Preparation method of aluminum oxide ceramic surface electric conduction and heat conduction composite coating

By using high-pressure cold spraying technology to prepare composite coatings of Al-Al2O3 transition coating and pure Al coating on the surface of alumina ceramics, the problem of insufficient conductivity and thermal conductivity of alumina ceramics is solved, and the problem of mismatch of thermal expansion coefficients is alleviated. , improves the density and mechanical properties of the coating and expands its application areas.

CN118910606AActive Publication Date: 2024-11-08HARBIN INST OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410973186.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The electrical and thermal conductivity of alumina ceramic materials is insufficient, and their thermal expansion coefficient does not match the metal materials, resulting in large stress between the coating and the substrate, limiting its application in aerospace and other fields.

Method used

The Al-Al2O3 transition coating was prepared by spraying mixed powders of aluminum oxide and aluminum on the surface of alumina ceramics by high-pressure cold spraying technology. The powder was evenly distributed through low-energy ball milling, and a pure aluminum coating was deposited on it to form an Al-Al2O3 transition The composite coating of coating and pure Al coating relieves the difference in thermal expansion coefficients and achieves a gradient transition of composition and performance.

Benefits of technology

The thermal conductivity of the surface of alumina ceramics has been improved, the stress between the coating and the substrate is reduced, the density and mechanical properties of the coating are improved, and the application field of alumina ceramics is broadened.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910606A_ABST
    Figure CN118910606A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an aluminum oxide ceramic surface electric-conduction and heat-conduction composite coating. Belongs to the technical field of material surface engineering. In order to solve the problems that the electric conduction and heat conduction performance of the aluminum oxide ceramic is poor and the thermal expansion coefficient of a metal coating prepared on the surface of the aluminum oxide ceramic is not matched, the composite coating with excellent electric conduction and heat conduction performance is prepared on the surface of the aluminum oxide ceramic by using aluminum oxide powder and aluminum powder through low-energy ball milling and high-pressure cold spraying technologies. The preparation method comprises the following steps: mixing aluminum oxide powder and aluminum powder according to a certain ratio, and performing low-energy ball milling to obtain mixed powder; spraying the mixed powder on aluminum oxide ceramic by adopting a high-pressure cold spraying technology to form a transition coating; and pure aluminum powder is sprayed on the transition coating to form the composite coating. The preparation method has the advantages of being high in efficiency, simple and easy to operate and the like, the prepared composite coating can endow the surface of the aluminum oxide ceramic with good electric conductivity and heat conductivity, and the application field of the aluminum oxide ceramic is widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material surface engineering, and in particular relates to a method for preparing an electrically conductive and thermally conductive composite coating on the surface of an alumina ceramic. Background Art

[0002] Alumina ceramics have broad application prospects in many industries such as aerospace, electronic power, chemical industry, etc. due to their high strength, high hardness, excellent high temperature resistance, corrosion resistance and wear resistance. However, the inherent limitations of alumina ceramics, such as poor electrical conductivity, limited thermal conductivity and weak impact resistance, restrict the further application of alumina ceramics. In contrast, metal materials usually have excellent electrical conductivity, thermal conductivity, ductility and excellent machinability. In order to make full use of the advantages of these two materials, a metal coating can be prepared on the surface of alumina ceramics to give the surface of alumina ceramics good electrical conductivity and efficient thermal conductivity. This technology can combine the advantages of ceramics and metals, greatly broaden the application field of alumina ceramics, and promote the further development of materials science.

[0003] Cold spraying is a material surface coating technology based on the principles of aerodynamics. Cold spraying technology uses supersonic airflow to drive the spray powder particles to hit the substrate surface at high speed in a gas-solid bidirectional flow. The particles undergo strong plastic deformation and form a mechanical bond with the substrate, thereby being deposited on the substrate surface to form a coating. Due to the short contact time with the gas, the particle temperature is much lower than the melting point of the particles, and the particles always remain in a solid state. The continuous high-speed impact of the particles may produce a shot peening or "compacting" effect, resulting in the densification of the coating, and its density is close to the theoretical density. The cold spraying process is expected to become a method for efficiently and quickly preparing metal coatings on ceramic surfaces. CN115874173A discloses a cold-sprayed metal coating for improving the anti-multiple-shot performance of ceramic armor and a preparation method thereof. The method uses cold spraying technology to directly deposit an aluminum or copper metal coating on a roughened ceramic surface. CN114075664B discloses a method for preparing a patterned ceramic copper-clad laminate by cold spraying. The method first uses a cold spraying device to spray metal powder onto the surface of a ceramic substrate under certain conditions to form a transition layer, and then sprays high-purity copper powder on the surface of the prepared transition layer to obtain a pure copper coating on the surface of the ceramic substrate. Both methods prepare a metal coating on the ceramic surface, but CN115874173A directly deposits metal powder on the ceramic surface. The thermal expansion coefficients of the two materials differ greatly, and the stress at the interface between the coating and the substrate is relatively large. Although CN114075664B uses a transition layer, the composition of the transition layer is pure metal, binary metal mixture, ternary metal mixture, binary alloy or ternary alloy, which is still quite different from the physical properties of the ceramic substrate. Summary of the invention

[0004] In order to solve the deficiencies of the above-mentioned prior art, the present invention proposes a method for preparing an electrically conductive and thermally conductive composite coating on the surface of an alumina ceramic. A transition coating is prepared by innovatively using high-pressure cold spraying to spray a mixed powder of alumina and aluminum on the surface of the alumina ceramic. The physical properties of the transition coating are similar to those of the alumina ceramic, and the problem of thermal expansion coefficient mismatch between the coating and the substrate can be solved, stress can be alleviated, and a continuous change in composition, structure and performance from the ceramic substrate to the surface metal layer can be achieved.

[0005] The method for preparing the conductive and thermal conductive composite coating on the surface of alumina ceramics of the present invention is carried out according to the following steps:

[0006] Step 1: low-energy ball milling the alumina powder and the aluminum powder using a ball mill to uniformly distribute the alumina powder particles in the aluminum powder to obtain a mixed powder; the mass ratio of the aluminum powder to the alumina powder is (2-4):1;

[0007] The process of low-energy ball milling is as follows: weighed alumina powder and aluminum powder are mixed and loaded into a ball mill, the ball mill is vacuumized, and then an inert gas is introduced; the ball mill adopts a dry milling method, the ball-to-material mass ratio is controlled to be (3-4):1, the ball mill speed is set to 150-200r / min, the ball milling time is set to 2-4h, the ball mill is rotated in one direction during the ball milling, and the ball mill stops rotating for 5-10min after each ball milling for 0.5-1h;

[0008] Step 2: spraying the mixed powder obtained in step 1 onto an alumina ceramic substrate by cold spraying to obtain an Al-Al2O3 transition coating;

[0009] The cold spraying process is as follows: ultrasonically cleaning the alumina ceramic substrate to be sprayed with anhydrous ethanol, placing the alumina ceramic substrate in a drying oven for drying after ultrasonic cleaning, and fixing the alumina ceramic substrate on a fixture after drying; before spraying, loading the mixed powder obtained in step 1 into a powder feeder, using nitrogen as a working gas during spraying, the spraying trajectory is "S" shaped, the spraying trajectory line spacing is 2-3mm, the angle between the spraying beam and the surface to be sprayed is 90°, the spray gun moving speed is 150-200mm / s, the vertical distance between the end of the spray gun and the surface of the alumina ceramic substrate to be sprayed is 40-45mm, the working gas pressure is 5-7Mpa, the working gas temperature is 600-900°C, and the number of spray layers is 1-2 layers;

[0010] Step 3: cold spraying aluminum powder onto the Al-Al2O3 transition coating obtained in step 2 to obtain a composite coating of the Al-Al2O3 transition coating and the pure Al coating;

[0011] The cold spraying process is as follows: aluminum powder is loaded into a powder feeder, and the alumina ceramic substrate with an Al-Al2O3 transition coating deposited on the surface obtained in step 2 is fixed on a fixture; nitrogen is used as the working gas during spraying, the spraying trajectory is "S" shaped, the spraying trajectory line spacing is 2-3mm, the angle between the spraying beam and the surface to be sprayed is 90°, the movement speed of the spray gun is 150-200mm / s, the vertical distance between the end of the spray gun and the surface of the alumina ceramic substrate to be sprayed is 40-45mm, the working gas pressure is 3.5-4.5MPa, the working gas temperature is 550-650℃, and the number of spray layers is 2-6.

[0012] Principle and beneficial effects of the invention:

[0013] 1. The present invention adopts a cold spraying process, which can deposit coatings at a relatively low temperature (in the range of several hundred degrees Celsius) and at a relatively high deposition rate (coating deposition rate can reach millimeters per minute). The temperature during cold spraying is relatively low, which avoids the risk of deformation or damage of the substrate due to high temperature. The mixed powder is less affected by heat, and no phase change occurs during the spraying process, which greatly suppresses the generation of thermal defects in the coating, and the coating has excellent organizational morphology and mechanical properties.

[0014] 2. The present invention adopts a composite coating designed by combining an Al-Al2O3 transition layer and a pure Al coating. The Al-Al2O3 transition coating is used as an intermediate layer, and its physical properties are similar to those of alumina ceramics. It can solve the problem of thermal expansion coefficient mismatch between the coating and the substrate, relieve stress, and achieve a gradient transition from the ceramic substrate to the surface metal layer composition, structure and performance. The pure Al coating is used as the outer surface layer, and its excellent electrical and thermal conductivity can give the alumina ceramic surface good electrical conductivity and efficient thermal conductivity.

[0015] 3. When the present invention sprays the mixed powder containing alumina ceramic particles to prepare the transition coating, the alumina ceramic particles have poor plastic deformation ability and are difficult to deposit. Therefore, the present invention adopts high gas pressure and high gas temperature for deposition when cold spraying the transition coating, wherein the gas pressure reaches 5-7Mpa and the gas temperature is 600-900°C. By adopting high gas pressure and high gas temperature to achieve high-quality deposition of the mixed powder containing alumina ceramic particles, an Al-Al2O3 transition coating is prepared on the surface of alumina ceramic. Higher spraying gas pressure can enable the powder particles to obtain greater kinetic energy in the accelerated airflow, the more significant the bombardment and compaction of the particles, the higher the density of the coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a cross-sectional morphology of the composite coating prepared in step 3 of Example 1;

[0017] Figure 2This is a Vickers hardness transition diagram of the composite coating prepared in step three of Example 1. DETAILED DESCRIPTION

[0018] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any reasonable combination of the specific implementation modes.

[0019] Specific implementation method 1: The preparation method of the conductive and thermal conductive composite coating on the surface of alumina ceramics in this implementation method is carried out according to the following steps:

[0020] Step 1: low-energy ball milling the alumina powder and the aluminum powder using a ball mill to uniformly distribute the alumina powder particles in the aluminum powder to obtain a mixed powder; the mass ratio of the aluminum powder to the alumina powder is (2-4):1;

[0021] The process of low-energy ball milling is as follows: weighed alumina powder and aluminum powder are mixed and loaded into a ball mill, the ball mill is vacuumized, and then an inert gas is introduced; the ball mill adopts a dry milling method, the ball-to-material mass ratio is controlled to be (3-4):1, the ball mill speed is set to 150-200r / min, the ball milling time is set to 2-4h, the ball mill is rotated in one direction during the ball milling, and the ball mill stops rotating for 5-10min after each ball milling for 0.5-1h;

[0022] Step 2: spraying the mixed powder obtained in step 1 onto an alumina ceramic substrate by cold spraying to obtain an Al-Al2O3 transition coating;

[0023] The cold spraying process is as follows: ultrasonically cleaning the alumina ceramic substrate to be sprayed with anhydrous ethanol, placing the alumina ceramic substrate in a drying oven for drying after ultrasonic cleaning, and fixing the alumina ceramic substrate on a fixture after drying; before spraying, loading the mixed powder obtained in step 1 into a powder feeder, using nitrogen as a working gas during spraying, the spraying trajectory is "S" shaped, the spraying trajectory line spacing is 2-3mm, the angle between the spraying beam and the surface to be sprayed is 90°, the spray gun moving speed is 150-200mm / s, the vertical distance between the end of the spray gun and the surface of the alumina ceramic substrate to be sprayed is 40-45mm, the working gas pressure is 5-7Mpa, the working gas temperature is 600-900°C, and the number of spray layers is 1-2 layers;

[0024] Step 3: cold spraying aluminum powder onto the Al-Al2O3 transition coating obtained in step 2 to obtain a composite coating of the Al-Al2O3 transition coating and the pure Al coating;

[0025] The cold spraying process is as follows: aluminum powder is loaded into a powder feeder, and the alumina ceramic substrate with an Al-Al2O3 transition coating deposited on the surface obtained in step 2 is fixed on a fixture; nitrogen is used as the working gas during spraying, the spraying trajectory is "S" shaped, the spraying trajectory line spacing is 2-3mm, the angle between the spraying beam and the surface to be sprayed is 90°, the movement speed of the spray gun is 150-200mm / s, the vertical distance between the end of the spray gun and the surface of the alumina ceramic substrate to be sprayed is 40-45mm, the working gas pressure is 3.5-4.5MPa, the working gas temperature is 550-650℃, and the number of spray layers is 2-6.

[0026] 1. This embodiment adopts a cold spraying process, which can deposit coatings at a relatively low temperature (in the range of several hundred degrees Celsius) and at a relatively high deposition rate (coating deposition rate can reach millimeters per minute). The temperature during cold spraying is relatively low, which avoids the risk of deformation or damage of the substrate due to high temperature. The mixed powder is less affected by heat, and no phase change occurs during the spraying process, which greatly suppresses the generation of thermal defects in the coating, and the coating has excellent microstructure and mechanical properties.

[0027] 2. This embodiment adopts a composite coating designed by combining an Al-Al2O3 transition layer and a pure Al coating. The Al-Al2O3 transition coating is used as an intermediate layer. Its physical properties are similar to those of alumina ceramics. It can solve the problem of thermal expansion coefficient mismatch between the coating and the substrate, relieve stress, and achieve a gradient transition from the ceramic substrate to the surface metal layer composition, structure and performance. The pure Al coating is used as the outer surface layer. Its excellent electrical and thermal conductivity can give the alumina ceramic surface good electrical conductivity and efficient thermal conductivity.

[0028] 3. In this embodiment, when the mixed powder containing alumina ceramic particles is sprayed to prepare the transition coating, the alumina ceramic particles have poor plastic deformation ability and are difficult to deposit. Therefore, the present invention adopts high gas pressure and high gas temperature for deposition when cold spraying the transition coating, wherein the gas pressure reaches 5-7Mpa and the gas temperature is 600-900°C. By adopting high gas pressure and high gas temperature to achieve high-quality deposition of the mixed powder containing alumina ceramic particles, an Al-Al2O3 transition coating is prepared on the surface of the alumina ceramic. Higher spraying gas pressure can enable the powder particles to obtain greater kinetic energy in the accelerated airflow, the more significant the bombardment and compaction of the particles, the higher the density of the coating.

[0029] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that: the purity of the aluminum powder in step 1 is 99.9%, the particles are spherical, and the particle size is 20-35 μm.

[0030] Specific implementation method three: This implementation method is different from specific implementation methods one or two in that: the purity of the aluminum oxide powder in step one is 99.9%, the particles are irregular in shape, and the particle size is 20-60 μm.

[0031] Specific implementation method 4: This implementation method is different from any one of specific implementation methods 1 to 3 in that: the ball mill described in step 1 is a planetary ball mill.

[0032] Specific implementation mode 5: This implementation mode is different from any one of specific implementation modes 1 to 4 in that: the inert gas in step 1 is argon.

[0033] Specific embodiment six: This embodiment differs from any one of specific embodiments one to five in that: the process of low-energy ball milling is: the weighed alumina powder and aluminum powder are mixed and loaded into a ball mill, the ball mill is vacuumed, and then argon gas is introduced; the ball milling process adopts dry grinding, the ball-to-material mass ratio is controlled to 3:1, the ball mill speed is set to 200r / min, the ball milling time is set to 2h, the ball mill is rotated in one direction during the ball milling, and the ball mill stops rotating for 5min after each 0.5h of ball milling.

[0034] Specific implementation method seven: This implementation method is different from any one of specific implementation methods one to six in that: the ultrasonic cleaning time in step two is 10-30 minutes, the ultrasonic frequency is 20-80KHz, the drying temperature is 50-80°C, and the drying time is 10-30 minutes.

[0035] Specific embodiment eight: This embodiment differs from any one of specific embodiments one to seven in that: the cold spraying process described in step two includes the following steps: ultrasonically cleaning the alumina ceramic substrate to be sprayed with anhydrous ethanol, placing the alumina ceramic substrate in a drying oven for drying after ultrasonic cleaning, and fixing the alumina ceramic substrate on a fixture after drying; before spraying, loading the mixed powder obtained in step one into a powder feeder, using nitrogen as the working gas during spraying, the spraying trajectory is "S" shaped, the spraying trajectory line spacing is 2mm, the angle between the spray beam and the surface to be sprayed is 90°, the spray gun moving speed is 200mm / s, the vertical distance between the end of the spray gun and the surface of the alumina ceramic substrate to be sprayed is 40mm, the working gas pressure is 5Mpa, the working gas temperature is 650℃, and the number of spray layers is 2.

[0036] Specific implementation method 9: This implementation method is different from specific implementation methods 1 to 8 in that: the purity of the aluminum powder in step 3 is 99.9%, the particles are spherical, and the particle size is 20-35 μm.

[0037] Specific embodiment ten: This embodiment differs from any one of specific embodiments one to nine in that: the cold spraying process described in step three includes the following steps: loading aluminum powder into a powder feeder, fixing the alumina ceramic substrate with an Al-Al2O3 transition coating deposited on the surface obtained in step two on a fixture; using nitrogen as the working gas during spraying, the spraying trajectory is "S" shaped, the spraying trajectory line spacing is 2mm, the angle between the spray beam and the surface to be sprayed is 90°, the spray gun moving speed is 200mm / s, the vertical distance between the end of the spray gun and the surface of the alumina ceramic substrate to be sprayed is 40mm, the working gas pressure is 4MPa, the working gas temperature is 600℃, and the number of spray layers is 4.

[0038] Embodiment 1:

[0039] The preparation method of the conductive and thermal conductive composite coating on the surface of alumina ceramics in this embodiment is carried out according to the following steps:

[0040] Step 1: low-energy ball milling the alumina powder and the aluminum powder using a ball mill to uniformly distribute the alumina powder particles in the aluminum powder to obtain a mixed powder; the mass ratio of the aluminum powder to the alumina powder is 4:1;

[0041] The process of low-energy ball milling is as follows: weighed alumina powder and aluminum powder are mixed and loaded into a ball mill, the ball mill is vacuumized, and then an inert gas is introduced; the ball mill adopts a dry milling method, the ball-to-material mass ratio is controlled to be 3:1, the ball mill speed is set to 200r / min, the ball milling time is set to 2h, the ball mill is rotated in one direction during the ball milling, and the ball mill stops rotating for 5min after each ball milling of 0.5;

[0042] The aluminum powder has a purity of 99.9%, spherical particles, and a particle size of 20-35 μm;

[0043] The purity of the aluminum oxide powder is 99.9%, the particles are irregular in shape, and the particle size is 20-60 μm;

[0044] The ball mill is a planetary ball mill;

[0045] The inert gas is argon;

[0046] Step 2: spraying the mixed powder obtained in step 1 onto an alumina ceramic substrate by cold spraying to obtain an Al-Al2O3 transition coating;

[0047] The cold spraying process is as follows: the alumina ceramic substrate to be sprayed is ultrasonically cleaned with anhydrous ethanol for 30 minutes, the ultrasonic frequency is 50KHz, the alumina ceramic substrate is placed in a drying oven for drying for 30 minutes after ultrasonic cleaning, the drying temperature is 70°C, and the alumina ceramic substrate is fixed on a fixture after drying; before spraying, the mixed powder obtained in step 1 is loaded into a powder feeder, nitrogen is used as the working gas during spraying, the spraying trajectory is "S" shaped, the spraying trajectory line spacing is 2mm, the spraying beam and the surface to be sprayed The angle is 90°, the spray gun moving speed is 200mm / s, the vertical distance between the end of the spray gun and the surface of the alumina ceramic substrate to be sprayed is 40mm, the working gas pressure is 5Mpa, the working gas temperature is 650°C, and the number of spray layers is 2 layers;

[0048] Step 3: cold spraying aluminum powder onto the Al-Al2O3 transition coating obtained in step 2 to obtain a composite coating of the Al-Al2O3 transition coating and the pure Al coating;

[0049] The cold spraying process is as follows: aluminum powder is loaded into a powder feeder, and the alumina ceramic substrate with the Al-Al2O3 transition coating deposited on the surface obtained in step 2 is fixed on a fixture; nitrogen is used as the working gas during spraying, the spraying trajectory is "S" shaped, the spraying trajectory line spacing is 2mm, the angle between the spraying beam and the surface to be sprayed is 90°, the spray gun moving speed is 200mm / s, the vertical distance between the end of the spray gun and the surface of the alumina ceramic substrate to be sprayed is 40mm, the working gas pressure is 4.5MPa, the working gas temperature is 600℃, and the number of spray layers is 4;

[0050] The purity of the aluminum powder is 99.9%, the particles are spherical, and the particle size is 20-35 μm.

[0051] The thermal diffusion coefficient of the composite coating of Al-Al2O3 transition coating and pure Al coating obtained in this example is 70.951 mm 2 / s, and the thermal conductivity is 149.462W / (m·K). The Hall coefficient of the composite coating is 31.67×10 3 cm 3 / C, the Hall mobility is 2.61cm 3 / V·s, the resistance value is 6.89Ω, and the conductivity is 203.60×10 3 S / cm. The porosity of the composite coating is 0.55%.

[0052] Figure 1This is a cross-sectional morphology of the composite coating prepared in step 3 of Example 1. As can be seen from the figure, there is no obvious boundary between the Al-Al2O3 transition coating prepared on the surface of the alumina ceramic substrate by cold spraying technology and the pure Al coating, the Al2O3 particles are evenly distributed in the Al-Al2O3 transition coating, the internal interface of the composite coating is well bonded, the coating is dense, and there are no obvious pores and cracks. Figure 2 The Vickers hardness transition change diagram of the composite coating prepared in step 3 of Example 1. As can be seen from the figure, the coating hardness measured at points taken in sequence along the direction perpendicular to the Al2O3 ceramic substrate from the interface between the ceramic substrate and the composite coating to the surface of the composite coating changes relatively slowly, which indicates that the Al-Al2O3 transition coating prepared on the surface of the alumina ceramic substrate by cold spraying technology realizes a continuous change in hardness performance from the ceramic substrate to the surface metal layer.

[0053] Embodiment 2:

[0054] The preparation method of the conductive and thermal conductive composite coating on the surface of alumina ceramics in this embodiment is carried out according to the following steps:

[0055] Step 1: low-energy ball milling the alumina powder and the aluminum powder using a ball mill to uniformly distribute the alumina powder particles in the aluminum powder to obtain a mixed powder; the mass ratio of the aluminum powder to the alumina powder is 4:1;

[0056] The process of low-energy ball milling is as follows: weighed alumina powder and aluminum powder are mixed and loaded into a ball mill, the ball mill is vacuumized, and then an inert gas is introduced; the ball mill adopts a dry milling method, the ball-to-material mass ratio is controlled to be 3:1, the ball mill speed is set to 200r / min, the ball milling time is set to 2h, the ball mill is rotated in one direction during the ball milling, and the ball mill stops rotating for 5min after each ball milling for 0.5h;

[0057] The aluminum powder has a purity of 99.9%, spherical particles, and a particle size of 20-35 μm;

[0058] The purity of the aluminum oxide powder is 99.9%, the particles are irregular in shape, and the particle size is 20-60 μm;

[0059] The ball mill is a planetary ball mill;

[0060] The inert gas is argon;

[0061] Step 2: spraying the mixed powder obtained in step 1 onto an alumina ceramic substrate by cold spraying to obtain an Al-Al2O3 transition coating;

[0062] The cold spraying process is as follows: the alumina ceramic substrate to be sprayed is ultrasonically cleaned with anhydrous ethanol for 20 minutes, the ultrasonic frequency is 50KHz, the alumina ceramic substrate is placed in a drying oven for drying for 10 minutes after ultrasonic cleaning, the drying temperature is 70°C, and the alumina ceramic substrate is fixed on a fixture after drying; before spraying, the mixed powder obtained in step 1 is loaded into a powder feeder, nitrogen is used as the working gas during spraying, the spraying trajectory is "S" shaped, the spraying trajectory line spacing is 2mm, the spraying beam and the surface to be sprayed The angle is 90°, the spray gun moving speed is 200mm / s, the vertical distance between the end of the spray gun and the surface of the alumina ceramic substrate to be sprayed is 40mm, the working gas pressure is 5Mpa, the working gas temperature is 650°C, and the number of spray layers is 2 layers;

[0063] Step 3: cold spraying aluminum powder onto the Al-Al2O3 transition coating obtained in step 2 to obtain a composite coating of the Al-Al2O3 transition coating and the pure Al coating;

[0064] The cold spraying process is as follows: aluminum powder is loaded into a powder feeder, and the alumina ceramic substrate with the Al-Al2O3 transition coating deposited on the surface obtained in step 2 is fixed on a fixture; nitrogen is used as the working gas during spraying, the spraying trajectory is "S" shaped, the spraying trajectory line spacing is 2mm, the angle between the spraying beam and the surface to be sprayed is 90°, the spray gun moving speed is 200mm / s, the vertical distance between the end of the spray gun and the surface of the alumina ceramic substrate to be sprayed is 40mm, the working gas pressure is 4MPa, the working gas temperature is 600℃, and the number of spray layers is 4;

[0065] The purity of the aluminum powder is 99.9%, the particles are spherical, and the particle size is 20-35 μm.

[0066] The thermal diffusion coefficient of the composite coating of Al-Al2O3 transition coating and pure Al coating obtained in this example is 61.532 mm 2 / s, and the thermal conductivity is 131.654W / (m·K). The Hall coefficient of the composite coating is 25.12×10 3 cm 3 / C, the Hall mobility is 1.83cm 3 / V·s, the resistance value is 7.22Ω, and the conductivity is 153.30×10 3 S / cm. The porosity of the composite coating is 0.87%.

[0067] Embodiment 3:

[0068] The preparation method of the conductive and thermal conductive composite coating on the surface of alumina ceramics in this embodiment is carried out according to the following steps:

[0069] Step 1: low-energy ball milling the alumina powder and the aluminum powder using a ball mill to uniformly distribute the alumina powder particles in the aluminum powder to obtain a mixed powder; the mass ratio of the aluminum powder to the alumina powder is 4:1;

[0070] The process of low-energy ball milling is as follows: weighed alumina powder and aluminum powder are mixed and loaded into a ball mill, the ball mill is vacuumized, and then an inert gas is introduced; the ball mill adopts a dry milling method, the ball-to-material mass ratio is controlled to be 3:1, the ball mill speed is set to 200r / min, the ball milling time is set to 2h, the ball mill is rotated in one direction during the ball milling, and the ball mill stops rotating for 5min after each ball milling for 0.5h;

[0071] The aluminum powder has a purity of 99.9%, spherical particles, and a particle size of 20-35 μm;

[0072] The purity of the aluminum oxide powder is 99.9%, the particles are irregular in shape, and the particle size is 20-60 μm;

[0073] The ball mill is a planetary ball mill;

[0074] The inert gas is argon;

[0075] Step 2: spraying the mixed powder obtained in step 1 onto an alumina ceramic substrate by cold spraying to obtain an Al-Al2O3 transition coating;

[0076] The cold spraying process is as follows: the alumina ceramic substrate to be sprayed is ultrasonically cleaned with anhydrous ethanol for 30 minutes, the ultrasonic frequency is 50KHz, the alumina ceramic substrate is placed in a drying oven for drying for 10 minutes after ultrasonic cleaning, the drying temperature is 70°C, and the alumina ceramic substrate is fixed on a fixture after drying; before spraying, the mixed powder obtained in step 1 is loaded into a powder feeder, nitrogen is used as the working gas during spraying, the spraying trajectory is "S" shaped, the spraying trajectory line spacing is 2mm, the spraying beam and the surface to be sprayed The angle is 90°, the spray gun moving speed is 200mm / s, the vertical distance between the end of the spray gun and the surface of the alumina ceramic substrate to be sprayed is 40mm, the working gas pressure is 5Mpa, the working gas temperature is 650°C, and the number of spray layers is 2;

[0077] Step 3: cold spraying aluminum powder onto the Al-Al2O3 transition coating obtained in step 2 to obtain a composite coating of the Al-Al2O3 transition coating and the pure Al coating;

[0078] The cold spraying process is as follows: aluminum powder is loaded into a powder feeder, and the alumina ceramic substrate with an Al-Al2O3 transition coating deposited on the surface obtained in step 2 is fixed on a fixture; nitrogen is used as the working gas during spraying, the spraying trajectory is "S" shaped, the spraying trajectory line spacing is 2mm, the angle between the spraying beam and the surface to be sprayed is 90°, the spray gun moving speed is 200mm / s, the vertical distance between the end of the spray gun and the surface of the alumina ceramic substrate to be sprayed is 40mm, the working gas pressure is 3.5MPa, the working gas temperature is 600℃, and the number of spray layers is 4.

[0079] The aluminum powder has a purity of 99.9%, spherical particles, and a particle size of 20-35 μm;

[0080] The thermal diffusion coefficient of the composite coating of Al-Al2O3 transition coating and pure Al coating obtained in this example is 52.698 mm 2 / s, and the thermal conductivity is 114.154W / (m·K). The Hall coefficient of the composite coating is 15.33×10 3 cm 3 / C, the Hall mobility is 1.02cm 3 / V·s, the resistance value is 7.37Ω, and the conductivity is 120.20×10 3 S / cm. The porosity of the composite coating is 1.32%.

Claims

1. A method for preparing an electrically conductive and thermally conductive composite coating on the surface of an alumina ceramic, characterized in that: The preparation method of the conductive and thermal conductive composite coating on the surface of alumina ceramic is carried out according to the following steps: Step 1: low-energy ball milling the alumina powder and the aluminum powder using a ball mill to uniformly distribute the alumina powder particles in the aluminum powder to obtain a mixed powder; the mass ratio of the aluminum powder to the alumina powder is (2-4):1; The process of low-energy ball milling is as follows: weighed alumina powder and aluminum powder are mixed and loaded into a ball mill, the ball mill is vacuumized, and then an inert gas is introduced; the ball mill adopts a dry milling method, the ball-to-material mass ratio is controlled to be (3-4):1, the ball mill speed is set to 150-200r / min, the ball milling time is set to 2-4h, the ball mill is rotated in one direction during the ball milling, and the ball mill stops rotating for 5-10min after each ball milling for 0.5-1h; Step 2: spraying the mixed powder obtained in step 1 onto an alumina ceramic substrate by cold spraying to obtain an Al-Al2O3 transition coating; The cold spraying process is as follows: ultrasonically cleaning the alumina ceramic substrate to be sprayed with anhydrous ethanol, placing the alumina ceramic substrate in a drying oven for drying after ultrasonic cleaning, and fixing the alumina ceramic substrate on a fixture after drying; before spraying, loading the mixed powder obtained in step 1 into a powder feeder, using nitrogen as a working gas during spraying, the spraying trajectory is "S" shaped, the spraying trajectory line spacing is 2-3mm, the angle between the spraying beam and the surface to be sprayed is 90°, the spray gun moving speed is 150-200mm / s, the vertical distance between the end of the spray gun and the surface of the alumina ceramic substrate to be sprayed is 40-45mm, the working gas pressure is 5-7Mpa, the working gas temperature is 600-900℃, and the number of spray layers is 1-2 layers; Step 3: cold spraying aluminum powder onto the Al-Al2O3 transition coating obtained in step 2 to obtain a composite coating of the Al-Al2O3 transition coating and the pure Al coating; The cold spraying process is as follows: aluminum powder is loaded into a powder feeder, and the alumina ceramic substrate with an Al-Al2O3 transition coating deposited on the surface obtained in step 2 is fixed on a fixture; nitrogen is used as a working gas during spraying, the spraying trajectory is "S" shaped, the spraying trajectory line spacing is 2-3mm, the angle between the spraying beam and the surface to be sprayed is 90°, the movement speed of the spray gun is 150-200mm / s, the vertical distance between the end of the spray gun and the surface of the alumina ceramic substrate to be sprayed is 40-45mm, the working gas pressure is 3.5-4.5MPa, the working gas temperature is 550-650℃, and the number of spray layers is 2-6.

2. The method for preparing the conductive and thermal conductive composite coating on the surface of alumina ceramics according to claim 1, characterized in that: The purity of the aluminum powder in step 1 is 99.9%, the particles are spherical, and the particle size is 20-35 μm.

3. The method for preparing the conductive and thermal conductive composite coating on the surface of alumina ceramics according to claim 1, characterized in that: The purity of the aluminum oxide powder in step 1 is 99.9%, the particles are irregular in shape, and the particle size is 20-60 μm.

4. The method for preparing the conductive and thermal conductive composite coating on the surface of alumina ceramics according to claim 1, characterized in that: The ball mill in step 1 is a planetary ball mill.

5. The method for preparing the conductive and thermal conductive composite coating on the surface of alumina ceramics according to claim 1, characterized in that: The inert gas in step 1 is argon.

6. The method for preparing the conductive and thermal conductive composite coating on the surface of alumina ceramics according to claim 1, characterized in that: The process of low-energy ball milling is as follows: weighed alumina powder and aluminum powder are mixed and loaded into a ball mill, the ball mill is vacuumed, and then argon gas is introduced; the ball mill adopts dry milling, the ball-to-material mass ratio is controlled to be 3:1, the ball mill speed is set to 200r / min, the ball mill time is set to 2h, the ball mill is rotated in one direction during the ball milling, and the ball mill stops rotating for 5min after each ball milling for 0.5h.

7. The method for preparing the conductive and thermal conductive composite coating on the surface of alumina ceramics according to claim 1, characterized in that: The ultrasonic cleaning time in step 2 is 10-30 minutes, the ultrasonic frequency is 20-80KHz, the drying temperature is 50-80°C, and the drying time is 10-30 minutes.

8. The method for preparing the conductive and thermal conductive composite coating on the surface of alumina ceramics according to claim 1, characterized in that: The cold spraying process in step 2 includes the following steps: ultrasonically cleaning the alumina ceramic substrate to be sprayed with anhydrous ethanol, placing the alumina ceramic substrate in a drying oven for drying after ultrasonic cleaning, and fixing the alumina ceramic substrate on a fixture after drying; before spraying, loading the mixed powder obtained in step 1 into a powder feeder, using nitrogen as the working gas during spraying, the spraying trajectory is "S" shaped, the spraying trajectory line spacing is 2mm, the angle between the spray beam and the surface to be sprayed is 90°, the spray gun moving speed is 200mm / s, the vertical distance between the end of the spray gun and the surface of the alumina ceramic substrate to be sprayed is 40mm, the working gas pressure is 5Mpa, the working gas temperature is 650℃, and the number of spray layers is 2.

9. The method for preparing the conductive and thermal conductive composite coating on the surface of alumina ceramics according to claim 1, characterized in that: The purity of the aluminum powder in step 3 is 99.9%, the particles are spherical, and the particle size is 20-35 μm.

10. The method for preparing the conductive and thermal conductive composite coating on the surface of alumina ceramics according to claim 1, characterized in that: The cold spraying process in step 3 includes the following steps: loading aluminum powder into a powder feeder, fixing the alumina ceramic substrate with an Al-Al2O3 transition coating deposited on the surface obtained in step 2 on a fixture; using nitrogen as the working gas during spraying, the spraying trajectory is "S" shaped, the spraying trajectory line spacing is 2mm, the angle between the spray beam and the surface to be sprayed is 90°, the spray gun moving speed is 200mm / s, the vertical distance between the end of the spray gun and the surface of the alumina ceramic substrate to be sprayed is 40mm, the working gas pressure is 4MPa, the working gas temperature is 600℃, and the number of spray layers is 4.

Citation Information

Patent Citations

  • Cold spraying aluminum-based self-lubrication abrasion-resistant coating and preparation method thereof

    CN105525287A

  • Aluminum oxide ceramic coating and preparation method thereof

    CN109440051A

  • Preparation method of stainless steel surface coating with excellent wear resistance and corrosion resistance

    CN111172537A

  • Method for improving corrosion resistance through cold spraying of double-layer coating

    CN114182249A