Environment-friendly efficient acid pickling high-strength steel surface silane pretreatment liquid and preparation method thereof
By using a pickled high-strength steel surface silane pretreatment solution composed of environmentally friendly solvents and silane coupling agents, the problems of limited effect on the surface treatment of high-strength steel by traditional pickled technology are solved, and the corrosion resistance and coating of metal surfaces are significantly improved. The installation adhesion provides new technical ideas for the field of metal surface treatment.
Patent Information
- Application Number
- CN202411210874.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The traditional pickling process has limited effect on the surface treatment of high-strength steel and has environmental protection problems, which is difficult to meet the high requirements of modern industry for material surface quality. The strong acids used at the same time are harmful to the human body and the environment.
Using environmentally friendly and efficient pickling high-strength steel surface silane pretreatment liquid composed of environmentally friendly solvents, silane coupling agents, additives, etc., control reaction conditions and treatment steps by optimizing the types and dosage of components, improving the surface treatment effect and forming stable The chemical bonding significantly improves the corrosion resistance and coating adhesion of metal surfaces.
Effectively improve the wetting and corrosion resistance of metal surfaces, improve the quality and durability of coatings, solve the environmental protection problems of traditional pickling processes, and provide new technical ideas for the field of metal surface treatment.
Smart Images

Figure BDA0005020286190000051 
Figure BDA0005020286190000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal material surface treatment, and specifically relates to an environmentally friendly and efficient pickling high-strength steel surface silane pretreatment liquid and a preparation method thereof. Background Art
[0002] In the field of metal material processing, high-strength steel is valued for its excellent mechanical properties and wide range of applications. However, during the production, processing and storage of high-strength steel, its surface is easily affected by oxidation, rust and other adverse effects, which not only damages the appearance of the material, but also reduces its service life and performance. Therefore, pre-treatment of the surface of high-strength steel to enhance its corrosion resistance and coating adhesion has become an important research direction in the field of metal surface treatment.
[0003] The traditional pickling process is a commonly used method in metal surface treatment. It can effectively remove pollutants such as scale and rust on the surface of steel, providing a clean metal surface for subsequent painting or anti-rust treatment. However, the traditional pickling process mostly uses strong acids, such as sulfuric acid and hydrochloric acid. These strong acids are not only harmful to the human body, but the waste liquid and waste gas generated during the treatment process will cause serious pollution to the environment. At the same time, the traditional pickling process has limited treatment effect on high-strength steel and it is difficult to meet the high requirements of modern industry for material surface quality. In recent years, with the increasing awareness of environmental protection and the continuous development of surface treatment technology, it has become a top priority to develop an environmentally friendly and efficient pickling high-strength steel surface treatment method. Summary of the invention
[0004] The present invention proposes an environmentally friendly and efficient silane pretreatment liquid for pickling high-strength steel surface and a preparation method thereof. The pretreatment liquid is composed of an environmentally friendly solvent, a silane coupling agent, an auxiliary agent, etc., and the type and amount of each component are optimized to achieve efficient and environmentally friendly treatment of the pickled high-strength steel surface. This technical solution ensures the treatment effect of the pretreatment liquid by controlling the reaction conditions and treatment steps, which not only solves the environmental protection problems existing in the traditional pickling process, but also improves the surface treatment effect of pickled high-strength steel, providing a new technical idea for the development of the field of metal surface pretreatment.
[0005] In order to achieve the above-mentioned purpose of the invention, the present invention provides an environmentally friendly and efficient silane pretreatment liquid for pickling high-strength steel surface, wherein the silane pretreatment liquid for pickling high-strength steel surface comprises the following components in parts by weight: 20 to 32 parts of silane coupling agent, 30 to 52 parts of organic solvent, 1 to 6 parts of acid catalyst, 0.5 to 5 parts of surfactant, 0.1 to 5 parts of corrosion inhibitor, 0.5 to 5 parts of stabilizer, 0.1 to 3 parts of defoaming agent, 0.1 to 4 parts of preservative, and 60 to 85 parts of deionized water.
[0006] In the above technical solution, further, the silane coupling agent is prepared by mixing γ-aminopropyl triethoxysilane, N-β-(aminoethyl)-γ-aminopropyl trimethoxysilane and 3-glycidyloxypropyl trimethoxysilane in a weight ratio of (3-4):3:3. The silane coupling agent is the main film-forming component. As a new type of surface treatment agent, the silane coupling agent has environmental protection characteristics such as non-toxic, odorless, and pollution-free. At the same time, it can form a stable chemical bond with the metal surface, significantly improving the corrosion resistance and coating adhesion of the metal surface.
[0007] Furthermore, the organic solvent is prepared by mixing ethanol (purity>99.8%) and isopropanol (purity≥99.7%) in a weight ratio of (2-3):2, and the organic solvent is used to dissolve the silane coupling agent.
[0008] The acidic catalyst is prepared by mixing acetic acid and phosphoric acid in a weight ratio of (6-7):3, and is used to promote the hydrolysis reaction of silane.
[0009] The surfactant is prepared by mixing sodium lauryl sulfate, polyoxyethylene octylphenol ether, fatty alcohol polyoxyethylene ether and cocamidopropyl betaine in a weight ratio of (5-6):5:5:4, and the surfactant is used to improve its wettability.
[0010] In addition, corrosion inhibitors, stabilizers, defoamers and preservatives are added to prevent metal corrosion, chelate metal ions, eliminate foam and inhibit bacteria and mold. Through reasonable agent selection and proportion control, the aim is to obtain a silane pretreatment agent with stable performance.
[0011] The corrosion inhibitor is prepared by mixing benzotriazole, methylbenzotriazole and 5,6-dimethylbenzotriazole in a weight ratio of (4-5):3:2, and is used for preventing metal corrosion.
[0012] The stabilizer is prepared by mixing disodium salt (EDTA) and trisodium salt (NTA) in a weight ratio of (2-3):2, and is used for chelating metal ions.
[0013] The defoamer is prepared by mixing an organic silicon defoamer, a polyether defoamer and a mineral oil defoamer in a weight ratio of (4-5):3:2, and is used for eliminating foam.
[0014] The preservative is prepared by mixing sodium benzoate and potassium sorbate in a weight ratio of (6-7):3, and is used for inhibiting bacteria and mold.
[0015] The deionized water as a solvent can ensure the stability and compatibility of each component in the treatment liquid. Through the dilution and mixing effect of the deionized water, each component can be evenly dispersed in the entire treatment liquid to form a uniform and stable system.
[0016] A method for preparing the above-mentioned environmentally friendly and efficient pickling high-strength steel surface silane pretreatment liquid, the preparation method comprising the following steps:
[0017] ① Pour ethanol (concentration>99.8%) and isopropanol (concentration≥99.7%) into a clean container according to the formula ratio and turn on the stirrer, stir at a speed of 200-300 rpm for 15-20 minutes to fully mix the two solvents to obtain an organic solvent.
[0018] ② Add acetic acid (concentration>80%) and phosphoric acid (concentration>85%) into another container according to the formula ratio and mix them. Use a stirrer to stir at a speed of 200-350 rpm for 10-15 minutes to obtain an acid catalyst.
[0019] ③ Add sodium lauryl sulfate, polyoxyethylene octylphenol ether, fatty alcohol polyoxyethylene ether and cocamidopropyl betaine into a container according to the formula ratio, mix, and stir at a speed of 300-400 rpm for 15-20 minutes to obtain a surfactant.
[0020] ④ Mix benzotriazole, methylbenzotriazole and 5,6-dimethylbenzotriazole according to the formula ratio, and stir at a speed of 400 to 500 rpm for 15 to 20 minutes to obtain a corrosion inhibitor.
[0021] ⑤ Mix disodium salt (EDTA) and trisodium salt (NTA) according to the formula ratio, and stir at a speed of 400-500 rpm for 20-30 minutes to obtain a stabilizer.
[0022] ⑥ Mix the organosilicon defoamer, polyether defoamer and mineral oil defoamer according to the formula ratio, and stir at a speed of 200 to 300 rpm for 15 to 20 minutes to obtain the defoamer.
[0023] ⑦ Mix sodium benzoate and potassium sorbate according to the formula ratio, and stir at a speed of 300-400 rpm for 20-30 minutes to obtain a preservative.
[0024] ⑧ γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-glycidyloxypropyltrimethoxysilane are mixed according to the formula ratio, and stirred at a speed of 400 to 500 rpm for 30 to 45 minutes to obtain a silane coupling agent.
[0025] ⑨ Pour the prepared organic solvent into the reactor, set the stirring speed to 200-300 rpm for stirring, slowly add the silane coupling agent into the reactor, and at the same time increase the stirring speed to 300-400 rpm, control the heating temperature to 50°C-60°C, and continue stirring for 60-90 minutes until the silane coupling agent is completely dissolved. Keep the stirring speed and heating temperature unchanged, add the prepared acidic catalyst, continue stirring for 25-30 minutes, and then add the prepared surfactant, corrosion inhibitor, stabilizer, defoamer and preservative in turn. After each additive is added, continue stirring for 10-15 minutes. After all components are added, adjust the stirring speed to 500-600 rpm, increase the heating temperature to 75-85°C, and stir for 120-150 minutes to finally obtain an environmentally friendly and efficient pickling high-strength steel surface silane pretreatment liquid.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The environmentally friendly and efficient silane pretreatment liquid for pickling high-strength steel surface provided by the present invention is characterized in that it can effectively improve the wettability and corrosion resistance of the metal surface, thereby improving the quality and durability of the coating, improving the surface treatment effect of pickling high-strength steel, and providing a new idea for the development of the field of metal surface treatment. The high-strength steel surface silane pretreatment liquid prepared by the method has a wide range of application prospects and can be applied to the surface treatment of metal materials in the fields of automobiles, ships, and construction, which is of great significance to improving the service life and performance of materials. DETAILED DESCRIPTION
[0028] The present invention is further described below in conjunction with specific examples, but the present invention is not limited in any way. To avoid redundant description, the raw materials in the following examples are all commercially available products unless otherwise specified, and the methods used are all conventional methods unless otherwise specified.
[0029] The invention discloses an environmentally friendly and efficient silane pretreatment liquid for pickling high-strength steel surface. The silane pretreatment liquid for pickling high-strength steel surface comprises the following components in parts by weight: 20 to 32 parts of a silane coupling agent, 30 to 52 parts of an organic solvent, 1 to 6 parts of an acidic catalyst, 0.5 to 5 parts of a surfactant, 0.1 to 5 parts of a corrosion inhibitor, 0.5 to 5 parts of a stabilizer, 0.1 to 3 parts of a defoaming agent, 0.1 to 4 parts of a preservative, and 60 to 85 parts of deionized water.
[0030] The matters not described in the following embodiments are the same as the description of the above specific implementation methods.
[0031] Example
[0032] An environmentally friendly and efficient silane pretreatment liquid for pickling high-strength steel surface. The components and mass contents of the silane pretreatment liquid for pickling high-strength steel surface of Examples 1-10 are shown in Table 1.
[0033] Table 1 Components and contents of silane pretreatment liquid for pickled high-strength steel surface in Examples 1-10
[0034]
[0035] A method for preparing the above-mentioned environmentally friendly and efficient pickling high-strength steel surface silane pretreatment liquid, the specific process steps are:
[0036] ① Pour ethanol (concentration>99.8%) and isopropanol (concentration≥99.7%) into a clean container according to the formula ratio and turn on the stirrer, stir at 300 rpm for 20 minutes to fully mix the two solvents to obtain an organic solvent.
[0037] ② Add acetic acid (concentration>80%) and phosphoric acid (concentration>85%) into another container according to the formula ratio, and stir at 350 rpm for 15 minutes using a stirrer to obtain an acid catalyst.
[0038] ③ Add sodium lauryl sulfate, polyoxyethylene octylphenol ether, fatty alcohol polyoxyethylene ether and cocamidopropyl betaine into a container according to the formula ratio, mix, and stir at a speed of 400 rpm for 20 minutes to obtain a surfactant.
[0039] ④ Mix benzotriazole, methylbenzotriazole and 5,6-dimethylbenzotriazole according to the formula ratio, and stir at a speed of 500 rpm for 20 minutes to obtain a corrosion inhibitor.
[0040] ⑤ Mix disodium salt (EDTA) and trisodium salt (NTA) according to the formula ratio, and stir at a speed of 500 rpm for 30 minutes to obtain a stabilizer.
[0041] ⑥ Mix the organosilicon defoamer, polyether defoamer and mineral oil defoamer according to the formula ratio, and stir at a speed of 300 rpm for 20 minutes to obtain the defoamer.
[0042] ⑦ Mix sodium benzoate and potassium sorbate according to the formula ratio, and stir at a speed of 400 rpm for 30 minutes to obtain a preservative.
[0043] ⑧ γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-glycidyloxypropyltrimethoxysilane were mixed according to the formula ratio, and stirred at a speed of 500 rpm for 45 minutes to obtain a silane coupling agent.
[0044] ⑨ Pour the prepared organic solvent into the reactor, set the stirring speed to 300 rpm for stirring, slowly add the silane coupling agent into the reactor, and at the same time increase the stirring speed to 300-400 rpm, control the heating temperature to 60°C, and continue stirring for 90 minutes until the silane coupling agent is completely dissolved. Keep the stirring speed and heating temperature unchanged, add the prepared acid catalyst, continue stirring for 30 minutes, and then add the prepared surfactant, corrosion inhibitor, stabilizer, defoamer and preservative in turn. After each additive is added, continue stirring for 15 minutes. After all components are added, adjust the stirring speed to 600 rpm, increase the heating temperature to 85°C, and stir for 150 minutes to finally obtain an environmentally friendly and efficient pickling high-strength steel surface silane pretreatment liquid.
[0045] The silane pretreatment liquid on the surface of pickled high-strength steel prepared by the above-mentioned process was used, and the test pieces were immersed in the silane pretreatment liquid on the surface of pickled high-strength steel prepared in Examples 1-10, and the test pieces were taken out and the anti-rust performance was tested according to SHT 0533 "Rust Assessment Method for Rust Test Pieces of Anti-Rust Grease". In addition, the contact angle of the surface silane pretreatment liquid was measured by the Sessile drops method using the Dataphysics OCA50 fully automatic contact angle measuring instrument. The experimental temperature was room temperature, and the droplet volume was controlled to 4 μL using a precision syringe. The instrument measured an angle range of 0 to 180°, the video speed was 120 images per second, the measurement error was ±0.1°, and the average value was taken for multiple measurements. Because the surface tension spreads into a certain arc on the surface of the substrate, the software automatically calculates the contact angles on the left and right sides after selecting the reference plane. When the contact angles at both ends are close, the average value is taken as the wetting angle of the rolling liquid. Table 2 shows the application and implementation technology effects of the products obtained in Examples 1-10.
[0046] Table 2 Implementation technical effects of products obtained in Examples 1-10
[0047]
[0048] The present invention proposes an environmentally friendly and efficient silane pretreatment liquid for pickling high-strength steel surface. The implementation technical effects of the products obtained by Examples 1-10 in Table 2 show that the pretreatment liquid not only meets the actual production needs, but also solves the environmental problems existing in the traditional pickling process. Therefore, it has important industry promotion significance.
[0049] For any technician familiar with the art, without departing from the scope of the technical solution of the present invention, the technical content disclosed above can be used to make many possible changes and modifications to the technical solution of the present invention, or modified into equivalent embodiments with equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention should still fall within the scope of protection of the technical solution of the present invention.
Claims
1. An environmentally friendly and efficient silane pretreatment solution for pickling high-strength steel surface, characterized in that: The silane pretreatment liquid for pickling high-strength steel surface comprises the following components in parts by weight: 20 to 32 parts of silane coupling agent, 30 to 52 parts of organic solvent, 1 to 6 parts of acidic catalyst, 0.5 to 5 parts of surfactant, 0.1 to 5 parts of corrosion inhibitor, 0.5 to 5 parts of stabilizer, 0.1 to 3 parts of defoaming agent, 0.1 to 4 parts of preservative and 60 to 85 parts of deionized water.
2. The silane pretreatment liquid for pickling high-strength steel surface according to claim 1, characterized in that: The silane coupling agent is prepared by mixing gamma-aminopropyl triethoxysilane, N-beta-(aminoethyl)-gamma-aminopropyl trimethoxysilane and 3-glycidyloxypropyl trimethoxysilane in a weight ratio of (3-4):3:
3.
3. The silane pretreatment liquid for pickling high-strength steel surface according to claim 1, characterized in that: The organic solvent is prepared by mixing ethanol and isopropanol in a weight ratio of (2-3):
2.
4. The silane pretreatment liquid for pickling high-strength steel surface according to claim 1, characterized in that: The acid catalyst is prepared by mixing acetic acid and phosphoric acid in a weight ratio of (6-7):
3.
5. The silane pretreatment liquid for pickling high-strength steel surface according to claim 1, characterized in that: The surfactant is prepared by mixing sodium lauryl sulfate, polyoxyethylene octylphenol ether, fatty alcohol polyoxyethylene ether and cocamidopropyl betaine in a weight ratio of (5-6):5:5:
4.
6. The silane pretreatment liquid for pickling high-strength steel surface according to claim 1, characterized in that: The corrosion inhibitor is prepared by mixing benzotriazole, methylbenzotriazole and 5,6-dimethylbenzotriazole in a weight ratio of (4-5):3:2; the stabilizer is prepared by mixing disodium salt EDTA and trisodium salt NTA in a weight ratio of (2-3):
2.
7. The silane pretreatment liquid for pickling high-strength steel surface according to claim 1, characterized in that: The defoamer is prepared by mixing an organosilicon defoamer, a polyether defoamer and a mineral oil defoamer in a weight ratio of (4-5):3:2; and the preservative is prepared by mixing sodium benzoate and potassium sorbate in a weight ratio of (6-7):
3.
8. A method for preparing an environmentally friendly and efficient silane pretreatment solution for pickling high-strength steel surface as claimed in claim 1, characterized in that: The preparation method comprises the following steps: ① Mix ethanol and isopropanol according to the formula ratio, and stir at a speed of 200 to 300 rpm for 15 to 20 minutes to obtain an organic solvent; ② Mix acetic acid and phosphoric acid according to the formula ratio, and stir at a speed of 200 to 350 rpm for 10 to 15 minutes to obtain an acid catalyst; ③ Mix sodium lauryl sulfate, polyoxyethylene octylphenol ether, fatty alcohol polyoxyethylene ether and cocamidopropyl betaine according to the formula ratio, and stir at a speed of 300 to 400 rpm for 15 to 20 minutes to obtain a surfactant; ④ Mix benzotriazole, methylbenzotriazole and 5,6-dimethylbenzotriazole according to the formula ratio, and stir at a speed of 400 to 500 rpm for 15 to 20 minutes to obtain a corrosion inhibitor; ⑤ Mix disodium salt EDTA and trisodium salt NTA according to the formula ratio, and stir at a speed of 400 to 500 rpm for 20 to 30 minutes to obtain a stabilizer; ⑥ Mix the organosilicon defoamer, polyether defoamer and mineral oil defoamer according to the formula ratio, and stir at a speed of 200 to 300 rpm for 15 to 20 minutes to obtain the defoamer; ⑦ Mix sodium benzoate and potassium sorbate according to the formula ratio, and stir at a speed of 300 to 400 rpm for 20 to 30 minutes to obtain a preservative; ⑧ γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-glycidyloxypropyltrimethoxysilane are mixed according to the formula ratio, and stirred at a speed of 400 to 500 rpm for 30 to 45 minutes to obtain a silane coupling agent; ⑨ Pour the prepared organic solvent into the reactor, set the stirring speed to 200-300 rpm for stirring, slowly add the silane coupling agent into the reactor, and at the same time increase the stirring speed to 300-400 rpm, control the heating temperature to 50°C-60°C, and continue stirring for 60-90 minutes until the silane coupling agent is completely dissolved; keep the stirring speed and heating temperature unchanged, add the prepared acid catalyst, continue stirring for 25-30 minutes, and then add the prepared surfactant, corrosion inhibitor, stabilizer, defoamer and preservative in turn. After each additive is added, continue stirring for 10-15 minutes; after all components are added, adjust the stirring speed to 500-600 rpm, increase the heating temperature to 75-85°C, and stir for 120-150 minutes to finally obtain an environmentally friendly and efficient pickling high-strength steel surface silane pretreatment liquid.
Citation Information
Patent Citations
Silane forming agent and preparation method thereof
CN102978594A
Metal surface treatment agent with silane coupling agents as main components and preparation method thereof
CN105441920A
Silane self-assembly treating agent for metal coating pretreatment and application of silane self-assembly treating agent
CN106637174A
Silicane treating agent and method for preparing silicane treating agent
CN107460465A
Environment-friendly multi-metal water-based antirust agent and preparation method
CN109763120A