High-strength and high-precision stainless steel seamless steel pipe and manufacturing method thereof

Through specific raw material ratio and process optimization, the problem of insufficient strength and accuracy of existing stainless steel seamless steel pipes is solved, and high-strength and high-precision stainless steel seamless steel pipes are manufactured, meeting the performance requirements of high-end fields and improving corrosion resistance and wear resistance.

CN118910514APending Publication Date: 2024-11-08江苏鸿青新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410985460.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing stainless steel seamless steel pipes have shortcomings in strength, accuracy, etc., and it is difficult to meet the needs of high-end fields.

Method used

Using specific raw material ratios and manufacturing processes, including arc smelting, refining, continuous casting, heating, perforation, pipe rolling, diameter sizing, heat treatment and pickling, etc., by optimizing process parameters such as smelting temperature, pipe rolling speed and heat treatment temperature, Form high-strength, high-precision stainless steel seamless steel pipes.

Benefits of technology

The stainless steel seamless steel pipe produced has tensile strength of more than 1050MPa, yield strength of more than 850MPa, dimensional accuracy of ±0.08mm, and surface roughness of less than 0.4μm. It meets the performance requirements of high-end fields and improves corrosion resistance and wear resistance. , extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910514A_ABST
    Figure CN118910514A_ABST
Patent Text Reader

Abstract

The invention discloses a high-strength and high-precision stainless steel seamless steel tube and a manufacturing method thereof, and relates to the technical field of seamless steel tube manufacturing, the high-strength and high-precision stainless steel seamless steel tube comprises the following raw materials by mass: 18.0-20.0% of chromium (Cr); nickel (N i): 10.0 to 12.0%; molybdenum (Mo): 2.5 to 3.0%; niobium (Nb): 0.1 to 0.3%; titanium (Ti): 0.05 to 0.1%; 0.005%-0.03% of carbon (C) and 0.1%-1.0% of silicon (Si); manganese (Mn): 0.05% to 2.0%; phosphorus (P): 0.005% to 0.035%; sulfur (S): 0.005% to 0.030%; and the balance of iron (Fe) and unavoidable impurities. According to the invention, by optimizing the raw material ratio and the manufacturing process, the manufactured stainless steel seamless steel tube has the characteristics of high strength and high precision, the tensile strength of the stainless steel seamless steel tube can reach more than 1050 MPa, the yield strength of the stainless steel seamless steel tube can reach more than 850 MPa, and the dimensional precision of the stainless steel seamless steel tube can reach + / -0.08 mm; and meanwhile, the stainless steel seamless steel pipe has good toughness and ductility, and can meet the performance requirements of the high-end field on the stainless steel seamless steel pipe.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of seamless steel pipe manufacturing, in particular to a high-strength and high-precision stainless steel seamless pipe and a manufacturing method thereof. Background Art

[0002] Stainless steel seamless pipes have good corrosion resistance, high temperature resistance and high strength, and are widely used in the fields of petroleum, chemical industry, aerospace, machinery manufacturing, etc. With the rapid development of equipment manufacturing industry, the demand for small-hole thick-walled seamless pipes used in some special equipment is increasing.

[0003] At present, the main industrial methods for producing seamless pipes are deep hole machining, hot extrusion and hot perforation. Among them, the hot perforation pipe is made by obliquely rolling and perforating the hot bar billet to obtain a rough pipe, and then hot rolling to reduce the diameter and wall, and then rolling through a sizing unit to obtain a seamless pipe of the target size. However, the existing stainless steel seamless pipes still have certain deficiencies in strength and precision, and it is difficult to meet the needs of some high-end fields.

[0004] In view of this, this application is hereby filed. Summary of the invention

[0005] The object of the present invention is to provide a high-strength and high-precision stainless steel seamless pipe and a manufacturing method thereof to solve the problems raised in the above-mentioned background technology.

[0006] In order to solve the above technical problems, the present invention provides a high-strength and high-precision stainless steel seamless pipe and a manufacturing method thereof, comprising the following composition, the raw materials are calculated by mass %: chromium (Cr): 18.0-20.0%; nickel (Ni): 10.0-12.0%; molybdenum (Mo): 2.5-3.0%; niobium (Nb): 0.1-0.3%; titanium (Ti): 0.05-0.1%; carbon (C): 0.005%-0.03%; the balance is iron (Fe) and inevitable impurities;

[0007] Furthermore, the raw materials are calculated by mass % as follows: chromium (Cr): 19.0%; nickel (Ni): 11.0%; molybdenum (Mo): 2.8%; niobium (Nb): 0.2%; titanium (Ti): 0.08%; and carbon (C): 0.02%.

[0008] Furthermore, it also includes silicon (Si): 0.1%-1.0%; manganese (Mn): 0.05%-2.0%; phosphorus (P): 0.005%-0.035%; sulfur (S): 0.005%-0.030%; wherein silicon (Si) 0.8%; manganese (Mn)

[0009] 1.5%; Phosphorus (P) 0.025%; Sulfur (S) 0.020%.

[0010] A method for manufacturing a high-strength and high-precision stainless steel seamless pipe comprises the following steps: S1: smelting: smelting the raw materials in an electric arc furnace at a smelting temperature of 1550-1650°C for 2-3 hours to obtain molten steel; S2: refining: transferring the molten steel to a refining furnace for refining at a refining temperature of 1600-1700°C for 1-2 hours, while introducing argon gas into the molten steel for stirring to remove inclusions and gas in the molten steel; S3: continuous casting: continuously casting the refined molten steel to obtain a steel billet, wherein during the continuous casting process, the billet drawing speed is 1.0-1.5 m / min, and the cooling water volume of the crystallizer is 80-100 m 3 / h; S4: Heating: Put the steel billet into the heating furnace for heating, the heating temperature is 1150-1250℃, the heating time is 2-3 hours, and ensure that the steel billet is evenly heated; S5: Punching: Use a conical puncher to punch the heated steel billet, the punching speed is 80-100 times / min, and the punching head diameter is 0.8-0.9 times the billet diameter; S6: Pipe rolling: The perforated rough pipe is rolled, using a three-roller pipe mill, the rolling speed is 50-60 times / min, and the roller diameter is 300-400mm; S7: Sizing: Sizing the steel pipe after pipe rolling, using a sizing machine, the sizing speed is 30-40 times / min, and the sizing roller diameter is 200-300mm; S8: Heat treatment: The sizing steel pipe is solution treated, the treatment temperature is 1050-1150℃, the insulation time is 1-2 hours, and then rapidly cooled.

[0011] Furthermore, the power of the electric arc furnace is 5000-6000kW, and the furnace capacity is 20-30t; the power of the refining furnace is 3000-4000kW, and the furnace capacity is 15-20t.

[0012] Furthermore, the piercing force of the tapered piercer is 5000-6000 kN, and the piercing taper is 5-8°; the rolling force of the three-roller tube mill is 8000-10000 kN, and the roller speed is 100-150 r / min.

[0013] Furthermore, it also includes S9: pickling: pickling the heat-treated steel pipe to remove oxide scale and impurities on the surface.

[0014] Furthermore, it also includes S10: Inspection: inspecting the steel pipe after pickling to ensure that the dimensional accuracy, mechanical properties and surface quality of the steel pipe meet the requirements.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] 1. The stainless steel seamless pipe manufactured by the present invention has the characteristics of high strength and high precision. Its tensile strength can reach more than 1050MPa, its yield strength can reach more than 850MPa, and its dimensional accuracy can reach ±0.08mm; the surface roughness Ra value is less than 0.4μm, and it has good toughness and ductility, which can meet the performance requirements of stainless steel seamless pipes in high-end fields.

[0017] 2. By optimizing the raw material ratio and manufacturing process, the corrosion resistance and wear resistance of the steel pipe are improved, and the service life of the steel pipe is extended.

[0018] 3. The manufacturing method of the present invention has simple process, easy operation, high production efficiency, low cost, and good economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The present invention is a flow chart of a method for manufacturing a high-strength and high-precision stainless steel seamless pipe. DETAILED DESCRIPTION

[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] See also Figure 1 , the present invention provides a technical solution:

[0022] Embodiment 1:

[0023] See also Figure 1 As shown, a high-strength and high-precision stainless steel seamless steel pipe includes the following composition, the raw materials are calculated by mass %: chromium (Cr): 19.0%; nickel (Ni): 11.0%; molybdenum (Mo): 2.8%; niobium (Nb): 0.2%; titanium (Ti): 0.08%; carbon (C): 0.02%; silicon (Si): 0.8%; manganese (Mn):

[0024] 1.5%; Phosphorus (P): 0.025%; Sulfur (S): 0.020%.

[0025] Among them: Chromium (Cr): Its main function is to improve the corrosion resistance and oxidation resistance of stainless steel. It plays a role in the entire manufacturing process, especially in the refining and heat treatment steps, which helps to form a stable oxide layer and enhance the corrosion resistance of the steel pipe.

[0026] Nickel (Ni): It can improve the toughness, ductility and corrosion resistance of stainless steel. It affects the performance of steel pipes in various links such as smelting and refining.

[0027] Molybdenum (Mo): Enhances the corrosion resistance and high temperature strength of stainless steel. Its role is reflected in the smelting, refining and subsequent heat treatment steps.

[0028] Niobium (Nb): It can refine the grains and improve the strength and toughness. It plays a role in melting and subsequent hot working steps.

[0029] Titanium (Ti): It stabilizes carbon and prevents intergranular corrosion. It is added during the smelting process and its role runs through the entire manufacturing process.

[0030] Carbon (C): A moderate amount of carbon can improve the strength of steel, but too much carbon will reduce toughness and corrosion resistance. Controlling its content during smelting has an important impact on the performance of subsequent steel pipes.

[0031] Silicon (Si): helps improve the oxidation resistance and strength of steel. Its role is manifested in the melting and refining steps.

[0032] Manganese (Mn): It has the functions of deoxidation and desulfurization, and can improve the strength of steel. It plays a role in the smelting process.

[0033] Phosphorus (P) and sulfur (S): These elements are impurity elements. They have limited direct effect on grain refinement, but controlling their content helps maintain the purity and overall performance of steel. Their content needs to be strictly controlled to avoid reducing the toughness and corrosion resistance of steel. They should be removed as much as possible during the smelting and refining process.

[0034] Embodiment 2:

[0035] See also Figure 1 As shown, a high-strength and high-precision stainless steel seamless steel pipe includes the following composition, the raw materials are calculated by mass %: chromium (Cr): 17.5%; nickel (Ni): 9.5%; molybdenum (Mo): 2.2%; niobium (Nb): 0.08%; titanium (Ti): 0.04%; carbon (C): 0.03%; silicon (Si): 1.2%; manganese (Mn):

[0036] 2.5%; Phosphorus (P): 0.038%; Sulfur (S): 0.032%.

[0037] Embodiment three:

[0038] See also Figure 1As shown, a high-strength and high-precision stainless steel seamless steel pipe includes the following composition, the raw materials are calculated by mass %: chromium (Cr): 20.5%; nickel (Ni): 12.5%; molybdenum (Mo): 3.2%; niobium (Nb): 0.35%; titanium (Ti): 0.12%; carbon (C): 0.01%; silicon (Si): 0.5%; manganese (Mn):

[0039] 1.0%; Phosphorus (P): 0.020%; Sulfur (S): 0.015%.

[0040] Embodiment 4:

[0041] See also Figure 1 As shown, a high-strength and high-precision stainless steel seamless steel pipe includes the following composition, the raw materials are calculated by mass %: chromium (Cr): 18.0%; nickel (Ni): 10.0%; molybdenum (Mo): 2.5%; niobium (Nb): 0.1%; titanium (Ti): 0.05%; carbon (C): 0.04%; silicon (Si): 1.5%; manganese (Mn):

[0042] 2.8%; Phosphorus (P): 0.040%; Sulfur (S): 0.035%.

[0043] Embodiment five:

[0044] See also Figure 1 As shown, a high-strength and high-precision stainless steel seamless steel pipe includes the following composition, the raw materials are calculated by mass %: chromium (Cr): 19.5%; nickel (Ni): 11.5%; molybdenum (Mo): 2.7%; niobium (Nb): 0.25%; titanium (Ti): 0.09%; carbon (C): 0.025%; silicon (Si): 0.6%; manganese (Mn):

[0045] 1.2%; Phosphorus (P): 0.030%; Sulfur (S): 0.025%.

[0046] A method for manufacturing a high-strength and high-precision stainless steel seamless pipe comprises the following steps:

[0047] S1: Melting: The raw materials are melted in an electric arc furnace at a temperature of 1550-1650°C for 2-3 hours to obtain molten steel; various raw materials are melted at high temperature in an electric arc furnace to form uniform molten steel, so that various elements are fully mixed, providing a basis for subsequent refining;

[0048] S2: Refining: The molten steel is transferred to a refining furnace for refining at a refining temperature of 1600-1700°C for 1-2 hours. At the same time, argon gas is introduced into the molten steel for stirring to remove inclusions and gases in the molten steel; the inclusions and gases in the molten steel are further removed to improve the purity of the molten steel, reduce impurities, improve the quality of the steel, and improve the performance and reliability of the steel pipe;

[0049] S3: Continuous casting: The refined molten steel is continuously cast to obtain steel billets. During the continuous casting process, the billet drawing speed is 1.0-1.5m / min, and the cooling water volume of the crystallizer is 80-100m 3 / h; solidify the refined molten steel into billets; realize continuous production and improve production efficiency; at the same time, control the billet drawing speed and the amount of cooling water in the crystallizer to help obtain good billet structure;

[0050] S4: Heating: Place the steel billet in a heating furnace for heating at a temperature of 1150-1250°C for 2-3 hours to ensure that the steel billet is evenly heated; make the steel billet reach a suitable temperature for subsequent processing, ensure that the steel billet is evenly heated, reduce internal stress, and improve processing performance;

[0051] S5: Punching: Use a conical puncher to punch holes in the heated billet at a speed of 80-100 times / min. The diameter of the punch head is 0.8-0.9 times the billet diameter. Initial holes are formed on the billet, providing a basis for subsequent pipe rolling processes. Controlling the piercing speed and head diameter can ensure the quality and dimensional accuracy of the holes.

[0052] S6: Pipe rolling: The perforated rough pipe is rolled using a three-roller pipe rolling mill with a rolling speed of 50-60 times / min and a roller diameter of 300-400mm; the perforated rough pipe is further rolled into the required pipe diameter and wall thickness; the dimensional accuracy and internal structure of the steel pipe are improved, and the mechanical properties are improved;

[0053] S7: Sizing: Sizing the steel pipe after rolling, using a sizing machine with a sizing speed of 30-40 times / min and a sizing roller diameter of 200-300mm; accurately control the outer diameter of the steel pipe to reach the specified size; ensure the dimensional accuracy of the steel pipe to meet the use requirements;

[0054] S8: Heat treatment: The sizing steel pipe is subjected to solution treatment at a temperature of 1050-1150°C for 1-2 hours, followed by rapid cooling. Through solution treatment, the alloy elements are fully dissolved, the structure and performance are improved, and the strength, toughness and corrosion resistance of the steel pipe are improved.

[0055] S9: Pickling: Pickling the heat-treated steel pipe to remove the oxide scale and impurities on the surface; remove the oxide scale and impurities on the surface of the steel pipe; improve the surface quality of the steel pipe, enhance the appearance and corrosion resistance;

[0056] S10, Inspection: Inspect the steel pipes after pickling to ensure that the dimensional accuracy, mechanical properties and surface quality of the steel pipes meet the requirements; inspect the dimensional accuracy, mechanical properties and surface quality of the steel pipes; ensure that the steel pipes meet the quality standards, ensure product quality, and improve product reliability and safety.

[0057] The experimental data are as follows:

[0058] In Example 1, the steel pipe performance values ​​are obtained: tensile strength: 1050 MPa; yield strength: 850 MPa; dimensional accuracy: ±0.08 mm; surface roughness Ra value is less than 0.4 μm;

[0059] In Example 2, the steel pipe performance values ​​are obtained: tensile strength: 900 MPa; yield strength: 700 MPa; dimensional accuracy: ±0.12 mm; surface roughness Ra value is less than 0.5 μm;

[0060] In Example 3, the steel pipe performance values ​​are obtained: tensile strength: 1000 MPa; yield strength: 850 MPa; dimensional accuracy: ±0.09 mm; surface roughness Ra value is less than 0.4 μm;

[0061] In Example 4, the steel pipe performance values ​​are obtained: tensile strength: 850MPa; yield strength: 650MPa; dimensional accuracy: ±0.15mm; surface roughness Ra value is less than 0.5μm

[0062] In Example 5, the steel pipe performance values ​​obtained are: tensile strength: 950 MPa; yield strength: 750 MPa; dimensional accuracy: ±0.10 mm; surface roughness Ra value is less than 0.4 μm.

[0063] In summary, the steel pipe prepared by adopting the raw material ratio of embodiment 1 through the steps of smelting, refining, continuous casting, heating, perforating, tube rolling, sizing, heat treatment, pickling and inspection has the best performance value of tensile strength: 1050 MPa; yield strength: 850 MPa; dimensional accuracy: ±0.08 mm; surface roughness Ra value less than 0.4 μm.

Claims

1. A high-strength and high-precision stainless steel seamless pipe, characterized in that: It includes the following composition, the raw materials are calculated by mass %: Chromium (Cr): 18.0-20.0%; Nickel (Ni): 10.0-12.0%; Molybdenum (Mo): 2.5-3.0%; Niobium (Nb): 0.1-0.3%; Titanium (Ti): 0.05-0.1%; Carbon (C): 0.005%-0.03%; the balance is iron (Fe) and inevitable impurities.

2. A high-strength and high-precision stainless steel seamless pipe as claimed in claim 1, characterized in that: The raw materials are calculated by mass % as follows: chromium (Cr): 19.0%; nickel (Ni): 11.0%; molybdenum (Mo): 2.8%; niobium (Nb): 0.2%; titanium (Ti): 0.08%; Carbon (C): 0.02%.

3. The high-strength and high-precision stainless steel seamless pipe according to claim 1, characterized in that: It also includes silicon (Si): 0.1%-1.0%; manganese (Mn): 0.05%-2.0%; phosphorus (P): 0.005%-0.035%; sulfur (S): 0.005%-0.030%; among which, silicon (Si) 0.8%; manganese (Mn) 1.5%; phosphorus (P) 0.025%; Sulfur (S) 0.020%.

4. A method for manufacturing a high-strength and high-precision stainless steel seamless pipe, characterized in that: The following steps are involved: S1: Melting: Melting the raw materials in an electric arc furnace at a temperature of 1550-1650°C for 2-3 hours to obtain molten steel; S2: Refining: The molten steel is transferred to a refining furnace for refining at a temperature of 1600-1700°C for 1-2 hours, while argon is introduced into the molten steel for stirring to remove inclusions and gases in the molten steel; S3: Continuous casting: The refined molten steel is continuously cast to obtain steel billets. During the continuous casting process, the billet drawing speed is 1.0-1.5m / min, and the cooling water volume of the crystallizer is 80-100m 3 / h; S4: Heating: Place the steel billet in a heating furnace for heating at a temperature of 1150-1250°C for 2-3 hours to ensure that the steel billet is evenly heated; S5: Punching: The heated billet is punched with a conical puncher at a speed of 80-100 times / min, and the punch head diameter is 0.8-0.9 times the billet diameter; S6: Pipe rolling: The perforated rough pipe is rolled using a three-roller pipe rolling mill with a rolling speed of 50-60 times / min and a roller diameter of 300-400 mm; S7: Sizing: Sizing the steel pipe after rolling, using a sizing machine, the sizing speed is 30-40 times / min, and the diameter of the sizing roller is 200-300mm; S8: Heat treatment: The sized steel pipe is subjected to solution treatment at a temperature of 1050-1150°C for 1-2 hours, followed by rapid cooling.

5. The method for manufacturing a high-strength and high-precision stainless steel seamless pipe according to claim 4, characterized in that: The power of the electric arc furnace is 5000-6000kW, and the furnace capacity is 20-30t; the power of the refining furnace is 3000-4000kW, and the furnace capacity is 15-20t.

6. The method for manufacturing a high-strength and high-precision stainless steel seamless pipe according to claim 4, characterized in that: The piercing force of the tapered piercing machine is 5000-6000 kN, and the piercing taper is 5-8°; the rolling force of the three-roller tube mill is 8000-10000 kN, and the roller speed is 100-150 r / min.

7. The method for manufacturing a high-strength and high-precision stainless steel seamless pipe according to claim 4, characterized in that: Also includes S9: Pickling: Pickling the heat-treated steel pipe to remove surface oxide scale and impurities.

8. The method for manufacturing a high-strength and high-precision stainless steel seamless pipe according to claim 4, characterized in that: Also includes S10: Inspection: Inspect the steel pipe after pickling to ensure that the dimensional accuracy, mechanical properties and surface quality of the steel pipe meet the requirements.