Method for eliminating mechanical anisotropy of titanium alloy workpiece
By performing three insulation treatments at different temperatures, the continuous grain boundary α phase in the titanium alloy workpiece is broken, the problem of anisotropy of the mechanical properties of titanium alloy is solved, the consistency of its mechanical properties is improved, and the application potential in the aerospace field is enhanced .
Patent Information
- Application Number
- CN202410972137.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
The columnar grains formed by titanium alloys in the laser cladding additive manufacturing process lead to anisotropy of their mechanical properties, which seriously restricts their application in the aerospace field.
By performing three insulation treatments at different temperatures, cooling to room temperature, the first insulation treatment (T1, Tβ-30℃≤T1≤Tβ-10℃, 0.5h~2h), and the second insulation treatment (T2, T1-60℃≤T2≤T1-20℃, 1h~4h), and the third insulation treatment (T3, 500℃≤T3≤650℃, 2h~6h) to crush the continuous grain boundary α in the titanium alloy workpiece phase, achieve the homogenization of microstructure.
It effectively reduces the anisotropy of the mechanical properties of titanium alloy workpieces, improves its mechanical properties consistency in all directions, and enhances plasticity, fatigue strength and fracture toughness.
Smart Images

Figure CN118910523A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of metal processing, and in particular to a method for eliminating the mechanical anisotropy of a titanium alloy workpiece. Background Art
[0002] Titanium alloy is one of the metal materials widely studied in additive manufacturing technology. It has excellent comprehensive properties such as high specific strength, corrosion resistance, low temperature resistance, non-magnetic, and good biocompatibility. It has been widely used in aerospace, transportation, biomedicine and other fields. However, the microstructure of titanium alloy shows columnar grains due to rapid solidification during the laser cladding additive manufacturing process. This technical microstructure usually appears in parts processed by laser cladding additive manufacturing, and it is easy to form coarse columnar crystals perpendicular to the laser scanning direction and throughout the entire cladding deposition layer during the laser cladding deposition process. Studies have shown that compared with equiaxed organization, the columnar grain morphology will lead to prominent anisotropy of titanium alloy components, poor plasticity, fatigue strength and fracture toughness, which seriously restricts its actual promotion and application in the aerospace field.
[0003] Therefore, there is an urgent need for a method to reduce the anisotropy of the mechanical properties of additively manufactured titanium alloys. Summary of the invention
[0004] The main purpose of this application is to provide a method for eliminating the mechanical anisotropy of titanium alloy workpieces, aiming to solve the technical problem that the existing technology cannot reduce the anisotropy of the mechanical properties of additively manufactured titanium alloys.
[0005] In order to solve the above technical problems, the embodiment of the present application proposes: a method for eliminating the mechanical anisotropy of a titanium alloy workpiece, comprising the following steps:
[0006] After performing a first heat preservation treatment on the titanium alloy workpiece at a first preset temperature T1, the workpiece is cooled to room temperature to obtain a first titanium alloy workpiece;
[0007] The first titanium alloy workpiece is subjected to a second heat preservation treatment at a second preset temperature T2, and cooled to room temperature to obtain a second titanium alloy workpiece;
[0008] The second titanium alloy workpiece is subjected to a third heat preservation treatment at a third preset temperature T3, and cooled to room temperature to obtain a third titanium alloy workpiece;
[0009] The first preset temperature T1, the second preset temperature T2 and the third preset temperature T3 are different and are all lower than the β phase transition point T β .
[0010] As some optional implementations of the present application, the first preset temperature T1 ≥ the second preset temperature T2 > the third preset temperature T3.
[0011] As some optional embodiments of the present application, the first preset temperature T1 is greater than the β phase transition point T β The relationship is: T β -30℃≤T1≤T β -10℃.
[0012] As some optional implementation modes of the present application, the insulation time of the first insulation treatment is 0.5h to 2h.
[0013] As some optional implementations of the present application, the relationship between the second preset temperature T2 and the first preset temperature T1 is T1-60°C≤T2≤T1-20°C.
[0014] As some optional implementation modes of the present application, the insulation time of the second insulation treatment is 1 hour to 4 hours.
[0015] As some optional implementations of the present application, the third preset temperature T3 is 500°C≤T3≤650°C.
[0016] As some optional implementation modes of the present application, the insulation time of the third insulation treatment is 2h to 6h.
[0017] As some optional embodiments of the present application, the titanium alloy workpiece is obtained by additive manufacturing.
[0018] As some optional embodiments of the present application, the manufacturing powder used in the additive manufacturing is a dual-phase titanium alloy powder, and the average particle size of the dual-phase titanium alloy powder is 53 μm to 150 μm.
[0019] At present, titanium alloy workpieces are usually obtained by laser additive manufacturing, but an important problem with laser directional deposition additive manufacturing of titanium alloys is that titanium alloy components form coarse original β columnar crystals in the deposition direction, and continuously growing grain boundary α phases are distributed at the β columnar grain boundaries. The α phases in the grains are distributed in lamellar layers. Due to the difference in grain structure, the mechanical properties are anisotropic in the deposition direction and perpendicular to the deposition direction. In the deposition direction (Z direction), it often exhibits the characteristics of low strength and relatively good plasticity, while in the direction perpendicular to the deposition direction (X direction), it exhibits the characteristics of high strength and low plasticity. Therefore, in view of the above-mentioned defects in the prior art, the method for eliminating the mechanical anisotropy of a titanium alloy workpiece described in the present application comprises the following steps: subjecting the titanium alloy workpiece to a first heat preservation treatment at a first preset temperature T1, and cooling it to room temperature to obtain a first titanium alloy workpiece; subjecting the first titanium alloy workpiece to a second heat preservation treatment at a second preset temperature T2, and cooling it to room temperature to obtain a second titanium alloy workpiece; subjecting the second titanium alloy workpiece to a third heat preservation treatment at a third preset temperature T3, and cooling it to room temperature to obtain a third titanium alloy workpiece; wherein the first preset temperature T1, the second preset temperature T2, and the third preset temperature T3 are different and are all lower than the β phase transition point T β The titanium alloy components obtained by additive manufacturing are heat treated at three different temperatures respectively, so that the continuous grain boundary α phase at the original β grain boundary is broken, so as to achieve the homogenization of the microstructure through solid-state phase transformation, reduce the anisotropy of the mechanical properties of the titanium alloy workpiece, and thus enhance the mechanical properties of the titanium alloy workpiece. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a schematic diagram of a process for eliminating mechanical anisotropy of a titanium alloy workpiece according to an embodiment of the present application;
[0021] Figure 2 is a microstructure diagram of the XOY plane (the plane perpendicular to the deposition direction) of the titanium alloy workpiece described in Example 1 of the present application;
[0022] Figure 3 is a microstructure diagram of the XOZ plane (plane parallel to the deposition direction) of the titanium alloy workpiece described in Example 1 of the present application;
[0023] Figure 4 It is a microstructure diagram of the XOY plane of the titanium alloy workpiece described in Comparative Example 1 of the present application;
[0024] Figure 5 It is a microstructure diagram of the XOZ surface of the titanium alloy workpiece described in Comparative Example 1 of the present application. DETAILED DESCRIPTION
[0025] It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0026] Titanium alloy is one of the metal materials widely studied in additive manufacturing technology. It has excellent comprehensive properties such as high specific strength, corrosion resistance, low temperature resistance, non-magnetic, and good biocompatibility. It has been widely used in aerospace, transportation, biomedicine and other fields. However, the microstructure of titanium alloy shows columnar grains due to rapid solidification during laser cladding additive manufacturing. This technical microstructure usually appears in parts processed by laser cladding additive manufacturing, and it is often easy to form coarse columnar crystals perpendicular to the laser scanning direction and throughout the entire cladding deposition layer during the laser cladding deposition process. Studies have shown that compared with equiaxed structures, such as: coarse original β columnar crystals formed in the deposition direction, continuously growing grain boundary α phases are distributed at the β columnar grain boundaries, and the α phases in the grains are distributed in lamellar layers. Due to the difference in grain structure, the mechanical properties are anisotropic in the deposition direction and perpendicular to the deposition direction. In the deposition direction, it often shows the characteristics of low strength and relatively good plasticity, while in the direction perpendicular to the deposition direction, it shows the characteristics of high strength and low plasticity. However, the columnar grain morphology will lead to prominent anisotropy of titanium alloy components, poor plasticity, fatigue strength and fracture toughness, which seriously restricts its actual promotion and application in the aerospace field.
[0027] At present, in order to solve the problem of coarse columnar crystals generated by titanium alloys during laser cladding additive manufacturing, the methods for refining laser cladding titanium alloy grains are mainly divided into chemical treatment (adding rare earth elements) and physical treatment (pulse frequency, ultrasonic vibration, etc.). However, during chemical treatment, if the amount of rare earth elements introduced is too small, the strengthening effect is not obvious, and if too much rare earth elements are introduced, the grains will be coarsened, segregated, and enriched at the grain boundaries, deteriorating the material properties. During physical treatment, as the deposition layer increases and the size of the component increases, the effect of the ultrasonic energy field on the solidification of the alloy in the molten pool at the top of the component becomes smaller and smaller, so this technology is difficult to apply to the additive manufacturing of large-sized titanium alloy components.
[0028] Therefore, in view of the above technical defects, Figure 1 As shown, the embodiment of the present application proposes: a method for eliminating the mechanical anisotropy of a titanium alloy workpiece, comprising the following steps:
[0029] Step S10, subjecting the titanium alloy workpiece to a first heat preservation treatment at a first preset temperature T1, and then cooling it to room temperature to obtain a first titanium alloy workpiece.
[0030] In a specific application, the first preset temperature T1 is approximately equal to the β phase transition point T β The relationship is: T β -30℃≤T1≤T β-10℃; the insulation time of the first insulation treatment is 0.5h~2h. In actual application, the first insulation treatment is carried out in a high-temperature air resistance furnace. Water cooling or oil cooling should not be used for cooling. In order to avoid deformation of titanium alloy workpieces due to thin walls and differences in mechanical properties, air cooling or furnace cooling should be used as much as possible.
[0031] In a specific application, the above steps may be: after the temperature in the high-temperature air resistance furnace is raised to the first preset temperature T1, the titanium alloy workpiece is placed in the furnace for the first heat preservation treatment; when the temperature in the high-temperature air resistance furnace rises back to the first preset temperature T1, the timing is started, and the heat preservation is stopped after 0.5h to 2h, and the workpiece is cooled to room temperature to obtain the first titanium alloy workpiece. Preferably, if the α phase of the titanium alloy workpiece grain boundary is to be broken, the temperature should be close to the β phase transformation point and lower than T β Heating is performed to provide more particles for the nucleation of the α phase. However, the holding time during this period should not be too long (e.g., 0.5h to 2h) to prevent the α phase from coarsening after nucleation. The temperature should not be higher than T locally. β , to prevent plasticity from decreasing.
[0032] In a specific application, the temperature in the high-temperature air resistance furnace is uniform, the test temperature is T, and the temperature control range of the working area in the resistance furnace is T±5°C.
[0033] Step S20: subjecting the first titanium alloy workpiece to a second heat preservation treatment at a second preset temperature T2, and cooling the first titanium alloy workpiece to room temperature to obtain a second titanium alloy workpiece.
[0034] In a specific application, the relationship between the second preset temperature T2 and the first preset temperature T1 is T1-60℃≤T2≤T1-20℃; the insulation time of the second insulation treatment is 1h to 4h. In actual application, the second insulation treatment is carried out in a high-temperature air resistance furnace, and water cooling or oil cooling is not selected as much as possible for the cooling. In order to avoid deformation of the titanium alloy workpiece due to thin walls and differences in mechanical properties, air cooling or furnace cooling is selected as much as possible.
[0035] In a specific application, the above steps can be: after the temperature in the high-temperature air resistance furnace is raised to the second preset temperature T2, the titanium alloy workpiece is placed in the furnace for a second insulation treatment; when the temperature in the high-temperature air resistance furnace rises back to the second preset temperature T2, the timing is started, and the insulation is stopped after 1h to 4h, and the workpiece is cooled to room temperature to obtain a second titanium alloy workpiece.
[0036] In specific applications, the second preset temperature T2 should not be too high, and the holding time should not be too short, so as to promote the growth of α phase in the titanium alloy workpiece and break up the coarse Widmanstatten structure in the deposited titanium alloy; wherein, the Widmanstatten structure refers to the fact that in the overheating zone of welding, due to the very coarse growth of austenite grains, this coarse austenite will form a special overheating structure under a faster cooling rate, such as many parallel ferrite (cementite) needle plates will be formed in a coarse austenite grain, and the remaining austenite between the ferrite needle plates will eventually transform into pearlite. This overheating structure is called ferrite (cementite) Widmanstatten structure; for example, the lamellar coherent precipitated phase is usually precipitated on a certain crystal plane of the matrix (called the habitual plane of precipitation) to maintain coherence, because the crystal planes in the crystal are arranged in parallel in several groups with different directions, so the precipitated phase is also arranged in parallel in several groups, becoming a Widmanstatten structure.
[0037] Step S30, subjecting the second titanium alloy workpiece to a third heat preservation treatment at a third preset temperature T3, and cooling the second titanium alloy workpiece to room temperature to obtain a third titanium alloy workpiece;
[0038] In a specific application, the third preset temperature T3 is 500℃≤T3≤650℃; the insulation time of the third insulation treatment is 2h~6h. In actual application, the third insulation treatment is carried out in a high-temperature air resistance furnace, and water cooling or oil cooling is not selected as much as possible. In order to avoid deformation of titanium alloy workpieces due to thin walls and differences in mechanical properties, air cooling or furnace cooling is selected as much as possible.
[0039] In a specific application, the above steps can be: after the temperature in the high-temperature air resistance furnace is raised to the third preset temperature T3, the titanium alloy workpiece is placed in the furnace for a third insulation treatment; when the temperature in the high-temperature air resistance furnace rises back to the third preset temperature T3, the timing is started, and the insulation is stopped after 2h to 6h, and the workpiece is cooled to room temperature to obtain the third titanium alloy workpiece.
[0040] It can be seen that in the method described in the present application, the first preset temperature T1, the second preset temperature T2 and the third preset temperature T3 are different; preferably, due to being higher than T β The material strength and plasticity will decrease, so the first preset temperature T1, the second preset temperature T2 and the third preset temperature T3 are all lower than the β phase transition point T β ; More preferably, the first preset temperature T1 ≥ the second preset temperature T2 > the third preset temperature T3. Specifically, the heat treatment temperature is generally from high to low. If it is from low to high, the previous two heat treatments are of little significance for performance adjustment. T1 is a higher temperature, which can break the continuous grain boundary α phase; T2 is a slightly lower temperature, which is a solution treatment; T3 is the aging temperature, which is lower and improves the material strength.
[0041] In a specific application, the titanium alloy workpiece is obtained by additive manufacturing, and the manufacturing powder used in the additive manufacturing is a dual-phase titanium alloy powder, and the average particle size of the dual-phase titanium alloy powder is 53μm to 150μm. In the embodiment of the present application, the additive manufacturing process is not specifically limited, and processing can be performed according to existing process parameters.
[0042] At present, titanium alloy workpieces are usually obtained by laser additive manufacturing, but an important problem with laser directional deposition additive manufacturing of titanium alloys is that titanium alloy components form coarse original β columnar crystals in the deposition direction, and continuously growing grain boundary α phases are distributed at the β columnar grain boundaries. The α phases in the grains are distributed in lamellar layers. Due to the difference in grain structure, the mechanical properties are anisotropic in the deposition direction and perpendicular to the deposition direction. In the deposition direction (Z direction), it often exhibits the characteristics of low strength and relatively good plasticity, while in the direction perpendicular to the deposition direction (X direction), it exhibits the characteristics of high strength and low plasticity. Therefore, in view of the above-mentioned defects of the prior art, the method for eliminating the mechanical anisotropy of the titanium alloy workpiece described in the present application includes the following steps: after the titanium alloy workpiece is subjected to the first heat preservation treatment at a first preset temperature T1, it is cooled to room temperature to obtain a first titanium alloy workpiece; the first titanium alloy workpiece is subjected to the second heat preservation treatment at a second preset temperature T2, and is cooled to room temperature to obtain a second titanium alloy workpiece; the second titanium alloy workpiece is subjected to the third heat preservation treatment at a third preset temperature T3, and is cooled to room temperature to obtain a third titanium alloy workpiece; wherein the first preset temperature T1, the second preset temperature T2 and the third preset temperature T3 are different. That is, the titanium alloy component obtained by additive manufacturing is heat treated at three different temperatures respectively, so that the continuous grain boundary α phase at the original β grain boundary is broken, so as to achieve the homogenization of the microstructure through solid-state phase transformation, reduce the anisotropy of the mechanical properties of the titanium alloy workpiece, and thus enhance the mechanical properties of the titanium alloy workpiece.
[0043] In addition, the method described in the present application does not require repeated cyclic heating and does not require magnetic field treatment, and has low requirements for heat treatment equipment, thereby reducing the cost and equipment requirements for heat treatment.
[0044] Now, in conjunction with the specific implementation manner, the method described in this application is described in detail:
[0045] Example 1
[0046] A titanium alloy block is prepared by a laser directional deposition method, and the titanium alloy block is removed from a substrate by a wire cutting method.
[0047] After the temperature in the high-temperature air resistance furnace is raised to 960°C ~ 1020°C, the titanium alloy workpiece is placed in the furnace for the first insulation treatment; when the temperature in the high-temperature air resistance furnace rises back to 960°C ~ 1020°C, the timing is started, and the insulation is stopped after 0.5h ~ 2h, and the workpiece is cooled to room temperature to obtain the first titanium alloy workpiece.
[0048] After the temperature in the high-temperature air resistance furnace is raised to 900°C ~ 960°C, the titanium alloy workpiece is placed in the furnace for a second insulation treatment; when the temperature in the high-temperature air resistance furnace rises back to 900°C ~ 960°C, the timing starts, and the insulation is stopped after 1h ~ 4h, and the workpiece is cooled to room temperature to obtain a second titanium alloy workpiece.
[0049] After the temperature in the high-temperature air resistance furnace is raised to 500°C ~ 650°C, the titanium alloy workpiece is placed in the furnace for the third insulation treatment; when the temperature in the high-temperature air resistance furnace rises back to 500°C ~ 650°C, the timing starts, and the insulation is stopped after 2h ~ 6h, and the workpiece is cooled to room temperature to obtain the third titanium alloy workpiece.
[0050] The microstructure diagram of the third titanium alloy workpiece is as follows Figure 2-Figure 3 As shown, Figure 2 is a microstructure diagram of the third titanium alloy workpiece on the XOY plane, Figure 3 This is a microstructure diagram of the third titanium alloy workpiece on the XOZ plane.
[0051] Example 2
[0052] A titanium alloy block is prepared by a laser directional deposition method, and the titanium alloy block is removed from a substrate by a wire cutting method.
[0053] After the temperature in the high-temperature air resistance furnace is raised to 950°C ~ 1000°C, the titanium alloy workpiece is placed in the furnace for the first insulation treatment; when the temperature in the high-temperature air resistance furnace rises back to 950°C ~ 1000°C, the timing starts, and the insulation is stopped after 0.5h ~ 2h, and the workpiece is cooled to room temperature to obtain the first titanium alloy workpiece.
[0054] After the temperature in the high-temperature air resistance furnace is raised to 920°C ~ 970°C, the titanium alloy workpiece is placed in the furnace for a second insulation treatment; when the temperature in the high-temperature air resistance furnace rises back to 920°C ~ 970°C, the timing starts, and the insulation is stopped after 1h ~ 4h, and the workpiece is cooled to room temperature to obtain a second titanium alloy workpiece.
[0055] After the temperature in the high-temperature air resistance furnace is raised to 500°C ~ 650°C, the titanium alloy workpiece is placed in the furnace for the third insulation treatment; when the temperature in the high-temperature air resistance furnace rises back to 500°C ~ 650°C, the timing starts, and the insulation is stopped after 2h ~ 6h, and the workpiece is cooled to room temperature to obtain the third titanium alloy workpiece.
[0056] Comparative Example 1
[0057] The titanium alloy workpiece was prepared by the same laser directional deposition process as in Example 1. The microstructure of the titanium alloy workpiece is shown in FIG. Figure 4-Figure 5 As shown, Figure 4 is the microstructure diagram of the titanium alloy workpiece on the XOY plane, Figure 5 It is the microstructure diagram of the titanium alloy workpiece on the XOZ plane.
[0058] The TC11 titanium alloy treated by the method described in Example 1 (hereinafter referred to as titanium alloy 1), the TC11 titanium alloy treated by the method described in Example 2 (hereinafter referred to as titanium alloy 2), and the TC11 titanium alloy of Comparative Example 1 (hereinafter referred to as blank titanium alloy) were tested for room temperature tensile properties according to GB 228.1. The results are shown in Table 1. In the following table, the Z direction refers to the direction parallel to the deposition direction, and the X direction refers to the direction perpendicular to the deposition direction:
[0059] Table 1:
[0060] Yield Strength tensile strength Elongation Titanium alloy-X direction 1086MPa 1147MPa 4.5% Titanium alloy-Z direction 973MPa 1052MPa 10.2% Titanium alloy 1-X direction 980MPa 1120MPa 10.8% Titanium alloy 1-Z direction 977MPa 1115MPa 12.1% Titanium alloy 2-X direction 997MPa 1124MPa 11.2% Titanium alloy 2-Z direction 996MPa 1117MPa 11.5%
[0061] from Figure 2-Figure 5 It can be seen that Figure 2-Figure 3 The microstructure of the titanium alloy workpiece after being treated by the heat treatment method described in the present application shows that the α phase at the grain boundary is effectively broken; Figure 4-Figure 5 The microstructure of the titanium alloy workpiece that has not been treated by the heat treatment method described in this application can be clearly seen to have a coarse and continuous grain boundary α phase, as well as a local Widmanstatten structure and a basketweave structure. Combined with the above Table 1, it can be seen that the titanium alloy workpiece obtained by the heat treatment method described in this application, compared with the untreated titanium alloy workpiece, the titanium alloy workpiece obtained by the heat treatment method described in this application has a broken continuous grain boundary α phase at the original β grain boundary, a more uniform microstructure, and improves the consistency of the mechanical properties of the titanium alloy workpiece in all directions.
[0062] The above are only preferred embodiments of the present application, and are not intended to limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.
Claims
1. A method for eliminating mechanical anisotropy of a titanium alloy workpiece, characterized in that: The following steps are involved: After performing a first heat preservation treatment on the titanium alloy workpiece at a first preset temperature T1, the workpiece is cooled to room temperature to obtain a first titanium alloy workpiece; The first titanium alloy workpiece is subjected to a second heat preservation treatment at a second preset temperature T2, and cooled to room temperature to obtain a second titanium alloy workpiece; The second titanium alloy workpiece is subjected to a third heat preservation treatment at a third preset temperature T3, and cooled to room temperature to obtain a third titanium alloy workpiece; The first preset temperature T1, the second preset temperature T2 and the third preset temperature T3 are different and are all lower than the β phase transition point T β .
2. The method for eliminating mechanical anisotropy of a titanium alloy workpiece according to claim 2, characterized in that: The first preset temperature T1 ≥ the second preset temperature T2 > the third preset temperature T3.
3. The method for eliminating mechanical anisotropy of a titanium alloy workpiece according to claim 2, characterized in that: The first preset temperature T1 is equal to the β phase transition point T β The relationship is: T β -30℃≤T1≤T β -10℃.
4. The method for eliminating mechanical anisotropy of a titanium alloy workpiece according to claim 3, characterized in that: The insulation time of the first insulation treatment is 0.5h to 2h.
5. The method for eliminating mechanical anisotropy of a titanium alloy workpiece according to claim 2, characterized in that: The relationship between the second preset temperature T2 and the first preset temperature T1 is T1-60°C≤T2≤T1-20°C.
6. The method for eliminating mechanical anisotropy of a titanium alloy workpiece according to claim 5, characterized in that: The insulation time of the second insulation treatment is 1h to 4h.
7. The method for eliminating mechanical anisotropy of a titanium alloy workpiece according to claim 2, characterized in that: The third preset temperature T3 is 500°C≤T3≤650°C.
8. The method for eliminating mechanical anisotropy of a titanium alloy workpiece according to claim 7, characterized in that: The insulation time of the third insulation treatment is 2h to 6h.
9. The method for eliminating mechanical anisotropy of a titanium alloy workpiece according to claim 1, characterized in that: The titanium alloy workpiece is obtained by additive manufacturing.
10. The method for eliminating mechanical anisotropy of a titanium alloy workpiece according to claim 9, characterized in that: The manufacturing powder used in the additive manufacturing is a dual-phase titanium alloy powder, and the average particle size of the dual-phase titanium alloy powder is 53 μm to 150 μm.