling temperature is controlled at 810-870°C; the thickness of the finished steel plate is 3-8mm;

[0052] 5) Cooling to a temperature not exceeding 400°C at a cooling rate of not less than 30°C / s and then coiling;

[0053] 6) Pretreatment after cross-cutting: heat the steel plate to 770-800°C in a quenching furnace and keep it at this temperature for 9-11 minutes;

[0054] 7) quenching, cooling to no more than 400°C at a cooling rate greater than 30°C / s;

[0055] 8) Tempering, control the tempering temperature at 500-580°C, and keep warm at this temperature. The holding time is as follows:

[0056] Steel plate thickness t+10min;

[0057] Where: t is the steel plate thickness data in mm;

[0058] 9) Set aside.

[0059] Table 1 Chemical composition list of various embodiments and comparative examples of the present invention (wt%)

[0060]

[0061]

[0062] Table 1

[0063]

[0064] Table 2 List of main process parameters of various embodiments of the present invention and comparative examples

[0065]

[0066]

[0067] Table 2

[0068]

[0069]

[0070] Table 3 List of mechanical properties test results of various embodiments of the present invention and comparative examples

[0071]

[0072] As can be seen from Table 3, compared with the comparative example, the present invention can obtain relatively excellent strength and low-temperature toughness based on the more economical composition design, the yield strength of the material can reach more than 800MPa, the tensile strength can reach more than 850MPa, the elongation after fracture can reach more than 20%, and the low-temperature impact energy of -60℃ can reach more than 130J. On the basis of meeting the above performance, according to statistics, the production cost in the test is reduced by more than 5% compared with the prior art.

[0073] This specific implementation is only the best example and is not a restrictive implementation of the technical solution of the present invention.

Claims

1. A high-strength and toughness steel suitable for extremely cold regions, the components and weight percentages of which are: C: 0.10-0.18%, Si: 0.10-0.25%, Mn: 1.2-1.5%, P: ≤0.015%, S: ≤0.005%, Cr: 0.10-0.30% ; Ti: 0.01~0.03%, Nb: 0.02~0.05, B: 0.001~0.003; Als: 0.02-0.05%, N≤0.006%, the balance is Fe and unavoidable impurities.

2. The high-strength and toughness steel suitable for extremely cold regions as claimed in claim 1, Features: The weight percentage content of Cr is 0.19-0.26%.

3. The high-strength and toughness steel suitable for extremely cold regions as claimed in claim 1, Features: The weight percentage content of B is 0.001-0.0025%.

4. A method for producing a high-strength and toughness steel suitable for use in extremely cold regions as claimed in claim 1, comprising the following steps: 1) After desulfurization of molten iron, conventional smelting is performed to the set composition; 2) After being cast into a slab, the slab is heated, and the heating temperature of the slab is controlled at 1250-1300°C, and the insulation time is 150-170 minutes; 3) Perform high-pressure water descaling before rolling, and control the descaling water pressure at 280-420 bar; 4) After conventional rough rolling, finishing rolling is carried out, and the reduction ratio of the first two passes is controlled to be greater than 20%, and the cumulative reduction ratio of the first three passes is not less than 50%, and the final rolling temperature is controlled at 810-870°C; the thickness of the finished steel plate is 3-8mm; 5) Cooling to a temperature not exceeding 400°C at a cooling rate of not less than 30°C / s and then coiling; 6) Pretreatment after cross-cutting: heat the steel plate to 770-800°C in a quenching furnace and keep it at this temperature for 9-11 minutes; 7) quenching, cooling to no more than 400°C at a cooling rate greater than 30°C / s; 8) Tempering, control the tempering temperature at 500-580°C, and keep warm at this temperature. The holding time is as follows: Steel plate thickness t+10min; Where: t is the steel plate thickness data in mm; 9) Set aside.

5. A method for producing high-strength and toughness steel suitable for extremely cold regions as claimed in claim 4, Features: The pretreatment heating temperature is between 776 and 793°C.

6. A method for producing high-strength and toughness steel suitable for extremely cold regions as claimed in claim 4, Features: The quenching is carried out at a cooling rate greater than 35°C / s to a temperature not exceeding 350°C.

7. A method for producing high-strength and toughness steel suitable for extremely cold regions as claimed in claim 4, Features: The tempering temperature is between 535 and 568°C.

Citation Information

Patent Citations

  • Cryogenic steel of which yield strength is 800 MPa class and production method thereof

    CN102644030A

  • 800 MPa-level high-strength-tenacity steel plate used for engineering machine in extremely cold environment and manufacturing method for 800 MPa-level high-strength-tenacity steel plate

    CN105779899A

  • High tensile strength steel having excellent low temperature toughness and reduced strength anisotropy, and method for producing the same

    JP2008266758A

  • Thick-walled high-strength hot rolled steel sheet with excellent low-temperature toughness and method for producing same