Method for co-production of combustible gas-biochar and nano carbon material by electrochemical cracking of biomass with molten salt
By performing thermoelectrochemical coupling conversion of biomass in a molten salt electrochemical environment, using the anodization effect and the capture ability of molten salt medium, the problems of high energy consumption, low product quality and secondary emissions in the thermal conversion of biomass are solved. , realizes efficient production of biochar and nanocarbon materials.
Patent Information
- Application Number
- CN202410976010.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
In the biomass thermal conversion process, there are problems such as high energy consumption, low product quality, serious secondary emissions such as carbon dioxide and easy carbon deposition and deactivation of catalysts.
Modified salt electrochemical method is adopted to conduct thermoelectrochemical coupling conversion of biomass in molten salt electrolytes, and to improve the pore structure and combustible gas quality of biochar using the anodized effect, and capture carbon dioxide through molten salt medium to avoid secondary emissions and generate Nanocarbon material.
It improves the quality of the thermoelectrochemical conversion products of biomass, enhances the functionality of biochar, reduces production costs, and avoids the emission of carbon dioxide and other pollutants, solving the problem of catalyst carbon deposition and inactivation.
Smart Images

Figure CN118910625A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of biomass energy production, and in particular to a method for molten salt electrochemical cracking of biomass to co-produce combustible gas-biochar and nano-carbon materials. Background Art
[0002] Biomass thermal conversion can convert biomass (including wood, agricultural and forestry waste, microalgae, municipal sludge, etc.) into fuels, biochar, chemicals and other useful products through thermochemical processes. Biomass thermal conversion aims to reduce dependence on fossil fuels, reduce carbon dioxide emissions, and promote the use of renewable energy. Among them, biomass gasification and biomass carbonization can obtain combustible gases and biochar to achieve resource recycling. Biomass gasification is the process of decomposing biomass into combustible gases (such as carbon monoxide, hydrogen, methane and carbon dioxide) and ash at high temperatures (usually over 700°C). Biomass carbonization is the process of decomposing biomass into solid carbon and gas at high temperatures (300-800°C). Biochar is widely used in agriculture, soil improvement and environmental governance.
[0003] However, biomass thermal conversion also faces bottleneck problems, the most important of which are high conversion costs and low product value. For example, the quality of the gas produced during biomass gasification is often low and contains more impurities and harmful substances. This limits the use of gas in high-end applications (such as power generation, chemical raw materials, etc.). The pore structure of biochar produced by biomass carbonization is underdeveloped and its functionality is poor. The use of catalysts can effectively enhance the quality of biomass thermal conversion products, but the high-temperature conversion process can easily lead to catalyst sintering and carbon deposition deactivation. In addition, due to the complex composition of biomass and the presence of multiple elements, carbon dioxide, sulfur oxides, and nitrogen oxides are inevitably emitted during the thermal conversion process. These secondary emissions seriously affect the clean production of the conversion process and the realization of carbon neutrality goals. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the present invention provides a method for molten salt electrochemical cracking of biomass to co-produce combustible gas - biochar and nano-carbon materials, which effectively solves the problems of high energy consumption, low product quality, serious secondary emissions such as carbon dioxide, and easy carbon accumulation and deactivation of catalysts in the existing biomass thermal conversion process.
[0005] To achieve the above-mentioned purpose, the technical solution adopted by the present invention to solve the technical problem is: to provide a method for co-producing combustible gas-biochar and nano-carbon materials by electrochemical cracking of biomass by molten salt, comprising the following steps:
[0006] S1. Heating the salt containing oxygen ions until it is completely melted to obtain a molten salt electrolyte;
[0007] S2. The biomass is dried and fixed on the anode surface in a two-electrode system, and then the cathode and anode are placed below the molten salt electrolyte liquid level for electrolysis, whereby combustible gas and biochar are obtained at the anode and nanocarbon materials are obtained at the cathode.
[0008] Furthermore, in step S1, oxygen ions are derived from the added metal oxide or the molten salt electrolyte itself being ionized at high temperature.
[0009] Furthermore, the oxide is at least one of lithium oxide, sodium oxide, potassium oxide and calcium oxide.
[0010] The beneficial effect of adopting the above further scheme is that the added metal oxide and the molten salt electrolyte under high temperature ionization provide oxygen ions together.
[0011] Furthermore, the salt is a carbonate salt or a chloride salt.
[0012] Furthermore, the carbonate is at least one of lithium carbonate, sodium carbonate, potassium carbonate and calcium carbonate.
[0013] Furthermore, the chloride salt is at least one of lithium chloride, sodium chloride, potassium chloride and calcium chloride.
[0014] Furthermore, the molten salt electrolyte is a mixed salt of carbonates of lithium carbonate, sodium carbonate and potassium carbonate.
[0015] Furthermore, the molar ratio of lithium carbonate, sodium carbonate and potassium carbonate is 43.5:31.5:25.
[0016] Further, the temperature is first increased to 250-350°C at 3-8°C / min and kept at this temperature for 20-30h, and then increased to 400-1000°C at 5-15°C / min and kept at this temperature for 25-35min.
[0017] Further, the temperature was first increased to 300°C at 5°C / min and kept at this temperature for 24h, and then increased to 400-1000°C at 10°C / min and kept at this temperature for 30min.
[0018] Furthermore, in step S2, the biomass is one of agricultural and forestry waste, kitchen waste, livestock and poultry manure and microalgae.
[0019] Further, the biomass is dried at 60-100°C to a moisture content of 5-10%.
[0020] Furthermore, the biomass is fixed on the anode surface via the metal foam.
[0021] Furthermore, the foam metal is one of foamed nickel, foamed nickel alloy, foamed aluminum, foamed aluminum alloy, foamed copper and foamed copper alloy.
[0022] Furthermore, in the two-electrode system, the anode electrode material is one of gold, silver, platinum, nickel, copper, nickel-iron alloy, nickel-iron-copper alloy, ruthenium dioxide, nickel-doped yttria-stabilized zirconia, cobalt-doped yttria-stabilized zirconia, copper-doped gadolinium-doped cerium oxide, ruthenium-doped gadolinium-doped cerium oxide, lanthanum strontium manganese oxide and graphite.
[0023] Furthermore, the cathode electrode material is one of gold, silver, platinum, nickel, copper, molybdenum, nickel-iron alloy, nickel-iron-copper alloy and graphite.
[0024] Furthermore, the structure of the anode electrode material and the cathode electrode material is a sheet structure or a mesh structure.
[0025] Furthermore, electrolysis is performed in a constant cell voltage or constant current manner.
[0026] Furthermore, the constant cell voltage is 1.5-5V, and the constant current is 0.05-2A.
[0027] In summary, the present invention has the following beneficial effects:
[0028] 1. The present invention is the first to transform biomass materials by simultaneously coupling thermochemistry and electrochemistry in a molten salt electrolyte environment, and the biomass undergoes thermochemical and electrochemical reactions simultaneously. The catalytic ability of the molten salt medium and the anodic oxidation potential are used to improve the quality of the gas-phase products of the thermo-electrochemical coupled transformation of biomass; at the same time, with the help of the anodic oxidation effect, the carbon element in the biochar is converted in situ, and the solid carbon is converted into hydrocarbons or carbon dioxide, enriching the pore structure of the biochar and enhancing the functionality of the biochar. The anodic oxidation effect can also cleverly eliminate carbon deposits on the biomass conversion interface, which is beneficial to the continuous renewal and long-term stability of the biomass conversion interface, that is, the three-phase reaction interface composed of electrode-biomass-molten salt.
[0029] 2. The present invention also utilizes the ability of molten salt to capture and convert pollutants in situ, captures the carbon dioxide generated in the thermal conversion process in situ as carbonate ions, and then fixes it in the form of nano solid carbon through an electrochemical reduction process, thereby avoiding the emission of carbon dioxide. The composition structure of the obtained nanocarbon material can be regulated, and structures such as carbon nanotubes, carbon nanowires, and graphite sheets can be obtained by regulating the electrode material, which often have high added value and can reduce the cost of the entire production process. The dissolution capacity of molten salt is used to eliminate secondary pollution emissions such as sulfur oxides and nitrogen oxides.
[0030] 3. The method provided by the present invention uses a molten salt rich in oxygen ions as an electrolyte. With the help of the catalytic ability of the molten salt, the biomass undergoes a thermo-electrochemical coupling reaction on the anode to convert it into biochar, combustible gas, carbon dioxide, sulfur oxides, nitrogen oxides, etc. The electrochemical oxidation of the anode can consume part of the carbon element in the biochar and enhance the porosity of the biochar. Subsequently, with the help of the efficient dissolution capacity of the molten salt medium, the generated carbon dioxide, sulfur oxides, and nitrogen oxides are captured in situ by the oxygen ions in the electrolyte to form carbonate ions, sulfate ions, and nitrate ions, eliminating secondary pollution emissions. Carbonates can further be electrochemically reduced to solid nanocarbon materials at the cathode, and oxygen ions are released to ensure the stability of the molten salt electrolyte components. This method cleverly utilizes the ability of the molten salt electrolyte containing oxygen ions to catalyze thermal conversion and capture carbon dioxide, and electrochemically cracks the biomass into biochar and combustible gas at the anode, and nanocarbon materials produced at the cathode. The oxidation of the anode and the liquid phase environment of the molten salt eliminate the risk of carbon deposition at the interface, enhance the porosity of the biochar, and avoid secondary emissions throughout the process. It effectively solves the shortcomings of existing biomass thermal conversion processes, such as high energy consumption, low product quality, serious secondary emissions such as carbon dioxide, and easy carbon deposition and deactivation of catalysts. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 is a current curve diagram of anode constant tank pressure electrolysis in Example 1;
[0032] Figure 2 The graph of the concentration change of gas products corresponding to the constant tank pressure electrolysis in Example 1;
[0033] Figure 3 This is a scanning electron microscope image of the nanocarbon product on the cathode of constant-tank pressure electrolysis in Example 1;
[0034] Figure 4 This is a comparison chart of nitrogen adsorption-desorption curves of the bamboo biochar obtained in Example 1 and the bamboo biochar obtained by pyrolysis under a conventional nitrogen atmosphere. DETAILED DESCRIPTION
[0035] The principles and features of the present invention are described below, and the examples are only used to explain the present invention and are not used to limit the scope of the present invention. If no specific conditions are specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.
[0036] Example 1
[0037] The method for co-producing combustible gas-biochar and nano-carbon materials by electrochemical cracking of biomass with molten salt comprises the following steps:
[0038] S1. Take 200 g of lithium carbonate, sodium carbonate and potassium carbonate in total, wherein the molar ratio of lithium carbonate, sodium carbonate and potassium carbonate is 43.5:31.5:25, add 4 g of lithium oxide to increase the oxygen ion content in the molten salt, mix well and put into a corundum crucible and place in a tubular electric furnace, heat to 300 ° C at a heating rate of 5 ° C / min and keep warm for 24 hours to remove moisture from the salt, then heat to 500 ° C at a heating rate of 10 ° C / min and keep warm for 30 minutes until the salt is completely melted to obtain a molten salt electrolyte;
[0039] S2. Select metallic nickel with a flaky structure as the anode material and metallic nickel with a flaky structure as the cathode material. Crush 20g of bamboo and dry it to a moisture content of 5%. Then fix the dried bamboo on the surface of the anode with a nickel foam sheet. Place the cathode and anode below the liquid level of the molten salt electrolyte. Connect the two electrodes to a potentiostat. Set the constant cell pressure electrolysis parameter of the potentiostat to 2.0V. Obtain combustible gas and biochar at the anode and obtain nanocarbon material at the cathode.
[0040] Example 2
[0041] The method for co-producing combustible gas-biochar and nano-carbon materials by electrochemical cracking of biomass with molten salt comprises the following steps:
[0042] S1. Take 200g of sodium chloride and calcium chloride in a mass ratio of 1:1, add 4g of calcium oxide to increase the oxygen ion content in the molten salt, mix well, put into a corundum crucible and place in a tubular electric furnace, heat to 300°C at a heating rate of 5°C / min and keep warm for 24h to remove moisture from the salt, then heat to 800°C at a heating rate of 10°C / min and keep warm for 30min until the salt is completely melted to obtain a molten salt electrolyte;
[0043] S2. Select flaky nickel-doped yttria-stabilized zirconia as the anode material, select flaky metal nickel as the cathode material, dry 20 g of Chlorella to a moisture content of 5%, then press the dried Chlorella powder into tablets and fix them on the anode surface through a nickel foam sheet, then place the cathode and anode below the molten salt electrolyte level, connect the two electrodes to a constant current meter, set the current electrolysis parameter of the constant current meter to 1A, obtain combustible gas and biochar at the anode, and obtain nanocarbon material at the cathode.
[0044] Example 3
[0045] The method for co-producing combustible gas-biochar and nano-carbon materials by electrochemical cracking of biomass with molten salt comprises the following steps:
[0046] S1. Take 200 g of lithium carbonate, sodium carbonate and potassium carbonate in total, wherein the molar ratio of lithium carbonate, sodium carbonate and potassium carbonate is 43.5:31.5:25, add 4 g of sodium oxide to increase the oxygen ion content in the molten salt, mix well, put into a corundum crucible and place in a tubular electric furnace, heat to 250 ° C at a heating rate of 3 ° C / min and keep warm for 20 hours to remove moisture from the salt, then heat to 400 ° C at a heating rate of 5 ° C / min and keep warm for 25 minutes until the salt is completely melted to obtain a molten salt electrolyte;
[0047] S2. Select a nickel-iron alloy with a mesh structure as the anode material, select a graphite with a flake structure as the cathode material, dry 20g of chicken manure to a moisture content of 5%, and then fix the chicken manure on the anode surface through a foam aluminum sheet, then place the cathode and anode below the molten salt electrolyte liquid level, connect the two electrodes to a constant current meter, set the current electrolysis parameter of the constant current meter to 0.05A, obtain combustible gas and biochar at the anode, and obtain nanocarbon material at the cathode.
[0048] Comparative Example
[0049] The method for obtaining bamboo biochar by pyrolyzing bamboo under a conventional nitrogen atmosphere comprises the following steps:
[0050] S1. Take 200 g of lithium carbonate, sodium carbonate and potassium carbonate in total, wherein the molar ratio of lithium carbonate, sodium carbonate and potassium carbonate is 43.5:31.5:25, add 4 g of lithium oxide, mix well, put into a corundum crucible and place in a tubular electric furnace, heat to 300 ° C at a heating rate of 5 ° C / min and keep warm for 24 hours to remove moisture from the salt, then heat to 500 ° C at a heating rate of 10 ° C / min and keep warm for 30 minutes until the salt is completely melted to obtain a molten salt medium;
[0051] S2. Crush 20 g of bamboo and dry it to a moisture content of 5%, then immerse the dried bamboo directly below the surface of a molten salt medium for pyrolysis for 2 h to obtain bamboo biochar.
[0052] Test Example 1
[0053] During the electrolysis process of Example 1, the curve of current change over time was recorded, and the result was as follows: Figure 1 As shown, the online gas analyzer is turned on to detect the anode gas product in real time. The results are as follows Figure 2 shown.
[0054] Depend on Figure 1 and Figure 2 It can be seen that after the start of electrolysis, the concentrations of combustible gases such as carbon monoxide, hydrogen, methane, ethane, and ethylene increased significantly, rising to 600 ppm, and no carbon dioxide, sulfur oxides, or nitrogen oxides were generated.
[0055] Test Example 2
[0056] The biochar obtained at the anode and the nanocarbon material obtained at the cathode in Example 1 were collected, washed with 1 mol / L dilute hydrochloric acid, and then observed under a scanning electron microscope. The results are as follows: Figure 3 shown.
[0057] Depend on Figure 3 It can be seen that the morphology of the cathode carbon material under the scanning electron microscope is nanowires.
[0058] Test Example 3
[0059] The nitrogen adsorption and desorption curves of the biochar produced by using bamboo as raw material in Example 1 and the bamboo biochar obtained by pyrolysis under a conventional nitrogen atmosphere in the comparative example were compared. Figure 4 shown.
[0060] Depend on Figure 4 It can be seen that the biochar obtained by the molten salt electrochemical process in Example 1 obviously has a more developed pore structure and a higher specific surface area.
[0061] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for co-producing combustible gas-biochar and nano-carbon materials by electrochemical cracking of biomass using molten salt, characterized in that: The following steps are involved: S1. Heating the salt containing oxygen ions until it is completely melted to obtain a molten salt electrolyte; S2. The biomass is dried and fixed on the anode surface in a two-electrode system, and then the cathode and anode are placed below the molten salt electrolyte liquid level for electrolysis, whereby combustible gas and biochar are obtained at the anode and nanocarbon materials are obtained at the cathode.
2. The method for co-producing combustible gas-biochar and nano-carbon materials by molten salt electrochemical cracking of biomass according to claim 1, characterized in that: In step S1, the oxygen ions are derived from the added metal oxide or the ionization of the molten salt electrolyte itself at high temperature, and the metal oxide is at least one of lithium oxide, sodium oxide, potassium oxide and calcium oxide.
3. The method for co-producing combustible gas-biochar and nano-carbon materials by molten salt electrochemical cracking of biomass according to claim 1, characterized in that: In step S1, the salt is a carbonate salt or a chloride salt; the carbonate salt is at least one of lithium carbonate, sodium carbonate, potassium carbonate and calcium carbonate; the chloride salt is at least one of lithium chloride, sodium chloride, potassium chloride and calcium chloride.
4. The method for co-producing combustible gas-biochar and nano-carbon materials by molten salt electrochemical cracking of biomass according to claim 1, characterized in that: In step S1, the temperature is first increased to 250-350°C at 3-8°C / min and kept at this temperature for 20-30h, and then increased to 400-1000°C at 5-15°C / min and kept at this temperature for 25-35min.
5. The method for co-producing combustible gas-biochar and nano-carbon materials by molten salt electrochemical cracking of biomass as claimed in claim 1, characterized in that: In step S2, the biomass is one of agricultural and forestry waste, kitchen waste, livestock and poultry manure and microalgae.
6. The method for co-producing combustible gas-biochar and nano-carbon materials by molten salt electrochemical cracking of biomass as claimed in claim 1, characterized in that: In step S2, the biomass is dried at 60-100°C to a moisture content of 5-10%.
7. The method for co-producing combustible gas-biochar and nano-carbon materials by molten salt electrochemical cracking of biomass as claimed in claim 1, characterized in that: In step S2, the biomass is fixed on the surface of the anode by means of foam metal, and the foam metal is one of foam nickel, foam nickel alloy, foam aluminum, foam aluminum alloy, foam copper and foam copper alloy.
8. The method for co-producing combustible gas-biochar and nano-carbon materials by molten salt electrochemical cracking of biomass as claimed in claim 1, characterized in that: In step S2, in the two-electrode system, the anode electrode material is one of gold, silver, platinum, nickel, copper, nickel-iron alloy, nickel-iron-copper alloy, ruthenium dioxide, nickel-doped yttria-stabilized zirconia, cobalt-doped yttria-stabilized zirconia, copper-doped gadolinium-doped cerium oxide, ruthenium-doped gadolinium-doped cerium oxide, lanthanum strontium manganese oxide and graphite; the cathode electrode material is one of gold, silver, platinum, nickel, copper, molybdenum, nickel-iron alloy, nickel-iron-copper alloy and graphite.
9. The method for co-producing combustible gas-biochar and nano-carbon materials by molten salt electrochemical cracking of biomass as claimed in claim 1, characterized in that: In step S2, electrolysis is performed in a constant cell voltage or constant current manner.
10. The method for co-producing combustible gas-biochar and nano-carbon materials by molten salt electrochemical cracking of biomass according to claim 9, characterized in that: The constant cell voltage is 1.5-5V, and the constant current is 0.05-2A.