High-toughness titanium alloy with bidirectional gradient structure and preparation method of high-toughness titanium alloy

By heating and aging treatment in titanium alloy, and radial gradient structure is constructed by using laser impact, the problem of cracks easily on the surface of titanium alloy during bending fatigue fracture is solved, and the fatigue life and overall performance are significantly improved.

CN118910524AActive Publication Date: 2024-11-08XIAN UNIV OF TECH

Patent Information

Application Number
CN202410999779.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

The axial gradient structure of existing titanium alloys is prone to cracks on the surface during bending fatigue fracture, resulting in fatigue failure of structural parts, and the thickness and volume fraction of gradient nanolayers are small, resulting in less significant improvement in strength.

Method used

By heating the titanium alloy to the β single-phase zone and water-cooling, combining aging treatment to form an axial gradient structure, and using surface laser impact enhancement technology to construct a radial gradient structure, the gradient transition from bistate tissue to sheet tissue is achieved.

Benefits of technology

The surface fatigue crack initiation resistance of titanium alloy is significantly improved, the fatigue life of the overall structural parts is improved, and the overall performance of the structural parts is improved without losing high strength and plastic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910524A_ABST
    Figure CN118910524A_ABST
Patent Text Reader

Abstract

The invention provides a high strength and toughness titanium alloy with a two-way gradient structure and a preparation method, the method comprises the following steps: heating a part of area of the high strength and toughness titanium alloy with the two-state structure to a beta single-phase area, keeping the temperature of the area at one end of the titanium alloy and the other end of the area as a cross section in the length direction of the titanium alloy, performing water cooling to room temperature, and performing aging treatment at 600-650 DEG C for 5-6 hours to obtain the high strength and toughness titanium alloy with the two-way gradient structure. And then air cooling is conducted to the room temperature, and the high-toughness titanium alloy with the axial gradient structure gradually changing from the double-state structure to the lamellar alpha phase is obtained. And the obtained titanium alloy is subjected to surface laser shock peening treatment, the high-toughness titanium alloy of a radial gradient structure from the surface to the center is obtained, the surface fatigue crack initiation resistance of the titanium alloy is remarkably improved while the functional effect of a high-toughness titanium alloy dual-performance structural part is achieved, and the service life of the titanium alloy is prolonged. And a new thought and a new way are provided for preparation and mechanical property optimization of the high-strength metastable beta titanium alloy dual-performance structural part, and wide application prospects and value are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of titanium alloy structure design and heat treatment, and in particular relates to a high-strength and toughness titanium alloy with a bidirectional gradient structure and a preparation method thereof. Background Art

[0002] Titanium alloys have high specific strength, corrosion resistance and high fatigue damage resistance, so they are widely used in key structural parts such as aircraft landing gear, frames and wing spars. In recent years, scientists have proposed the use of axial gradient structure design from equiaxed structure to lamellar structure, which can not only reduce the risk of weak connection caused by traditional welding, tenon and mortise connection methods, but also effectively improve the structural efficiency of aircraft and achieve weight reduction.

[0003] The axial gradient structure of titanium alloy is a key part of integral structural parts such as beams, blades and shafts. It is inevitably subjected to a variety of complex stresses such as bending and vibration during service. The resulting bending fatigue, especially rotary bending fatigue fracture, has become one of the main failure forms of integral structural parts such as beams and shafts. According to a large number of reports on bending fatigue fractures of titanium alloys, under bending loads, the surface shear stress is the largest, cracks are easy to initiate on the surface and extend toward the center. Therefore, most rotary bending fatigue fracture failures originate from the surface of the component. The preferential formation of fatigue damage on the surface is a key factor causing fatigue fracture of integral structural parts. Therefore, significantly improving the bending fatigue crack initiation resistance of the surface structure without losing the excellent basic mechanical properties of high-strength titanium alloy integral structural parts has become a core issue that needs to be urgently addressed in the design of high-strength and tough titanium alloy anti-bending fatigue damage structure and organization.

[0004] At present, surface gradient structures are mainly prepared by severe surface plastic deformation methods, such as surface shot peening, surface mechanical rolling, and surface mechanical grinding, but the thickness of the nanolayer is relatively thin, and the volume fraction of the nanolayer is usually relatively small. Since the thickness and volume fraction of the gradient nanolayer are key parameters affecting the strength and other properties of the gradient material, the strength improvement of the gradient nanostructured material is not significant. Summary of the invention

[0005] In response to the problems existing in the prior art, the present invention provides a high-strength and toughness titanium alloy with a bidirectional gradient structure and a preparation method. The alloy has simple operation, high production efficiency, is environmentally friendly and economical, and can be easily mass-produced. While achieving the functional effects of high-strength and toughness titanium alloy dual-performance structural parts, the alloy significantly improves its surface fatigue crack initiation resistance, providing a new idea and new approach for the preparation and mechanical property optimization of high-strength metastable β titanium alloy dual-performance structural parts, and has broad application prospects and value.

[0006] The present invention is achieved through the following technical solutions:

[0007] A method for preparing a high-strength and tough titanium alloy with a bidirectional gradient structure, comprising the following steps:

[0008] S1, heating a part of the high-strength and toughness titanium alloy with a dual-state structure to a β single-phase region, wherein one end of the region is one end of the high-strength and toughness titanium alloy, and the other end of the region is a cross section in the length direction of the high-strength and toughness titanium alloy, then keeping the temperature, and then water-cooling to room temperature, wherein the region gradually changes from the dual-state structure to the β phase along the axial direction;

[0009] S2, subjecting the titanium alloy obtained in S1 to aging treatment at 600-650°C for 5-6h, and then air-cooling to room temperature, to obtain a high-strength and tough titanium alloy with an axial gradient structure gradually changing from a dual-state structure to a lamellar α phase;

[0010] S3, performing surface laser shock strengthening treatment on the titanium alloy obtained in S2 to obtain a high-strength and tough titanium alloy with a radial gradient structure from the surface to the core.

[0011] Preferably, the β single-phase region described in S1 is 900-920°C.

[0012] Preferably, the high-strength and toughness titanium alloy described in S1 is in the shape of a round rod or a plate, and the cross section is located at the center of the high-strength and toughness titanium alloy.

[0013] Preferably, the holding time in S1 is 30 to 90 seconds.

[0014] Preferably, in S1, high-energy pulse current is used to heat the high-strength and toughness titanium alloy.

[0015] Furthermore, in S1, the high-strength and toughness titanium alloy is heated from room temperature at a heating rate of 30 to 35°C / s.

[0016] Preferably, the radial thickness of the surface fine grain structure in S3 is 30 to 100 μm.

[0017] Preferably, the laser pulse width in S3 is 8 to 10 ns.

[0018] Preferably, the number of laser shocks in S3 is 2 to 5 times.

[0019] A high-strength and toughness titanium alloy with a bidirectional gradient structure obtained by any of the above methods for preparing a high-strength and toughness titanium alloy with a bidirectional gradient structure.

[0020] Compared with the prior art, the present invention has the following beneficial technical effects:

[0021] The present invention discloses a method for preparing a high-strength and tough titanium alloy with a bidirectional gradient structure. First, a part of the titanium alloy is heated to the β single-phase region and then kept warm and water-cooled, which can quickly realize the transformation of the α phase to the β phase in the dual-state structure. The rapid cooling method of water cooling has the effect of dissolving a large amount of alloy elements, thereby obtaining an oversaturated fine-grained pure β phase region, laying a structural foundation for the subsequent aging precipitation of dispersed lamellar α phase. A long-term aging treatment at 600-650°C can promote the uniform precipitation and growth of the lamellar α phase, and a dispersed lamellar α phase can be obtained by time regulation, thereby transforming the pure β phase region into a fine-grained structure with a dispersed needle-shaped α phase, obtaining an axial gradient structure that gradually changes from the dual-state structure gradient to the fine lamellar structure, and significantly improving the strength and plasticity of the alloy. The axial gradient organization not only replaces the traditional welding, tenon and other connection methods of the structural parts, but also realizes the overall structural effect of the gradual change from equiaxed organization to lamellar organization, significantly improving the structural efficiency of the aircraft and reducing weight; on the surface of the axial gradient organization, the laser shock strengthening technology is continued to be used to construct the radial gradient organization, and the high-energy laser induces the generation of high-pressure (GPa level) plasma shock waves to strengthen the surface of the metal material, which can form a hardened layer and a compressive stress layer with a depth of 1mm or even deeper, and at the same time has a relatively low surface roughness, effectively improving the fatigue performance of the material, thereby significantly improving the surface fatigue crack initiation resistance of the overall structural parts, and improving the fatigue life of the overall structural parts. The present invention first combines heating with aging treatment to realize the rapid preparation and performance regulation of the overall structural parts of the titanium alloy with axial gradient organization, while not damaging the basic mechanical properties such as excellent strength and plasticity of the high-strength titanium alloy, the radial gradient organization is quickly constructed on the surface of the overall structural parts by high-energy laser shock strengthening technology, thereby significantly improving the bending fatigue crack initiation resistance of the surface organization of the titanium alloy overall structural parts, which is a new method for rapidly, energy-savingly and efficiently preparing the overall structural parts with the gradient transition from the dual-state organization to the lamellar organization. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a metallographic morphology image of the Ti55531 titanium alloy with a bidirectional gradient structure in Example 1 of the present invention;

[0023] Figure 2 for Figure 1 The enlarged characteristic image of the radial gradient tissue represented in ;

[0024] Figure 3 for Figure 1 Characteristic diagram of radial gradient fine grain structure in the middle and surface layers;

[0025] Figure 4 It is a radial characteristic map of the bidirectional gradient tissue in Example 2 of the present invention;

[0026] Figure 5 It is a radial characteristic map of the bidirectional gradient tissue in Example 3 of the present invention; DETAILED DESCRIPTION

[0027] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.

[0028] The present invention aims at the stress characteristics and damage mode of integral structural parts such as aerospace aircraft beams, blade disks and shafts, that is, the surface of the integral structural parts bears the greatest stress, and cracks are easily initiated from the surface and extend to the center. A method for preparing a high-strength and high-toughness titanium alloy with a bidirectional gradient structure is proposed, taking Ti55531 (high-strength and high-toughness β-type) titanium alloy as an example, comprising the following steps:

[0029] Step 1: A high-energy pulse current is used to rapidly heat one end and the center of a round rod or plate-shaped high-strength and toughness titanium alloy having a dual-state structure (a structure in which grains coexist in equiaxed α phase and lamellar α phase). The heating is started from room temperature, and the heating rate is 30-35°C / s. The heating temperature is 900-920°C (β single-phase region). After keeping the temperature for 30-90s, the alloy is cooled to room temperature with water. A dual-state structure gradually changes from a dual-state structure to a pure β phase is obtained in the axial direction in the heating area of ​​the titanium alloy.

[0030] Step 2: The titanium alloy containing dual-state structure in half of the area obtained in step 1 is subjected to aging treatment at 600-650°C for 5-6 hours, and air-cooled to room temperature. The unheated area in step 1 is an axial gradient of dual-state structure gradually changing to lamellar α phase, and the pure β phase in the heated area precipitates lamellar α phase, forming an axial gradient structure of dual-state structure gradually changing to lamellar α phase;

[0031] Step 3: The titanium alloy with axial gradient structure obtained in step 2 is subjected to surface laser shock strengthening treatment, with a laser pulse width of 8 to 10 ns and 2 to 5 shock times, so as to obtain a radial gradient structure from the surface to the core of the component, and the thickness of the radial surface fine grain structure is 30 to 100 μm. Finally, a bidirectional gradient structure with gradient distribution (gradual transition) in both axial and radial directions is obtained in the high-strength and toughness titanium alloy. The alloy has a gradient along the axial direction from a dual-state structure to a lamellar α-phase structure, which can realize a titanium alloy integral structure with dual performance functional effects; the surface radial gradient structure is to improve the surface bending fatigue crack initiation resistance of the integral structure, thereby effectively improving the service performance and safety stability of the titanium alloy integral structure.

[0032] Example 1

[0033] The present invention provides a method for preparing a Ti55531 titanium alloy with a bidirectional gradient structure, comprising the following steps:

[0034] (1) A copper plate is used to clamp and fix one end and the center of the Ti55531 alloy sample to be heated, so that the copper plate can conduct heat and achieve high-energy pulse current heating at a rate of 30°C / s. An infrared thermometer is used for real-time temperature measurement to ensure that the temperature of high-energy pulse current heating is 900°C, and the temperature is kept for 90s and then cooled to room temperature with water.

[0035] (2) The heated sample was placed in a tubular vacuum furnace and subjected to a long-term low-temperature aging treatment at a constant temperature of 650°C for 5 h, and then air-cooled to room temperature to obtain an axial gradient structure in which the equiaxed α phase gradually changes into a lamellar α phase, such as Figure 1 As shown, the up and down directions are axial, the upper part is the dual-state structure, and the lower part is the lamellar α phase. The black frame can be ignored.

[0036] (3) The titanium alloy with axial gradient structure obtained in step 2 is subjected to surface laser shock strengthening treatment, with a laser pulse width of 8 ns and 5 shock times, so that the radial gradient structure from the surface to the core of the component is obtained, and the radial surface fine grain structure thickness is 100 μm, as shown in FIG. Figure 2 As shown, the horizontal direction indicates the radial direction, and the right side is the surface fine-grained area.

[0037] Figure 3 The red represents the α phase, and the green represents the β phase. Figure 3 It can be seen that in the bidirectional gradient structure, not only the gradient fine grain structure is achieved from the radial surface to the core, but also the α phase content shows a gradient decreasing trend from the surface to the core due to the stress-induced α phase transformation, thereby significantly increasing the α nucleation rate and relative content of the surface. Therefore, a bidirectional gradient structure with gradient distribution in both the axial and radial directions is finally obtained in the Ti55531 alloy.

[0038] Example 2

[0039] The present invention provides a method for preparing a Ti55531 titanium alloy with a bidirectional gradient structure, comprising the following steps:

[0040] (1) A copper plate is used to clamp and fix one end and the center of the Ti55531 alloy sample to be heated, so that the copper plate can conduct heat and achieve high-energy pulse current heating at a rate of 35°C / min. An infrared thermometer is used to measure the temperature in real time to ensure that the temperature of the high-energy pulse current heating is 920°C, and the temperature is kept for 30 seconds and then cooled to room temperature with water.

[0041] (2) The heated sample is placed in a tubular vacuum furnace and subjected to a long-term low-temperature aging treatment at a constant temperature of 600°C for 6 h, and then air-cooled to room temperature;

[0042] (3) The titanium alloy with axial gradient structure obtained in step 2 is subjected to surface laser shock strengthening treatment, with a laser pulse width of 10 ns and a shock frequency of 2 times, so as to obtain a component from the surface ( Figure 4 The radial gradient structure from the bright area on the left to the center has a radial surface fine grain structure thickness of 30 μm. Figure 4 As shown, a bidirectional gradient structure of the titanium alloy with gradient distribution in both the axial and radial directions is achieved, and the black frame can be ignored.

[0043] Example 3

[0044] The present invention provides a method for preparing a Ti55531 titanium alloy with a bidirectional gradient structure, comprising the following steps:

[0045] (1) A copper plate is used to clamp and fix one end and the center of the Ti55531 titanium alloy sample to be heated, so that the copper plate can conduct heat and achieve high-energy pulse current heating at a rate of 32°C / min. An infrared thermometer is used to measure the temperature in real time to ensure that the temperature of the high-energy pulse current heating is 910°C, and the temperature is kept for 60 seconds and then cooled to room temperature with water;

[0046] (2) The above sample was placed in a tubular vacuum furnace and subjected to a long-term low-temperature aging treatment at a constant temperature of 620°C for 5.5 hours, and then air-cooled to room temperature;

[0047] (3) The titanium alloy with axial gradient structure obtained in step 2 was subjected to surface laser shock strengthening treatment, with a laser pulse width of 9 ns and 3 shock times, thereby obtaining a radial gradient structure from the surface to the core of the component, and the radial surface fine grain structure thickness was 60 μm, as shown in FIG. Figure 5 As shown, a bidirectional gradient structure of the titanium alloy with gradient distribution in both the axial and radial directions is achieved, and the black frame can be ignored.

Claims

1. A method for preparing a high-strength and tough titanium alloy with a bidirectional gradient structure, characterized in that: The following steps are involved: S1, heating a part of the high-strength and toughness titanium alloy with a dual-state structure to a β single-phase region, wherein one end of the region is one end of the high-strength and toughness titanium alloy, and the other end of the region is a cross section in the length direction of the high-strength and toughness titanium alloy, then keeping the temperature, and then water-cooling to room temperature, wherein the region gradually changes from the dual-state structure to the β phase along the axial direction; S2, subjecting the titanium alloy obtained in S1 to aging treatment at 600-650°C for 5-6h, and then air-cooling to room temperature, to obtain a high-strength and tough titanium alloy with an axial gradient structure gradually changing from a dual-state structure to a lamellar α phase; S3, performing surface laser shock strengthening treatment on the titanium alloy obtained in S2 to obtain a high-strength and tough titanium alloy with a radial gradient structure from the surface to the core.

2. The method for preparing a high-strength and tough titanium alloy with a bidirectional gradient structure according to claim 1, characterized in that: The β single phase region described in S1 is 900-920°C.

3. The method for preparing a high-strength and tough titanium alloy with a bidirectional gradient structure according to claim 1, characterized in that: The high-strength and toughness titanium alloy described in S1 is in the shape of a round rod or a plate, and the cross section is located at the center of the high-strength and toughness titanium alloy.

4. The method for preparing a high-strength and tough titanium alloy with a bidirectional gradient structure according to claim 1, characterized in that: The holding time in S1 is 30 to 90 seconds.

5. The method for preparing a high-strength and tough titanium alloy with a bidirectional gradient structure according to claim 1, characterized in that: In S1, high-energy pulse current is used to heat the high-strength and toughness titanium alloy.

6. The method for preparing a high-strength and tough titanium alloy with a bidirectional gradient structure according to claim 5, characterized in that: In S1, the high-strength and toughness titanium alloy is heated from room temperature at a heating rate of 30 to 35°C / s.

7. The method for preparing a high-strength and tough titanium alloy with a bidirectional gradient structure according to claim 1, characterized in that: The radial thickness of the surface fine-grained structure in S3 is 30 to 100 μm.

8. The method for preparing a high-strength and tough titanium alloy with a bidirectional gradient structure according to claim 1, characterized in that: The laser pulse width in S3 is 8 to 10 ns.

9. The method for preparing a high-strength and tough titanium alloy with a bidirectional gradient structure according to claim 1, characterized in that: The number of laser shocks in S3 is 2 to 5 times.

10. A high-strength and tough titanium alloy with a bidirectional gradient structure obtained by the method for preparing a high-strength and tough titanium alloy with a bidirectional gradient structure as claimed in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Laser impact strengthening method of biphase titanium alloy additive component

    CN110629014A

  • Titanium alloy with gradient microstructure and preparation method of titanium alloy

    CN113502442A

  • Titanium alloy material gradient micro-nano structure impacted by laser and preparation method of titanium alloy material gradient micro-nano structure

    CN115287560A

  • Titanium / aluminum composite material with high interface bonding strength and rolling composite forming method

    CN116833222A

  • Near-alpha titanium alloy with double-state-lamellar gradient mixed tissue structure and preparation device and method

    CN116837310A

Cited By

  • Titanium alloy variable cross-section gradient structure dual-performance disc rolling integrated forming method and disc part

    CN119525411A