Steel for gear of gear box of new energy automobile and production method of steel
By using the 'vacuum degassing + continuous casting' process and specific chemical components in the production of gear steel for gear boxes of new energy vehicles, the problems of poor production continuity and unstable quality of traditional mold casting processes are solved, and high purity is achieved. The steel production with high mechanical properties and long life meets the high performance requirements of gearbox gears of new energy vehicles.
Patent Information
- Application Number
- CN202410573499.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-10
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-05-10
AI Technical Summary
The existing technology is difficult to produce and meet the requirements of high purity, high mechanical properties and long life of gear steel for gear boxes of new energy vehicles. The traditional mold casting process has problems such as poor production continuity, unstable quality and high cost, and vacuum degassing + Continuous casting process is not yet mature.
Using the 'vacuum degassing + continuous casting' process, the design of unique chemical composition and process flows, including initial refining of converter or electric furnace, ladle refining furnace refining, vacuum degassing, continuous casting, heating rolling, isothermal annealing and other steps, reduce the Non-metallic inclusions improve the purity and mechanical properties of steel, design chemical components such as C: 0.25-0.31%, Si: 0.2-0.4%, Mn: 1.0-1.3%, etc., and refine the grains with Nb and V to improve the Austenitic stability.
The steel for gears for new energy vehicle gearboxes with high cleanliness, high tissue uniformity, high hardenability and high fatigue life has high mechanical properties and long life not available in traditional mold casting technology, and has good process continuity , stable quality and more economical cost.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the iron-based alloy technology in the field of metallurgy, and more specifically relates to steel for automobile gear box gears and a production method thereof. Background Art
[0002] As the automobile market continues to develop and improve, environmental protection issues have gradually attracted global attention, and the new energy automobile industry, which has the advantages of low energy consumption and low pollution, has rapidly emerged. In order to meet people's increasing demand for automobile performance, higher requirements are placed on the performance of new energy vehicles compared to traditional vehicles, especially on their gearboxes: high efficiency, high wear resistance and high stability.
[0003] Automobile gearbox is a key component of new energy vehicles, and gearbox gear is an important component of gearbox transmission system. Gearbox gears are subjected to strong multiple alternating loads and impacts when running at high speed. In order to ensure the efficient, stable and reliable operation of gearbox gears, higher requirements are put forward for gearbox gear steel of new energy vehicles. Therefore, its material should have the following properties: high purity, high mechanical properties and long life. At present, domestic steel mills mainly produce such gear steel by die casting process, but this process has obvious disadvantages such as poor production continuity, unstable quality of different batches and high production cost. The "vacuum degassing + continuous casting" process with good production continuity, stable quality and more economical cost is not mature for the production of such rack steel, and the gear steel produced by the "vacuum degassing + continuous casting" process cannot meet the requirements of such gear steel. Therefore, the research and development of the "vacuum degassing + continuous casting" process to produce such gear steel is imperative. Summary of the invention
[0004] In order to obtain high-purity, high-mechanical-property and long-life new-energy vehicle gearbox gear steel, the present invention adopts a "vacuum degassing + continuous casting" process with good production continuity, stable quality and more economical, by reducing non-metallic inclusions, improving the purity of steel, reducing oxygen content and the content of residual harmful elements; adding appropriate special trace elements to improve mechanical properties and wear resistance; improving the uniformity of steel structure by designing a unique continuous casting process and a high-temperature rolling process, and developing a new production method for new-energy vehicle gearbox gear steel that meets market needs.
[0005] In order to meet the performance requirements of high cleanliness, fine grains, high mechanical properties and other performance requirements of steel for gearbox gears of new energy vehicles, the present invention has carried out a unique and reasonable chemical composition design, and its chemical composition design is as follows:
[0006] The mass percentage is C: 0.25-0.31%, Si: 0.2-0.4%, Mn: 1.0-1.3%, Cr: 1.0-1.3%, Ni: 0.2-0.3%, Nb: 0.010-0.020%, V: 0.03-0.06%, Al: 0.02-0.05%, N: 0.0080-0.0110%, S≤0.005%, P≤0.020%, Cu≤0.20%, Mo≤0.10%, Ti≤0.002%, O≤0.0009%, As≤0.04%, Sn≤0.03%, Sb≤0.005%, Pb≤0.002%, and the balance is Fe and unavoidable impurities.
[0007] 1) Determination of C content
[0008] C is the most basic element in steel and the most economical strengthening element. Among all elements, carbon has the greatest ability to improve steel strength. The strengthening effect of carbon on quenched and tempered steel is about 9 times that of chromium and 18 times that of manganese. Therefore, in order to ensure that the core of the gear has good toughness after carburizing heat treatment, the steel needs to have a suitable carbon content. The range of the C content in the present invention is determined to be 0.25-0.31%.
[0009] 2) Determination of Si content
[0010] Si is solid-dissolved in the ferrite phase and has a strong solid-solution strengthening effect, which can improve the strength, elastic limit and hardenability, but at the same time reduce the plasticity and toughness of the ferrite. The Si content of the steel of the present invention is determined to be in the range of 0.2-0.4%.
[0011] 3) Determination of Mn content
[0012] Mn, as a deoxidizing element in the steelmaking process, can improve the hardenability of steel. Mn can also fix the form of sulfur in steel and form MnS and (Fe, Mn)S, which are less harmful to the performance of steel, and reduce or inhibit the formation of FeS. Therefore, manganese in steel can improve the purity and performance of steel. At the same time, manganese plays the role of solid solution strengthening and grain refinement in steel to improve strength and significantly improve hardenability; however, if the manganese content is too high, it will promote the growth of austenite grains in steel. The range of Mn content in the present invention is determined to be 1.0-1.3%.
[0013] 4) Determination of Cr content
[0014] Cr can increase the hardenability of steel and has a secondary hardening effect, which can play a solid solution strengthening role on steel and improve the hardenability of steel. In addition, Cr reduces the activity of C, which can reduce the overheating tendency and surface decarburization rate of steel. However, if the Cr content is too high, it will combine with the carbon in the steel to easily form large carbides. Such insoluble carbides reduce the toughness of the steel and reduce the life of the gear. Therefore, the range of the Cr content in the present invention is determined to be 1.0-1.3%.
[0015] 5) Determination of Ni content
[0016] Ni strengthens ferrite and refines pearlite in steel, is an element that improves the hardenability of steel, and is also the most commonly used element that effectively improves the wear resistance of steel. Ni and Cr and residual P in steel combine to help improve the corrosion resistance and wear resistance of steel. The content of Ni in the present invention is determined to be in the range of 0.2% to 0.3%.
[0017] 6) Determination of Nb and V content
[0018] By adding Nb and V to steel, the CCT curve of the steel can be moved to the lower right, and the stability of austenite can be increased. Most of the Nb in the steel exists in the form of carbide, nitride, and carbonitride precipitates. Such precipitates are usually nano-sized. These dispersed small-sized precipitates can pin the austenite grain boundaries, hinder the growth of austenite grains, and refine the austenite grains of the steel. The Nb content of the present invention is designed to be 0.010% to 0.020%, and the V content is designed to be 0.03% to 0.06%.
[0019] 7) Determination of Al content
[0020] Al is added as a deoxidizing element in steel. In addition to reducing the dissolved oxygen in the molten steel, Al and N form dispersed and fine aluminum nitride to refine the grains. However, when the Al content is too high, large particles of Al2O3 and other brittle inclusions are easily formed during the molten steel smelting process, which reduces the purity of the molten steel and affects the service life of the steel. The Al content of the present invention is determined to be in the range of 0.02-0.05%.
[0021] 8) Determination of N content
[0022] The N element precipitates with Nb, Ti, Al, etc. in the form of nitrides, which can significantly improve the stability of high-temperature austenite grains in gear steel and prevent the growth of high-temperature austenite grains. The nitrogen content of the present invention is determined to be N: 0.0080-0.0110%.
[0023] 9) Determination of Ti content
[0024] During the solidification of molten steel, Ti can easily combine with N or C to form TiN or Ti(C,N) non-metallic inclusions, which are usually blocky inclusions with "angular" shapes. Such inclusions have high hardness, seriously affecting the uniformity of the structure, and easily causing stress concentration at the angular parts during operation, seriously reducing the fatigue life of the bearing. The range of Ti content in the present invention is determined to be ≤0.002%.
[0025] 10) Determination of O content
[0026] Oxygen is the oxygen that naturally enters the steel during the steelmaking process and remains in the steel at a later stage. Oxygen exists in the steel mainly in the form of non-metallic inclusions such as SiO2 and Al2O3. In particular, Al2O3 inclusions seriously affect the fatigue life of bearings. A large number of fatigue life tests have shown that reducing the oxygen content is significantly beneficial to improving the purity of steel, especially reducing the content and size of oxide brittle inclusions. The range of the O content in the present invention is determined to be ≤0.0009%.
[0027] 11) Determination of P and S content
[0028] P causes serious segregation during solidification in steel. P dissolves in ferrite to cause grain distortion and coarsening, and increases cold brittleness. The content of P in the present invention is determined to be ≤0.020%; S causes hot brittleness in steel, reduces the ductility and toughness of steel, and the content of S in the present invention is determined to be ≤0.005%.
[0029] 12) Determination of As, Sn, Sb, and Pb content
[0030] Trace elements such as As, Sn, Sb, and Pb are all low-melting-point nonferrous metals. Their presence in steel causes soft spots on the surface of parts and uneven hardness. Therefore, they are regarded as harmful elements in steel. The content range of these elements in the present invention is determined as As≤0.04%, Sn≤0.03%, Sb≤0.005%, and Pb≤0.002%.
[0031] In order to obtain a new energy vehicle gearbox gear steel with high cleanliness, high mechanical properties, fine grains and long life, the present invention also clearly defines that the steel has the following main technical indicators:
[0032] The macrostructure of the steel of the present invention is inspected and graded according to GB / T226 and GB / T 1979, requiring that general porosity, central porosity and ingot-shaped segregation should not exceed level 1.5, and shrinkage cavities, cracks and subcutaneous bubbles are not allowed to appear.
[0033] The grain size of the steel material of the present invention is tested and graded by the carburizing method according to GB / T6394, and the grain size is required to be ≥7.5.
[0034] The non-metallic inclusions in the steel of the present invention are tested according to the K method of DIN 50602 standard, and the levels of various inclusions do not exceed the requirements of Table 1.
[0035] Table 1
[0036] category K1(S) K1(O) K3(S) K3(O) level 1.0 2.0 1.0 1.0
[0037] The macro defects of the steel of the present invention are tested by water immersion high frequency flaw detection method according to SEP 1927 (water immersion ultrasonic determination method for purity of forged steel bars), and the length of a single inclusion does not exceed 1mm, and the defect index does not exceed 5mm / dm3 .
[0038] The end hardenability of the steel of the present invention is tested according to GB / T225, and the heat treatment system is: normalizing at 920±10°C, keeping warm for 1 hour, air cooling; end quenching at 900±5°C, water cooling, and requiring J5≥55HRC and J7≥50HRC.
[0039] The mechanical properties of the steel of the present invention are tested according to GB / T228, and the specific requirements are shown in Table 2 below.
[0040] Table 2
[0041]
[0042] The steel of the present invention is subjected to a rotation bending fatigue life test according to GB / T 4337-2015. At room temperature (20°C ± 5°C) and 1000MPa cyclic stress conditions, data statistics and analysis are performed according to GB / T 24176-2009. The final requirement is that the rotation bending fatigue life of the steel is ≥1×10 7 Second-rate.
[0043] The present invention discloses a production method for gear steel used in gearboxes of new energy vehicles, and the process flow thereof comprises the following steps: primary refining in a converter or an electric furnace → refining in a ladle refining furnace (LF furnace) → vacuum degassing in an RH furnace or a VD furnace → continuous casting CCM (large cross-section) → heating and rolling → stack cooling → isothermal annealing → finishing → surface and internal flaw detection → packaging.
[0044] The main steps are as follows:
[0045] (1) Molten steel smelting:
[0046] Primary smelting in converter or electric furnace: high-quality molten iron, low-sulfur scrap steel (containing S≤0.01%) and raw and auxiliary materials are added to the converter or electric furnace for primary smelting. Oxygen is blown into the top of the furnace mouth for oxidation reaction, and argon is blown into the bottom for stirring. 35-40 cubic meters of oxygen and 5-6 cubic meters of argon are blown into one ton of steel, and active composite lime (CaO-SiO2-CaF2) is added. Under the combined action of oxygen and argon, harmful elements phosphorus (P≤0.020%) and titanium (Ti≤0.002%) are removed. The final carbon content when tapping from the primary smelting furnace is 0.15%-0.18%, and the tapping temperature is ≥1640℃. Slag blocking is used for tapping, and some alloys are added during tapping (initial adjustment of composition). After tapping, it is quickly lifted to the refining LF furnace for smelting.
[0047] Ladle refining furnace refining: During LF refining, SiC is added to the surface of the molten steel for diffusion deoxidation, and Al wire is fed into the molten steel for precipitation deoxidation. CaO-SiO2-MgO high-performance composite slag-making agent is added to the surface of the molten steel for diffusion deoxidation and adsorption to remove harmful non-metallic inclusions. During the smelting process, SiC (50-100Kg) is first added to the molten steel, and then Al wire (80-120m) is fed, and CaO-SiO2-MgO high-performance composite slag-making agent (300-350Kg) is added again, the ladle protection cover is covered, argon is connected to the bottom of the ladle, and then the electrode is inserted into the slag for submerged arc power supply. The molten steel is temperature measured and sampled for analysis every 15 minutes of power outage, and the required main elements (V, Nb, etc.) are added according to the target requirements. The number of temperature measurement and sampling of the refining furnace is controlled at 3-4 times until the composition meets the product requirements. The refining time is controlled to be more than 50 minutes, and the soft blowing time of the molten steel is ≥15 minutes.
[0048] Vacuum degassing: During RH or VD vacuum degassing, the maximum vacuum degree in the vacuum furnace is ≤1mbar, and the vacuum circulation treatment time of molten steel is maintained at ≥15min to ensure that harmful gases in the steel are effectively removed. After the vacuum treatment, argon is blown into the bottom of the ladle, and the argon flow rate is controlled so that the molten steel is not exposed to the air. The soft blowing time of the molten steel is ≤15min. At the same time, 80-100m of silicon-calcium wire is fed to convert Al2O3 or MgO·A12O3 in the molten steel into calcium aluminate and composite inclusions with lower melting points to further remove harmful inclusions.
[0049] (2) Continuous casting: Argon protection is used throughout the casting process to prevent secondary contamination and oxidation of the molten steel; preferably, large cross-sections of 300 mm×300 mm and above are used for continuous casting, and low superheat casting (superheat △T≤25°C) is adopted; the amount of molten steel in the tundish is controlled at 25 to 30 tons, and a light pressure control technology (pressure reduction of 13 mm to 15 mm) is adopted, and the casting speed is 0.4 to 0.6 m / min; an appropriate steel flow to water ratio (0.8 to 1.0 L / kg) is used, and electromagnetic stirring is used in the tundish to interrupt the bridging of the columnar crystal zone during the solidification of the continuous casting billet; through the above various control technologies, the central segregation of steel is further improved and the uniformity of steel structure is improved.
[0050] (3) Heating rolling: The continuous casting billet is hot sent to a heating furnace in a neutral or weakly oxidizing atmosphere for heating and then rolled into round bars. The specific rolling process is as follows: the continuous casting billet enters a walking beam heating furnace through a conveyor roller, the steel is heated to 1220℃~1260℃ in the heating furnace, the total heating time is ≥3h, the start rolling temperature is 1050℃~1150℃, the final rolling temperature is controlled to be ≥950℃, and a five-pass reciprocating turning large reduction technology is adopted (the steel is turned 90° after each pass of pressing), and the five-pass reduction amounts are 25%~30%, 15%~20%, 20%~25%, 15%~20%, and 10%~15% respectively, so that the core structure of the billet is deformed and recrystallized first during the deformation process, so that the central structure of the steel is more uniform and dense under the action of large pressure. The steel is then rolled alternately through 8 horizontal and vertical rolling mills, and finally rolled into round bars with a diameter of φ20mm to φ60mm, and then taken off the production line for stack cooling.
[0051] (4) Isothermal annealing: The round bars are cold-loaded and sent to a roller-hearth heating furnace in a neutral or weakly oxidizing atmosphere through a sling. The steel is heated to 940℃~960℃ in the heating furnace and kept at this temperature for 6-8 hours. After being taken out of the furnace, it is quickly (5-10 minutes) transferred to a furnace at 660℃~680℃ to cool down to room temperature before being taken out of the furnace.
[0052] (5) Finishing: including straightening, chamfering and other finishing processes to ensure that indicators such as size and curvature meet the requirements.
[0053] (6) The surface and interior are subjected to 100% non-destructive testing, and only those that pass the inspection can be considered qualified products.
[0054] The advantages of the present invention are:
[0055] 1. The present invention is a carburizing steel with a new chemical composition and a high fatigue life. Compared with the traditional domestic die casting process, the present invention has the advantages of good continuity, stable quality and a more economical cost of the "vacuum degassing + continuous casting" process. It not only has high cleanliness, high organizational uniformity and high hardenability, but also has high mechanical properties and high fatigue life that the traditional die casting process does not have. It is a steel for new energy vehicle gearbox gears.
[0056] 2. Special smelting process:
[0057] (1) Converter or electric furnace: Add high-quality molten iron, raw materials and low-sulfur scrap steel (containing S ≤ 0.01%) for primary smelting. Blow 35 to 40 cubic meters of oxygen and 5 to 6 cubic meters of argon into each ton of steel, and add active composite lime (CaO-SiO2-CaF2). Under the combined action of oxygen and argon, harmful elements phosphorus (P ≤ 0.020%) and titanium (Ti ≤ 0.002%) are removed.
[0058] (2) Refining furnace and vacuum degassing furnace: In the LF refining furnace, SiC is added to the surface of the molten steel for diffusion deoxidation, and Al wire is fed into the molten steel for precipitation deoxidation. CaO-SiO2-MgO high-performance composite slag-making agent is added to the surface of the molten steel for diffusion deoxidation and adsorption to remove harmful non-metallic inclusions. In the RH or VD vacuum degassing furnace, the maximum vacuum degree in the vacuum furnace is ≤1mbar, and non-metallic inclusions and harmful gases in the steel are removed in a vacuum environment. After the vacuum treatment, the molten steel is soft-blown for ≤15min. After soft blowing, 80-100m of silicon-calcium wire is fed to convert Al2O3 or MgO·A12O3 in the molten steel into calcium aluminate and composite inclusions with lower melting points, and further remove harmful inclusions. The molten steel is made cleaner and meets the requirements of long fatigue life for new energy vehicle gearbox gear steel.
[0059] (3) Continuous casting adopts argon protection throughout the pouring process to protect the molten steel from secondary oxidation contamination; large sections of 300mm×300mm and above are used for continuous casting, and low superheat pouring (superheat △T≤25℃) is adopted; the amount of molten steel in the tundish is controlled at 25-30 tons, and light pressure control technology (pressure reduction 13mm-15mm) is adopted, and the pouring speed is 0.4-0.6m / min; an appropriate steel flow water ratio (0.8-1.0L / kg) is used to further improve the center and ingot segregation of the steel and improve the uniformity of the steel structure.
[0060] 3. Special rolling process:
[0061] The five-pass reciprocating turning large reduction technology is adopted (the steel is turned 90° after each pass), and the five-pass reduction amounts are 25%-30%, 15%-20%, 20%-25%, 15%-20%, and 10%-15% respectively, so that the core structure of the ingot is deformed and recrystallized first during the deformation process, so that the central structure of the steel is more uniform and dense under the action of large pressure. The steel is then rolled alternately by 8 horizontal and vertical rolling mills, and finally rolled into round bars of Φ20mm-Φ60mm.
[0062] 4. Special isothermal annealing
[0063] The steel is heated to 940℃~960℃ in a heating furnace and kept at this temperature for 6-8h. After being taken out of the furnace, it is quickly (5-10min) transferred to a 660℃~680℃ furnace to be cooled to room temperature before being taken out of the furnace. The purpose of isothermal annealing is to make the structure more uniform, and uniform ferrite and pearlite structure is obtained after annealing. DETAILED DESCRIPTION
[0064] The present invention is further described in detail below in conjunction with examples. The examples are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.
[0065] The chemical composition (wt%) of the steel for gears in the gearbox of new energy vehicles of various embodiments of the present invention is shown in Table 3 and Table 4.
[0066] Table 3
[0067] C Si Mn P S Cr Cu Ni V Al Embodiment 1 of the present invention 0.28 0.30 1.16 0.008 0.002 1.17 0.02 0.25 0.045 0.032 Embodiment 2 of the present invention 0.28 0.30 1.16 0.009 0.001 1.16 0.03 0.25 0.046 0.033 Embodiment 3 of the present invention 0.29 0.31 1.15 0.008 0.002 1.16 0.02 0.24 0.045 0.031
[0068] Table 4
[0069]
[0070] Table 5 Non-metallic inclusions in the steel materials of each example
[0071]
[0072]
[0073] Table 6 Macro data of steel materials in various examples
[0074]
[0075] Table 7 Grain size data of each example steel
[0076]
[0077] Table 8 Water immersion high frequency flaw detection data of steel materials in various embodiments
[0078]
[0079] Table 9 Mechanical properties data of steel materials in various embodiments
[0080]
[0081] Table 10 End hardenability data of steel materials in various examples
[0082]
[0083] Table 11 Rotational bending fatigue life data of steel materials in various embodiments
[0084]
[0085] The present invention discloses a production method for gear steel used in gearboxes of new energy vehicles, and the process flow thereof comprises the following steps: primary refining in a converter or an electric furnace → refining in a ladle refining furnace (LF furnace) → vacuum degassing in an RH furnace or a VD furnace → continuous casting CCM (large cross-section) → heating and rolling → stack cooling → isothermal annealing → finishing → surface and internal flaw detection → packaging.
[0086] Specifically, high-quality molten iron, raw materials and low-sulfur scrap steel (containing S≤0.01%) are added together into a converter or an electric furnace for primary smelting. Oxygen is blown into the top of the furnace mouth for oxidation reaction, and argon is blown into the bottom for stirring. 35 to 40 cubic meters of oxygen and 5 to 6 cubic meters of argon are blown into each ton of steel, and 2 to 3 tons of active composite lime (CaO-SiO2-CaF2) are added. Smelting is carried out under the combined action of oxygen and argon. The final carbon content of steel tapped from the primary smelting furnace is 0.15% to 0.18%, the tapping temperature is 1645°C to 1650°C, the final P content is controlled at ≤0.020%, the final Ti content is ≤0.002%, slag blocking is used for tapping, and addition is made during tapping. Some alloys (initial composition adjustment) are quickly lifted to the refining LF furnace after steelmaking is completed; in the LF refining furnace, SiC (50-100Kg) is first added to the molten steel, and then Al wire (80-120m) is fed, and CaO-SiO2-MgO high-performance composite slag-making agent (300-350Kg) is added again, the ladle protection cover is covered, argon gas is connected to the bottom of the ladle, and then the electrode is inserted into the slag for submerged arc power-on. The power is cut off every 15 minutes to measure the temperature of the molten steel and take samples for analysis, and the required main elements (V, Nb, etc.) are added according to the target requirements. The number of temperature measurement and sampling of the refining furnace is controlled at 3-4 times until the composition meets the product requirements. The refining time is controlled to be more than 50min, and the soft blowing time of molten steel is ≥15min; during RH or VD vacuum degassing, the maximum vacuum degree in the vacuum furnace is ≤1mbar, and the vacuum circulation treatment time of molten steel is maintained for ≥15min to ensure that harmful gases in the steel are effectively removed. After the vacuum treatment, argon is blown into the bottom of the ladle, and the argon flow rate is controlled so that the molten steel is not exposed to the air. The soft blowing time of molten steel is ≤15min, and 80-100m of silicon-calcium wire is fed at the same time; large sections of 300mm×300mm and above are used for continuous casting, and low superheat casting (superheat △T≤25℃) is adopted; the amount of molten steel in the tundish is controlled to be 25-30 tons, and light Reduction control technology (reduction 13mm~15mm), pouring and drawing speed 0.4~0.6m / min; adopt appropriate steel flow ratio water volume (0.8~1.0L / kg); the continuous casting billet enters the walking type heating furnace through the conveyor roller, the steel is heated to 1220℃~1260℃ in the heating furnace, the total heating time is ≥3h, the starting rolling temperature is 1050℃~1150℃, the final rolling temperature is controlled to be ≥950℃, and the five-pass reciprocating turning large reduction technology is adopted (the steel is turned 90° after each pass), and the five-pass reductions are 25%~30%, 15%~20%, 20%~25%, 15%~20%, and 10%~15% respectively.The steel is then rolled alternately through 8 horizontal and vertical rolling mills, and finally rolled into round bars of Φ20mm~Φ60mm, which are then cooled to room temperature off the line; the round bars are cold-loaded and sent to a roller-hearth heating furnace in a neutral or weakly oxidizing atmosphere through a sling, and the steel is heated to 940℃~960℃ in the heating furnace and kept at this temperature for 6-8h. After being taken out of the furnace, it is quickly (5-10min) transferred to a furnace of 660℃~680℃ to cool with the furnace to room temperature before being taken out of the furnace, and then cooled to room temperature after being taken out of the furnace, and then the bars are subjected to subsequent flaw detection and finishing.
[0087] It can be seen from Tables 3, 4, 5, 6, 7, 8, 9, 10 and 11 that the steel for gearbox gears of new energy vehicles in each embodiment of the present invention has the control level of harmful elements such as phosphorus, sulfur, oxygen, titanium and non-metallic inclusions reaching the international advanced level. From the results of low magnification, mechanical properties, terminal hardenability, microstructure grain size and rotational bending fatigue life, the low magnification quality, hardenability, microstructure density, mechanical properties and rotational bending fatigue life of the present invention all meet the requirements of steel for gearbox gears of new energy vehicles.
[0088] At the same time, each embodiment was subjected to water immersion high frequency flaw detection according to the SEP 1927 method, and the macro inclusions reached zero defects.
[0089] In summary, a steel for gearbox gears of new energy vehicles in each embodiment of the present invention adopts a "vacuum degassing + continuous casting" process route with good continuity, stable quality and more economical cost, and obtains steel with high cleanliness, high organizational uniformity, high hardenability, high mechanical properties and high fatigue life through unique chemical composition design, special smelting process, rolling process and heat treatment process, thereby producing a new steel with high efficiency, large capacity, low cost and high quality production mode.
[0090] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.
Claims
1. A steel for gearbox gears of new energy vehicles, characterized by: The element composition by mass percentage is C: 0.25-0.31%, Si: 0.2-0.4%, Mn: 1.0-1.3%, Cr: 1.0-1.3%, Ni: 0.2-0.3%, Nb: 0.010-0.020%, V: 0.03-0.06%, Al: 0.02-0.05%, N: 0.0080-0.0110%, S≤0.005%, P≤0.020%, Cu≤0.20%, Mo≤0.10%, Ti≤0.002%, O≤0.0009%, As≤0.04%, Sn≤0.03%, Sb≤0.005%, Pb≤0.002%, and the balance is Fe and unavoidable impurities.
2. The steel according to claim 1, characterized in that: Macrostructure is inspected and graded according to GB / T226 and GB / T 1979, and the general porosity, central porosity and ingot segregation are all within 1.5 level, and there are no shrinkage cavities, cracks or subcutaneous bubbles; Non-metallic inclusions are tested according to DIN 50602 standard K method, and the levels of various inclusions meet the requirements of Table 1 Table 1 Macro defects are inspected according to the water immersion high-frequency flaw detection method of SEP 1927 "Water immersion ultrasonic determination method for purity of forged steel bars". The length of a single inclusion shall not exceed 1mm, and the defect index shall not exceed 5mm / dm 3 .
3. The steel according to claim 1, characterized in that: Carburizing method is used for testing and rating according to GB / T6394, and the grain size is ≥7.
5.
4. The steel according to claim 1, characterized in that: The end hardenability is tested according to GB / T225, heat treatment system: normalizing temperature 920±10℃, holding for 1 hour, air cooling; end quenching temperature 900±5℃, water cooling, J5≥55HRC, J7≥50HRC; The mechanical properties are tested according to GB / T228 and meet the requirements of Table 2. Table 2 The rotating bending fatigue life test was carried out in accordance with GB / T 4337-2015. At room temperature: 20℃±5℃ and 1000MPa cyclic stress conditions, data statistics and analysis were carried out in accordance with GB / T 24176-2009. The rotating bending fatigue life of steel is ≥1×10 7 Second-rate.
5. A method for producing the steel according to claim 1, characterized in that: The steps include, 1. Molten steel smelting: including primary refining, refining and vacuum degassing. Primary refining is to smelt high-quality molten iron, scrap steel containing S ≤ 0.01% and raw and auxiliary materials together. Oxygen is blown into the top of the furnace mouth for oxidation reaction, argon is blown into the bottom for stirring, and active composite lime CaO-SiO2-CaF2 is added to remove harmful elements of phosphorus and titanium. The final carbon of the primary refining furnace when tapping steel is 0.15% to 0.18%, the tapping temperature is ≥1640℃, slag blocking is used for tapping, and some alloys are added during tapping to adjust the composition. After tapping, it is quickly hoisted to the refining furnace; Refining in ladle refining furnace: Add SiC to the surface of molten steel for diffusion deoxidation, feed Al wire into the molten steel for precipitation deoxidation, add CaO-SiO2-MgO high-performance composite slag-making agent to diffuse deoxidation on the surface of molten steel and adsorb and remove harmful non-metallic inclusions; in the smelting process, first add SiC to the molten steel, then feed Al wire and add CaO-SiO2-MgO again, cover the ladle protection cover, connect argon gas to the bottom of the ladle, and then insert the electrode into the slag for submerged arc powering, and measure the temperature and sample the molten steel for analysis every 15 minutes of power outage, add the required alloy elements according to the target requirements, and control the number of temperature measurement and sampling of the refining furnace to 3-4 times until the composition meets the product requirements; Vacuum degassing: The maximum vacuum degree in the vacuum furnace is ≤1mbar, and the vacuum cycle treatment time of the molten steel is maintained for ≥15min. After the vacuum treatment is completed, argon is blown into the bottom of the ladle, and the argon flow rate is controlled so that the molten steel is not exposed to the air. The soft blowing time of the molten steel is ≤15min. At the same time, silicon calcium wire is fed to convert Al2O3 or MgO·A12O3 in the molten steel into calcium aluminate and composite inclusions with lower melting points; 2. Continuous casting: The whole process of continuous casting adopts argon protection pouring, and the continuous casting billet is cast. Low superheat pouring is adopted: superheat △T≤25℃; the amount of molten steel in the tundish is controlled at 25-30 tons, and the light pressure control technology is adopted: the pressure is 13mm-15mm, and the pouring speed is 0.4-0.6m / min; the appropriate steel flow water ratio is adopted: 0.8-1.0L / kg, and electromagnetic stirring is used in the tundish to interrupt the bridging of the columnar crystal area during the solidification of the continuous casting billet; 3. Heating and rolling: The continuous casting billet is heated in a heating furnace with a neutral or weakly oxidizing atmosphere and then rolled into round bars. The billet is rolled in the austenite phase. The continuous casting billet is first rolled in a five-pass reciprocating rolling method with a large reduction, and then rolled into round steel by alternating rolling in a horizontal and vertical rolling mill.
4. Isothermal annealing: The round steel is heated to 940℃~960℃ in a heating furnace and kept at this temperature for 6-8h. After being taken out of the furnace, it is quickly transferred to a furnace at 660℃~680℃ within 5-10min to be cooled to room temperature before being taken out of the furnace.
6. The method according to claim 5, characterized in that: In the initial refining stage of step one, 35 to 40 cubic meters of oxygen and 5 to 6 cubic meters of argon are blown into each ton of steel to reduce the P content in the molten iron to P≤0.020% and the titanium content to Ti≤0.002%; during the refining process, first add SiC: 50 to 100 kg to the molten steel, then feed Al wire: 80 to 120 m, and then add CaO-SiO2-MgO high-performance composite slag-making agent: 300 to 350 kg, the refining time is controlled at more than 50 minutes, and the soft blowing time of the molten steel is ≥15 minutes; after vacuum degassing, feed 80 to 100 m of silicon-calcium wire into the molten steel.
7. The method according to claim 5, characterized in that: Step three, the continuous casting billet enters the walking-beam heating furnace through the conveyor roller, the steel is heated to 1220℃~1260℃ in the heating furnace, the total heating time is ≥3h, the starting rolling temperature is 1050℃~1150℃, the final rolling temperature is controlled to be ≥950℃, and the five-pass reciprocating turning large-reduction rolling method is used: the steel is turned 90° after each pass, and the five-pass reduction amounts are 25%~30%, 15%~20%, 20%~25%, 15%~20%, and 10%~15% respectively, and then rolled alternately through 8 horizontal and vertical rolling mills, and finally rolled into φ20mm~φ60mm round bars, and then taken off the line for stack cooling.
8. The method according to claim 5, characterized in that: Step 4: The round bar is cold loaded through a sling and sent to a roller bottom heating furnace in a neutral or weakly oxidizing atmosphere for isothermal annealing.
9. The method according to claim 5, characterized in that: Step 2: Use continuous casting process to cast molten steel into continuous casting square billets with a cross-section of 300mm×300mm or above.
10. The method according to claim 5, characterized in that: After isothermal annealing in step 4, the round steel is also finished: straightening and chamfering to meet the size and curvature requirements.
Citation Information
Patent Citations
High-strength gear steel 23CrMnMoS and manufacturing method thereof
CN112899560A
Manufacturing method of steel for speed reducer gear of electric automobile
CN112981271A
Steel for automobile engine bearing shaft sleeve and production method thereof
CN114941101A
Steel for high-temperature carburizing shaft teeth and manufacturing method thereof
CN115537649A
Steel for gearbox bearing of high-speed motor car and manufacturing method of steel
CN116479322A