Faraday electrostatic shielding magnetron sputtering device
By introducing Faraday electrostatic shielding effect in magnetron sputtering equipment, the ground grid electrode is used to reduce the ion bombardment damage of MoS2 film, the defects introduced by high-energy particle bombardment in magnetron sputtering coating technology are solved, and the silicon-based MoS2 differentiation is improved Efficiency and photovoltaic performance of junction solar cells.
Patent Information
- Application Number
- CN202410954596.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
In photovoltaic cells, the stress and vacancy defects introduced by bombardment of high-energy particles in magnetron sputtering coating technology affect the magnetic moment, energy band structure and optical properties of the MoS2 film, resulting in a decrease in cell efficiency, and a full stoichiometric ratio of molybdenum sulfide is prepared Films are difficult, and traditional sputtering methods often lead to sulfur-poor molybdenum-rich state, affecting electrical and optical properties.
Faraday electrostatic shielded magnetron sputtering device is adopted to introduce electrostatic shielding effect into magnetron sputtering equipment through ground grid electrodes, reducing ion bombardment damage during sputtering, optimizing the film formation process of MoS2 films, and ensuring sufficient sulfur replenishment. , form high-quality MoS2 films.
It effectively reduces the vacancy defects of MoS2 thin film, improves the conversion efficiency of silicon-based MoS2 heterojunction solar cells, improves photovoltaic performance, and maintains the cost of existing processes and equipment stability.
Smart Images

Figure CN118910543A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of two-dimensional thin film preparation and photovoltaic application thereof, and specifically relates to a Faraday electrostatic shielding magnetron sputtering device. Background Art
[0002] Magnetron sputtering is a commonly used thin film deposition technology. It uses a magnetic field in a vacuum environment to accelerate ions, causing them to collide with a target material and deposit the atoms or molecules of the target material onto the surface of the substrate to form a thin film layer. The application of this technology in photovoltaic cells can be used to improve the light absorption, electron transmission performance or increase durability of the cell, thereby improving the efficiency and stability of photovoltaic cells.
[0003] In the field of photovoltaic cells, magnetron sputtering coating technology is an effective method for preparing MoS2 thin films, but during the sputtering process, due to the bombardment of high-energy particles in the plasma, stress and a large number of vacancy defects will inevitably be introduced into the prepared film. The formation of these defects can cause changes in the magnetic moment, band structure and optical properties of MoS2, which will have an adverse effect on its electronic and optoelectronic properties and reduce the efficiency of the battery; secondly, the physical properties of the two elements in the molybdenum disulfide film are quite different, so it is difficult to prepare a fully stoichiometric molybdenum sulfide film, the preparation technology is limited and the repeatability is relatively low. Due to the huge difference in the vaporization heat and saturated vapor pressure of molybdenum and sulfur, the molybdenum sulfide film prepared by the traditional sputtering method is mostly in a state of sulfur-poor and molybdenum-rich after film formation, which will affect the electrical and optical properties of molybdenum sulfide, and thus affect its photovoltaic applications. Summary of the invention
[0004] The purpose of the present invention is to provide a Faraday electrostatic shielding magnetron sputtering device, which can reduce the ion bombardment effect in the thin film deposition process, thereby improving the properties of MoS2 thin films and enhancing the photovoltaic performance of its silicon-based solar cells.
[0005] The technical solution adopted by the present invention is as follows:
[0006] A Faraday electrostatic shielding magnetron sputtering device, comprising a magnetron sputtering device, a solar cell and:
[0007] A grounded grid electrode, the grid electrode is placed between the substrate and the target and is in electrical contact with the substrate, and the metal grid has an aperture of 2 mm;
[0008] MoS2 thin film, wherein the MoS2 thin film introduces an electrostatic shielding effect during the preparation process using a magnetron sputtering method;
[0009] The solar cell structure is, from top to bottom, a front Ag metal gate electrode, a front ITO layer, a front MoS2 film, a front SiOx passivation film, a P-type silicon substrate, a back SiOx passivation film, a back boron-doped μc-SiOx:H layer, a back ITO layer, and a back Ag metal electrode.
[0010] The electrostatic shielding effect is used to reduce ion bombardment damage in the process of preparing MoS2 thin film by sputtering. The invention is characterized in that: a 99.99% high-purity MoS2 target is used as the sputtering target material, a 13.56MHz radio frequency source is used as the sputtering power source, high-purity Ar and high-purity H2 are used as the sputtering gas, and the introduced grounded grid electrode is installed in the magnetron sputtering equipment.
[0011] A method for preparing a solar cell, the method comprising the following steps:
[0012] S1: Select a P-type double-throw CZ low-resistance single crystal silicon with a thickness of 500 μm and a resistivity of 1 to 10 Ω·cm as the substrate, and use a 10% HF aqueous solution to remove the natural oxide layer on the surface;
[0013] S2: forming a passivation layer on the silicon surface by wet chemical passivation;
[0014] A SiOx passivation film of 1 to 1.5 nm is formed under the condition of high temperature oxidation at 110°C for 10 min in a concentrated nitric acid solution with a mass fraction of 68%.
[0015] S3: A MoS2 film with ordered microstructure and good crystal quality is obtained on the front side of the silicon substrate using a magnetron sputtering device, and a 50nm boron-doped μc-SiOx:H layer is grown on the reverse side of the silicon substrate using PECVD technology as a back surface reflection field to selectively transmit electrons;
[0016] S4: A 70nm thick indium tin oxide (ITO) film is sputtered on both sides of a silicon substrate by magnetron sputtering, a 700nm silver grid line is prepared on the front side, and a 700nm full silver electrode is prepared on the back side.
[0017] The solar cell is a silicon-based MoS2 heterojunction cell.
[0018] The invention discloses an application of a Faraday electrostatic shielding magnetron sputtering device, which is used to introduce a Faraday cage into the original magnetron sputtering equipment to reduce the bombardment of charged particles on the substrate surface during the coating process.
[0019] In magnetron sputtering equipment, a grounded metal grid is installed at the anode of the discharge electrode plate, so that the grid and the anode form a structure similar to a metal shell, called a "Faraday cage", and the deposition substrate is placed near the anode inside it. During the sputtering process, this grounded metal Faraday cage can produce an electrostatic shielding effect, making the potential difference and electrostatic field inside the area zero, and the charges distributed on the surface of the Faraday cage are conducted to the ground; in this way, the charged particles in the sputtering glow will not be accelerated by the electrostatic field when entering the Faraday cage, effectively reducing the ion bombardment kinetic energy near the surface of the substrate inside the cage, weakening the bombardment stress during the film growth process, and improving the vacancy defects in the MoS2 film caused by sputtering bombardment, and improving the efficiency of silicon-based MoS2 heterojunction solar cells.
[0020] Specific:
[0021] During magnetron sputtering, electrons collide with Ar atoms in the cavity under the action of the electric field. After the collision, Ar is ionized to form Ar ions. Electrons carry a large number of high-energy Ar ions to bombard the MoS2 target, causing the film precursor particles to detach from the target. These high-energy particles that detach from the target are blocked by the grounded grid while moving toward the substrate: the particles that pass through the grid have their charges conducted away, diffuse to the substrate base with kinetic energy, and adhere to the substrate surface to form a film, greatly reducing the bombardment of the substrate surface; and some of the precursor particles attached to the grid will desorb and evaporate under appropriate temperature conditions. Compared with metal molybdenum, sulfur has a lower melting and boiling point and a higher saturated vapor pressure. Therefore, when the ambient temperature and pressure meet the conditions, the S component attached to the grounded grid electrode will be preferentially and selectively evaporated, leaving the difficult-to-evaporate metal Mo. The gate-assisted magnetron sputtering preparation method not only weakens the bombardment of high-energy particles in magnetron sputtering, but also achieves the effect of "secondary sulfur replenishment" for the initially deposited MoS2 film.
[0022] The technical effects achieved by the present invention are:
[0023] A Faraday electrostatic shielding magnetron sputtering device of the present invention reduces ion bombardment during magnetron sputtering by grounding the grid to obtain a higher quality MoS2 film. For example, it is used to improve the conversion efficiency of silicon-based MoS2 heterojunction solar cells; it does not need to increase the cost, and only needs to add a grounding metal mesh on the basis of the existing mature process. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 1 is a SEM surface image of MoS2 thin film prepared under different preparation conditions in the embodiment of the present invention;
[0025] Among them, (a) non-gate assisted magnetron sputtering; (b) gate assisted magnetron sputtering;
[0026] Figure 2The XRD diffraction pattern of the MoS2 film prepared in the embodiment of the present invention and the Raman scattering spectrum of the MoS2 film prepared;
[0027] Figure 3 is the Mo-3d core level peak of the MoS2 film in the embodiment of the present invention;
[0028] (a) XPS fitting spectrum; (b) XPS spectrum corresponding to the S2p core level peak;
[0029] Figure 4 The MoS2 film is prepared in the embodiment of the present invention;
[0030] (a)(αhν) 1 / 2 (a) The relationship between the absorption coefficient (α) and the photon energy (hν); (b) The relationship between the absorption coefficient (α) and the photon energy;
[0031] Figure 5 It is a silicon-based MoS2 photovoltaic device prepared by additional gate magnetron sputtering in an embodiment of the present invention;
[0032] (a) Illumination JV characteristics, the illumination IV test condition is one sun; (b) External quantum efficiency;
[0033] Figure 6 (a) is a dark state JV curve of a MoS2 / p-Si heterojunction solar cell in a semi-logarithmic coordinate system in an embodiment of the present invention; (b) is a dark state JV characteristic curve of a MoS2 / p-Si heterojunction solar cell in a positive bias region in a double logarithmic coordinate system;
[0034] Figure 7 (a) An optical diagram of the basic structure of a gate-assisted magnetron sputtering device in an embodiment of the present invention; and (b) A schematic diagram of the principle structure of a gate-assisted magnetron sputtering process for depositing MoS2. DETAILED DESCRIPTION
[0035] In order to make the purpose and advantages of the present invention more clearly understood, the present invention is specifically described below in conjunction with embodiments. It should be understood that the following text is only used to describe one or several specific embodiments of the present invention, and does not strictly limit the scope of protection of the specific claims of the present invention.
[0036] The present invention can further improve the efficiency of silicon-based MoS2 heterojunction solar cells without increasing equipment and process costs, thereby reducing the production cost of commercial photovoltaic modules and promoting changes in energy consumption patterns.
[0037] Embodiment 1:
[0038] like Figure 1-Figure 7As shown, a Faraday electrostatic shielding magnetron sputtering device includes a magnetron sputtering device, a solar cell and a grounded metal grid, wherein the grid electrode is arranged between the substrate and the target material, and the metal grid aperture is 2 mm;
[0039] MoS2 thin film, MoS2 thin film introduces electrostatic shielding effect in the preparation of magnetron sputtering equipment;
[0040] The solar cell structure from top to bottom is: front Ag metal gate electrode, front ITO layer, front MoS2 film, front SiOx passivation film, P-type silicon substrate, back SiOx passivation film, back boron-doped μc-SiOx:H layer, back ITO layer, and back Ag metal electrode.
[0041] The electrostatic shielding effect is used to reduce ion bombardment damage in the process of preparing MoS2 thin film by sputtering. The invention is characterized in that: a 99.99% high-purity MoS2 target is used as the sputtering target material, a 13.56MHz radio frequency source is used as the sputtering power source, high-purity Ar and high-purity H2 are used as the sputtering gas, and the introduced grounded grid electrode is installed in the magnetron sputtering equipment.
[0042] Embodiment 2:
[0043] A method for preparing a solar cell, the method comprising the following steps:
[0044] S1: Select a P-type double-throw CZ low-resistance single crystal silicon with a thickness of 500 μm and a resistivity of 1 to 10 Ω·cm as the substrate, and use a 10% HF aqueous solution to remove the natural oxide layer on the surface;
[0045] S2: forming a passivation layer on the silicon surface by wet chemical passivation;
[0046] A SiOx passivation film of 1 to 1.5 nm is formed under the condition of high temperature oxidation at 110°C for 10 min in a concentrated nitric acid solution with a mass fraction of 68%.
[0047] S3: A MoS2 film with ordered microstructure and good crystal quality is obtained on the front side of the silicon substrate using a magnetron sputtering device, and a 50nm boron-doped μc-SiOx:H layer is grown on the reverse side of the silicon substrate using PECVD technology as a back surface reflection field to selectively transmit electrons;
[0048] S4: A 70nm thick indium tin oxide (ITO) film is sputtered on both sides of a silicon substrate by magnetron sputtering, a 700nm silver grid line is prepared on the front side, and a 700nm full silver electrode is prepared on the back side.
[0049] The solar cell is a silicon-based MoS2 heterojunction cell.
[0050] Embodiment 3:
[0051] The invention discloses an application of a Faraday electrostatic shielding magnetron sputtering device, which is used to introduce a Faraday cage into the original magnetron sputtering equipment to reduce the bombardment of charged particles on the substrate surface during the coating process.
[0052] Implementation:4:
[0053] like Figure 1-Figure 7 As shown, the SEM image, XPS image, XRD, and Raman of the silicon-based MoS2 film prepared in this embodiment;
[0054] In order to study the change of the crystalline structure of MoS2 film under different magnetron sputtering conditions, we first observed the change of its surface morphology with the sputtering method, such as Figure 1 a. It can be seen that in the MoS2 film sample prepared without gate-assisted magnetron sputtering, obvious petal-shaped MoS2 crystals have appeared, with a grain size of ~100nm. The MoS2 film has a high degree of crystallinity, but the film quality is poor; with the change of magnetron sputtering mode, the MoS2 grain size decreases and the grain density decreases significantly, indicating that the crystal quality of the film is improved at this time. After adding the grounded grid electrode, the film precursor particles are blocked by the grounded grid in the process of moving toward the substrate, and the particles passing through the grid diffuse to the substrate base only by kinetic energy and adhere to the substrate surface to form a film, which greatly reduces the bombardment of the substrate surface and improves the crystal quality of the film.
[0055] like Figure 2 As shown in Figure 2, the XRD diffraction pattern of MoS2 film was used to further study its crystalline structure characteristics, such as Figure 2 a. As can be seen from the figure, the XRD diffraction spectrum of the MoS2 film sample only has one diffraction peak near 13.5°, corresponding to the hexagonal molybdenite crystal. <002> The 2D atomic layer plane is parallel to the growth base. It is inferred that the prepared MoS2 film has a high degree of crystallinity and the atomic layer preferentially grows parallel to the Si substrate surface. This result is mainly due to the fact that in the process of conventional DC magnetron sputtering of MoS2, high-energy ion bombardment produces high-energy sites for the adsorption of precursor atoms, which in turn promotes <002> The formation of MoS2 crystals.
[0056] In order to study the molecular vibration characteristics of MoS2 film, we tested the Raman spectrum of MoS2 film. Figure 2 b It can be seen that the two Raman scattering characteristic peaks correspond to the two vibration modes of MoS2: ~380cm -1 Left and right in-plane vibration (E 2g 1 ) mode and ~410cm -1 Out-of-plane vibration near 1g ) mode, and the frequency difference between the two vibration modes is greater than 33cm-1 , indicating that the prepared MoS2 film is a multilayer bulk material MoS2.
[0057] like Figure 3 As shown, in order to reveal the influence of gate-assisted magnetron sputtering on the defect state distribution in MoS2 film, the chemical bonding characteristics of MoS2 film at 70W sputtering power were studied by XPS spectrum. Figure 3 a is the XPS fitting result of the Mo 3d core energy level peak of the MoS2 thin film sample prepared on a p-type c-Si substrate with a 70W-RF sputtering power. The sample XPS peak position is corrected by the C1s characteristic peak with a binding energy of 284.5eV. It can be seen that the three oxidation state energy level peaks of Mo (Mo 4+ 、Mo 5+ and Mo 6+ ) and S2s energy level characteristic peak (~226.4eV), indicating that bulk-like MoS2 thin film was prepared under RF power of 70W. The Gauss-Lorentz fitting results of the Mo 3d core energy level peak of the XPS spectrum can be used to obtain the relative content of Mo in different valence states in the sample. Under RF-70W conditions, the Mo in MoS2 thin film 4+ The relative content reaches a maximum value of 63.63%, while Mo 5+ The minimum relative content is 31.04%, indicating that the oxygen vacancy defect density of the MoS2 film prepared under this condition is the lowest.
[0058] like Figure 4 As shown in the figure, the optical properties of MoS2 thin film were analyzed using thin film optical absorption spectrum. Figure 4 Absorption spectrum of MoS2 thin film prepared by gate-assisted magnetron sputtering: Figure 4 The Tauc plot method shown in a obtains the Eg of the MoS2 film as 1.27738 eV and the B factor as 642.0753. Figure 4 The light absorption spectrum of the film in b deduces that the Eu energy of the MoS2 film is 0.51eV. In the traditional magnetron sputtering method, the particle surface bombardment effect is strong, and the dangling bonds and defects in the MoS2 film are dense. Therefore, the microstructure in the MoS2 film is relatively disordered (B factor ~500, Eu energy ~0.48eV). With the introduction of the grounding grid, the high-energy particle bombardment effect is weakened, the influence on the diffusion and crystallization process of the film-forming particles is reduced, the film crystallinity is improved, the microstructure becomes dense and orderly, and the B factor and Eu energy are improved.
[0059] like Figure 5 As shown, the MoS2 thin film prepared by gate-assisted magnetron sputtering was applied to silicon-based MoS2 heterojunction solar cells, and the current-voltage (JV) response and spectral response of the battery device were studied. Figure 5a shows the illumination JV curves of silicon-based MoS2 photovoltaic devices prepared by conventional magnetron sputtering and gate-assisted magnetron sputtering, with the irradiation light source power density of 100 mW / cm 2 In this experiment, the short-circuit current J of the battery device sc All are corrected by their external quantum efficiency EQE, and the device J sc The results are consistent with the corresponding EQE fitting results. Compared with the traditional magnetron sputtering silicon-based MoS2 heterojunction photovoltaic device, the photovoltaic characteristics of the silicon-based MoS2 heterojunction battery device prepared by the additional gate magnetron sputtering method are significantly improved, and the open circuit voltage V oc From 222mV to 262mV, short circuit current J sc By 30.8mA / cm 2 Increased to 32.68 mA / cm 2 . In heterojunction solar cells, heterojunction interface defect recombination and carrier extraction are key factors affecting cell performance. Therefore, the improvement in photovoltaic performance of silicon-based MoS2 heterojunction devices is mainly attributed to the electrostatic shielding effect during gate-assisted magnetron sputtering, which weakens the surface bombardment of high-energy particles and reduces the MoS2 / p-Si interface defect density. However, after adding the gate, the FF factor of the silicon-based MoS2 heterojunction photovoltaic device dropped from 45.4% to 42.68%, indicating that the carrier extraction efficiency of the heterojunction interface is reduced, which is mainly related to the low crystallinity of the MoS2 film prepared by additional gate magnetron sputtering.
[0060] Figure 5 b is the spectral response characteristics of silicon-based MoS2 heterojunction photovoltaic devices prepared by traditional magnetron sputtering and gate-assisted magnetron sputtering. It can be seen that the overall EQE response of the MoS2 / p-Si heterojunction battery device with an additional gate has been improved; and the change trend of EQE is different in different incident light bands: in the medium and short wavelength range of 300-800nm, the EQE of the silicon-based MoS2 battery device is significantly improved after the additional gate, which is mainly attributed to the reduction of the defect density of the MoS2 film caused by the weakening of the high-energy ion bombardment; and in the medium and long wavelength range of 800-1100nm, the EQE of the silicon-based MoS2 battery device is slightly reduced after the additional gate, which is mainly related to the reduction of the crystallinity of the MoS2 layer and the obstruction of carrier transmission between heterojunctions. In addition, with the increase of the thickness of the MoS2 film, the EQE value of the silicon-based MoS2 heterojunction device with an additional gate in the medium and long wavelength band continues to decrease, which is attributed to the larger carrier recombination loss in the thicker MoS2 layer and the lower carrier transmission efficiency at the heterojunction interface, which is related to the Figure 5 This corresponds to the lower FF factor value in the 15-nm MoS2 / p-Si device in a.
[0061] like Figure 6 As shown, Figure 6a is the dark state JV curve of MoS2 / p-Si heterojunction solar cell in semi-logarithmic coordinate system. It can be seen that both types of MoS2 / p-Si battery devices show rectification characteristics, and the rectification ratio (I +1 / I -1 ) exceeds 1×10 3 The rectification characteristics of the MoS2 / p-Si heterojunction device prepared by the additional gate magnetron sputtering method are more obvious, with a rectification ratio of up to 3.10×10 4 This indicates that a MoS2 / p-Si Schottky junction with good performance is formed under the electrostatic shielding effect. Figure 6 b shows the dark state JV characteristic curve of the positive bias region of the MoS2 / p-Si heterojunction solar cell in the double logarithmic coordinate system. It can be seen from the figure that with the increase of the external bias value, the dark state JV response of all battery devices shows three obvious linear regions, and the slopes of the JV curves in different linear regions are different, indicating that the main control transmission mechanism of carriers in different voltage transformation regions is different. In the low bias value region I (V﹤0.1V), the battery parallel resistance R sh It is the main influencing factor of dark current; in the middle area II (V = 0.1 ~ 0.3V), the carrier main control transmission process is affected by the diffusion limitation mechanism and the recombination limitation mechanism; in the high bias area III (V ﹥ 0.3V), the battery series resistance R s Determines the carrier transport mechanism. To obtain the ideal factor (n) of a photovoltaic device, it is necessary to fit the diode formula of the II region of the device's dark state JV response: J = J0 [exp (qV / nkT) -1 ]Where J0 and n represent the reverse saturation current density and ideal factor of the battery, k is the Boltzmann constant, and T is the thermodynamic temperature. According to the fitting results, the ideal factor of the silicon-based MoS2 heterojunction photovoltaic device prepared by the gate-assisted magnetron sputtering method is close to 2 and has a value of 10 -6 The lower J0 value of orders of magnitude indicates that the carrier recombination current in the space charge region of the device is the main control transport current, reflecting the reduction of defect density in the gate-assisted magnetron sputtered MoS2 film.
[0062] The above is only a preferred embodiment of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principles of the present invention, and these improvements and modifications should also be considered as the protection scope of the present invention. The structures, devices and operating methods not specifically described and explained in the present invention shall be implemented according to the conventional means in the art unless otherwise specified and limited.
Claims
1. A Faraday electrostatic shielding magnetron sputtering device, Features: It includes a magnetron sputtering device, a solar cell and a grounded metal grid, wherein the grid electrode is made of metal silver, and the grid electrode is arranged between the substrate and the target material and is in electrical contact with the target material; MoS 2 The MoS film 2 The electrostatic shielding effect is introduced in the process of film preparation by magnetron sputtering; The solar cell structure is as follows from top to bottom: front Ag metal gate electrode, front ITO layer, front MoS 2 Thin film, front SiOx passivation film, P-type silicon substrate, back SiOx passivation film, back boron-doped μc-SiOx:H layer, back ITO layer, back Ag metal electrode.
2. A Faraday electrostatic shielding magnetron sputtering device according to claim 1, Features: The metal grid has an aperture of 2 mm.
3. A Faraday electrostatic shielding magnetron sputtering device according to claim 1, Features: The solar cell is silicon-based MoS 2 Heterojunction battery.
4. A method for preparing a solar cell, Features: The method comprises the following steps: S1: Select a P-type double-throw CZ low-resistance single crystal silicon with a thickness of 500 μm and a resistivity of 1 to 10 Ω·cm as the substrate, and use a 10% HF aqueous solution to remove the natural oxide layer on the surface; S2: forming a passivation layer on the silicon surface by wet chemical passivation; A SiOx passivation film of 1 to 1.5 nm is formed under the condition of high temperature oxidation at 110°C for 10 min in a concentrated nitric acid solution with a mass fraction of 68%. S3: Magnetron sputtering equipment is used on the front side of the silicon substrate to obtain MoS with ordered microstructure and good crystal quality. 2 Thin film, using PECVD technology to grow a 50nm boron-doped μc-SiOx:H layer on the reverse side of the silicon substrate as a back surface reflection field to selectively transmit holes; S4: A 70nm thick indium tin oxide (ITO) film is sputtered on both sides of a silicon substrate by magnetron sputtering, a 700nm silver grid line is prepared on the front side, and a 700nm full silver electrode is prepared on the back side.
5. Application of a Faraday electrostatic shielding magnetron sputtering device, Features: A Faraday cage is introduced into the original magnetron sputtering equipment to reduce the bombardment damage of charged particles in the plasma glow discharge on the surface of the deposited film during the sputtering coating process.