Electrocatalytic coating with ultrahigh specific surface area, electrode and application
By introducing fullerene metal complexes into the metal oxide coating, an ultra-high specific surface area electrocatalytic coating is formed, and the uneven electrocatalytic performance of metal oxide coating electrodes under high current density and high electrode potential and lifetime are solved. The shorter problem achieves more efficient, more uniform electrolytic performance and longer electrode life.
Patent Information
- Application Number
- CN202410970346.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
Existing metal oxide coated electrodes exhibit uneven electrocatalytic performance, high electrode potential and short life at high current density, which is difficult to meet the strict requirements of modern industry for electrode performance.
Using an ultra-high specific surface area electrocatalytic coating composed of mixed metal oxides and fullerene metal complexes, the fullerene metal complex is formed by reacting fullerene with metal ions, combining metal oxides with electrocatalytic activity and The valve metal oxide forms an electrocatalytic coating with high catalytic activity and large specific surface area, and is coated on the valve metal substrate, and the electrode is formed after multiple sintering.
It improves the catalytic activity and real area of the electrode, reduces the current density and electrode potential during electrolysis, and extends the service life of the electrode. It is suitable for electrolytic copper foil, electrolytic chlorine production, PCB plating, hydrometallurgy, cathode protection and other fields.
Smart Images

Figure CN118910662A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrocatalytic coatings, and in particular to an ultra-high specific surface area electrocatalytic coating, an electrode and applications thereof. Background Art
[0002] In 1965, Dr. Beer invented the Ru-Ti metal oxide coating and applied it to the electrolysis of seawater to produce chlorine, achieving a breakthrough in the electrolysis industry. After decades of development, this electrode made of valve metal as the base material and metal oxide coating as the electrocatalytic material has made continuous breakthroughs. For example, the Ru-Ir-Ti ternary oxide coating anode has a good chlorine evolution function in alkaline electrolytes and is widely used in the chlor-alkali industry, electrolysis of chlorides to produce chlorates or hypochlorites, electrolysis of effective chlorine for water disinfection, cathodic protection and other fields. Iridium oxide and tantalum oxide mixed oxide coatings have the characteristics of low electrode potential and long life in acidic electrolytes, and are widely used in electrolytic extraction of non-ferrous metals, steel plate galvanizing, electrolytic copper foil and other fields. However, as modern industry has increasingly stringent requirements for the application of electrodes, the performance of metal oxide coated electrodes needs to be further improved. For example, in order to improve production efficiency, the electrode needs to adapt to electrolysis at a higher current density, the coating should have a more uniform electrocatalytic performance to ensure the quality of the electrolysis product, the electrode should have a lower electrode potential to reduce the energy consumption of electrolysis, and the electrode should have a longer life to reduce the cost of use.
[0003] Fullerene is a molecule composed of carbon atoms with a spherical, cylindrical or spherical-cylindrical structure. This special structure gives it the following excellent properties, making it a breakthrough in the application of electrolysis. (i) Fullerene is a zero-dimensional material with a carbon cage structure that gives it a large specific surface area; (ii) Fullerene is a catalyst that can catalyze redox reactions; (iii) Fullerene has high chemical stability, can resist chemical corrosion, and can be used for a long time in acidic or alkaline electrolytes; (iv) Fullerene is a semiconductor with a certain conductivity; (v) Fullerene has the chemical properties of electron-deficient olefins, can react with metals and free radicals, and exhibits the characteristics of aromaticity and electrophilic addition reactions; (vi) Some fullerene compounds (such as doped C60) exhibit good superconductivity, and their superconducting starting temperature can reach 18K. At present, the preparation of metal oxide coating electrodes in industry basically adopts the thermal decomposition method to prepare the coating, but the high temperature resistance of ordinary fullerene is limited, so it is necessary to modify and dope fullerene to enable it to be used on metal oxide coating electrodes. C60 itself is basically non-conductive, but after inserting alkali metals (lithium, sodium, potassium, ruthenium, cesium) or alkaline earth metals (beryllium, magnesium, calcium, strontium, barium, radium) between C60 and C60, the conductive properties of this new compound will change significantly. Some can become metal conductors, and some can even become superconductors. At the same time, the high temperature resistance of fullerene is greatly improved. In 1991, Koefod et al. synthesized the first iridium fullerene derivative, which enhanced the catalytic performance of fullerene.
[0004] Based on the above considerations, some problems currently encountered by metal oxide coated electrodes can be solved by modifying fullerenes and applying them in metal oxide coated electrodes. Summary of the invention
[0005] In response to the above technical problems in the related art, the present invention provides an ultra-high specific surface area electrocatalytic coating, electrode and application, which can solve the above problems.
[0006] To achieve the above technical objectives, the technical solution of the present invention is implemented as follows: An ultra-high specific surface area electrocatalytic coating, composed of a mixed metal oxide and a fullerene metal complex, wherein the fullerene metal complex is obtained by reacting fullerene and metal ions, and the mixed metal oxide is composed of a metal oxide with electrocatalytic activity and a valve metal oxide, wherein the mass proportions of the fullerene metal complex, the metal oxide with electrocatalytic activity, and the valve metal oxide in the electrocatalytic coating are (1%-50%): (30%-79%): (20%-49%).
[0007] Furthermore, the fullerene-metal complex includes an endogenous fullerene-metal complex, a doped fullerene-metal complex, and an exogenous fullerene-metal complex.
[0008] Furthermore, the metal oxide having electrocatalytic activity includes one or more metal oxides of gold, silver, platinum, palladium, rhodium, ruthenium, manganese, nickel, cobalt, lead, and tin.
[0009] Furthermore, the valve metal oxide includes one or more metal oxides of titanium, tantalum, niobium, zirconium, and hafnium.
[0010] An electrode comprises a valve metal substrate, on which the electrocatalytic coating is coated.
[0011] Furthermore, the valve metal substrate includes one or more of titanium, tantalum, niobium, zirconium, nickel, molybdenum or tungsten.
[0012] Furthermore, the valve metal substrate is in the shape of a sheet, a mesh, a tube, a perforated plate or particles.
[0013] Furthermore, the surface of the valve metal substrate is a roughened surface, which is prepared by one or more methods of grinding, sandblasting, etching, thermal spraying, anodizing, and micro-arc oxidation, and a layer of ceramic oxide film is deposited on the roughened surface as an intermediate layer.
[0014] Furthermore, the electrocatalytic coating is applied by one or more methods including dipping, spin coating, brushing, roller coating or spraying. After the electrocatalytic coating is applied, it is necessary to heat at a temperature of 300 to 550° C. for not less than 20 minutes, and then repeat the coating, drying and sintering for a total of 5 to 30 times after cooling.
[0015] An application of an electrode, wherein the electrode is used as an anode in electrolytic copper foil, electrolytic chlorine production, PCB electroplating, hydrometallurgy, cathode protection, water treatment, and electrolytic hydrogen production.
[0016] Beneficial effects of the present invention: The present invention introduces a fullerene metal complex into the mixed metal oxide coating. The introduction of the fullerene metal complex can improve the catalytic activity of the coating, and at the same time change the morphology of the coating so that it has an ultra-high specific surface area, thereby increasing the actual area of the prepared electrode and reducing the actual current density during electrolysis. At the same time, the electrode has the characteristics of uniform electrochemical performance, resistance to large current density, low electrode potential, and long service life. It can be applied to electrolytic copper foil, electrolytic chlorine production, PCB electroplating, hydrometallurgy, cathode protection, water treatment, electrolytic hydrogen production and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0018] The present invention is further described in detail below with reference to the accompanying drawings.
[0019] Figure 1 is a schematic structural diagram of an electrode according to an embodiment of the present invention; Figure 2 1 is a cyclic voltammetry curve diagram of the electrode prepared in the embodiment of the present invention and the comparative example; Figure 3 1 is a linear sweep voltammetry curve of the electrode prepared in the embodiment of the present invention and the comparative example; Figure 4 It is a performance comparison chart of the embodiments of the present invention and the comparative examples. DETAILED DESCRIPTION
[0020] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.
[0021] like Figure 1 As shown, according to the present invention, an ultra-high specific surface area electrocatalytic coating, electrode and application are disclosed, the electrocatalytic coating is composed of a mixed metal oxide and a fullerene metal complex, the fullerene metal complex is obtained by reacting fullerene and metal ions, the mixed metal oxide is composed of a metal oxide with electrocatalytic activity and a valve metal oxide, wherein the mass proportion of the fullerene metal complex, the metal oxide with electrocatalytic activity, and the valve metal oxide in the electrocatalytic coating is (1%-50%): (30%-79%): (20%-49%). An electrocatalytic coating 1 is applied on a valve metal substrate 3 to form an electrode, wherein a layer of ceramic oxide film 2 is deposited on the roughened surface of the valve metal substrate 3 as an intermediate layer. The electrode of the present application can be used in the fields of electrolytic copper foil, electrolytic chlorine production, PCB electroplating, hydrometallurgy, cathodic protection, water treatment, electrolytic hydrogen production, etc., and can be used as an anode therein.
[0022] Embodiment 1: This embodiment provides an ultra-high specific surface area electrocatalytic coating and an oxygen evolution electrode made therefrom, such as Figure 1As shown, it uses valve metal material as the substrate, ceramic oxide layer as the intermediate layer, fullerene metal complex and mixed metal oxide as the catalytic coating. The specific preparation process is as follows: S1 Matrix roughening: Processing: blast steel grit on an industrial pure titanium plate (made of TA1) with a specification of 100mm*100mm*1mm to obtain a roughened surface, then immerse the titanium plate in a 10% oxalic acid solution at 90-100°C for etching for 2 hours, and then rinse it with pure water after taking it out; Preparation of S2 intermediate layer: dissolve tin tetrachloride in isopropanol solution with a concentration of 0.1 mol / L, and evenly apply the prepared solution on the titanium substrate treated in step S1, sinter at 400°C for 30 min, and repeat the coating and sintering process 3 times to form a tin dioxide intermediate layer; S3 electrocatalytic coating preparation: Fullerene and iridium metal derivatives (hereinafter referred to as C 60 @Ir) is dissolved in carbon disulfide solution, then iridium trichloride and tantalum pentachloride are dissolved in isopropanol solution, and the above two solutions are mixed and stirred at room temperature for 12 hours to form a uniform solution; in the prepared solution, Ir:Ta:C 60 The molar ratio of @Ir is 7:3:1, and the total concentration is 0.2 mol / L. The prepared solution is evenly applied on the intermediate layer prepared by S2 and sintered at 480 °C for 30 min. The coating and sintering process is repeated 10 times.
[0023] Embodiment 2: This embodiment provides an ultra-high specific surface area electrocatalytic coating and an oxygen evolution electrode made therefrom, which is basically the same as the operation in embodiment 1, except that in step S3, Ir:Ta:C 60 @Ir molar ratio is 7:3:2.
[0024] Embodiment 3: This embodiment provides an ultra-high specific surface area electrocatalytic coating and an oxygen evolution electrode made therefrom, which is basically the same as the operation in Example 1, except that the fullerene metal complex used in step S3 is a metal derivative of fullerene and tantalum.
[0025] Embodiment 4: This embodiment provides an ultra-high specific surface area electrocatalytic coating and a chlorine evolution electrode made therefrom, which has the same structure as that in Example 1, and its specific preparation process is as follows: S1 Matrix roughening: Spray brown corundum on an industrial pure titanium plate (TA1) with a specification of 100 mm*100 mm*1 mm to obtain a roughened surface. Then immerse the titanium plate in a boiling 20% hydrochloric acid solution for etching for 20 minutes, and then rinse it with pure water after taking it out. S2 preparation of intermediate layer: dissolving titanium butoxide and tantalum pentachloride in isopropanol solution, wherein the molar ratio of titanium to tantalum is 4:6 and the total concentration is 0.1 mol / L, and evenly brushing the prepared solution on the titanium substrate treated in step S1, sintering at 450°C for 30 minutes, and repeating the brushing and sintering process 3 times to form an intermediate layer of titanium dioxide and tantalum pentoxide; S3 electrocatalytic coating preparation: Fullerene and ruthenium metal derivatives (hereinafter referred to as C 60 @Ru) was dissolved in a carbon disulfide solution, and then ruthenium trichloride, iridium trichloride, and titanium butoxide were dissolved in an isopropanol solution. The two solutions were mixed and stirred at room temperature for 12 hours to form a uniform solution. In the prepared solution, Ru:Ir:Ti: C 60 The molar ratio of @Ir is 1.5:1.5:7:2, and the total concentration is 0.2 mol / L. The prepared solution is evenly applied on the intermediate layer prepared by S2 and sintered at 450 °C for 30 min. The coating and sintering process is repeated 10 times.
[0026] Embodiment 5: This embodiment provides an ultra-high specific surface area electrocatalytic coating and a chlorine evolution electrode made therefrom, which is basically the same as that in Example 4, except that the fullerene metal complex used in step S3 is a metal derivative of fullerene and titanium.
[0027] Comparative Example 1: This comparative example provides an electrocatalytic coating and an oxygen evolution electrode made therefrom. For comparison, the coating does not contain a fullerene metal complex, and the molar ratio of Ir:Ta is 7:3.
[0028] Comparative Example 2: This comparative example provides an electrocatalytic coating and a chlorine evolution electrode made therefrom. For comparison, the coating does not contain a fullerene metal complex, and the molar ratio of Ru:Ir:Ti is 1.5:1.5:7.
[0029] test: The electrodes prepared in Examples 1-5 and Comparative Examples 1-2 were subjected to cyclic voltammetry, linear sweep voltammetry and accelerated life tests.
[0030] The cyclic voltammetry test conditions are as follows: the open circuit potential value is tested using an electrochemical workstation, and the test is carried out in a three-electrode electrolytic cell. The reference electrode is a saturated calomel electrode (SCE), the auxiliary electrode is a platinum electrode, the working electrode is the prepared electrode, and the test area is 2 cm 2The oxygen evolution electrode was tested in 0.5 mol / L H2SO4 solution as electrolyte, and the chlorine evolution electrode was tested in saturated NaCl solution. The temperature was controlled at 25±0.5 ℃. The cyclic voltammetry curve was completed in the range of 0-1.2 V at a scan rate of 20 mV / s. The voltammetric charge of the electrode can be obtained by integrating the obtained curve.
[0031] The linear sweep voltammetry test conditions are as follows: the open circuit potential value is tested using an electrochemical workstation, and the test is carried out in a three-electrode electrolytic cell. The reference electrode is a saturated calomel electrode, the auxiliary electrode is a platinum electrode, the working electrode is the prepared electrode, and the test area is 1 cm 2 The oxygen evolution electrode was tested in 0.5 mol / L H2SO4 solution as electrolyte, and the chlorine evolution electrode was tested in saturated NaCl solution. The temperature was controlled at 25±0.5 ℃. The polarization curve was completed in the range of 0-1.5 V at a scan rate of 2mV / s, and the electrode potential was obtained from the polarization curve.
[0032] The accelerated life test conditions are as follows: use a DC power supply, the electrolyte is 1 mol / L H2SO4 (oxygen evolution electrode) or saturated NaCl solution (chlorine evolution electrode), keep the water bath temperature at 60±1 ℃, the titanium sheet is used as the cathode, the prepared electrode is cut into 1*2cm size as the anode, the distance between the cathode and the cathode is 1cm, and the constant current density is 500 A / m 2 ,Record the change of cell voltage with time, and a sharp rise of 5V in cell voltage is considered as anode failure.
[0033] The test results are as follows Figure 2-4 As shown: Test analysis: Compare Examples 1-3 with Comparative Example 1, and Examples 4-5 with Comparative Example 2. Figure 4 and Figure 2 Analysis shows that whether fullerene metal complexes are introduced into the oxygen evolution electrode IrO2 / Ta2O5 or the ruthenium iridium titanium catalytic coating of the chlorine evolution electrode, the voltammetric charge increases significantly, and the area of the voltammetric curve is proportional to the number of active material centers on the oxide anode surface, indicating that the introduction of fullerene metal complexes makes the electrode have a larger active specific surface area and improves the electrocatalytic activity of the catalytic coating. Figure 4 and Figure 3 Analysis shows that the introduction of fullerene metal complexes reduces the oxygen evolution / chlorine evolution potential of the electrode to a certain extent, which helps the electrode to obtain a lower cell voltage during electrolysis. Figure 4 It can be seen that the introduction of fullerene metal complexes can also increase the electrolysis life of oxygen evolution / chlorine evolution electrodes by more than 50%.
[0034] In summary, the ultra-high specific surface area electrocatalytic coating of the present application and the electrode made therefrom have the following advantages compared with the metal oxide coating electrodes commonly used in the current electrolysis field: (1) Improve production efficiency: The coating has a higher specific surface area, which increases the actual area of the electrode and reduces the actual current density during electrolysis. This can meet the needs of industrial production to perform electrolysis at a higher current density in order to improve production efficiency.
[0035] (2) Improve product quality: The coating has more uniform electrocatalytic properties, the discharge is uniform during electrolysis, the performance of the electrolysis product is more uniform, and the quality is more stable.
[0036] (3) Reduce costs: The electrode has a lower electrode potential and a lower cell pressure during electrolysis, which can reduce the energy consumption of electrolysis. At the same time, the electrode life is longer, which reduces maintenance and extends the procurement cycle.
[0037] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An ultra-high specific surface area electrocatalytic coating, It is characterized in that It is composed of a mixed metal oxide and a fullerene metal complex, wherein the fullerene metal complex is obtained by reacting fullerene with metal ions, and the mixed metal oxide is composed of a metal oxide with electrocatalytic activity and a valve metal oxide, wherein the mass proportions of the fullerene metal complex, the metal oxide with electrocatalytic activity, and the valve metal oxide in the electrocatalytic coating are (1%-50%): (30%-79%): (20%-49%).
2. The ultra-high specific surface area electrocatalytic coating according to claim 1, It is characterized in that The fullerene metal complex includes an endogenous fullerene metal complex, a doped fullerene metal complex, and an exogenous fullerene metal complex.
3. The ultra-high specific surface area electrocatalytic coating according to claim 1, It is characterized in that The metal oxide having electrocatalytic activity includes one or more metal oxides selected from the group consisting of gold, silver, platinum, palladium, rhodium, ruthenium, manganese, nickel, cobalt, lead, and tin.
4. The ultra-high specific surface area electrocatalytic coating according to claim 1, It is characterized in that The valve metal oxide includes one or more metal oxides of titanium, tantalum, niobium, zirconium, and hafnium.
5. An electrode, It is characterized in that The invention comprises a valve metal substrate, on which the electrocatalytic coating according to any one of claims 1 to 4 is coated.
6. An electrode according to claim 5, It is characterized in that The valve metal substrate includes one or more of titanium, tantalum, niobium, zirconium, nickel, molybdenum or tungsten.
7. An electrode according to claim 5, It is characterized in that The valve metal substrate is in the form of a sheet, a mesh, a tube, a perforated plate or particles.
8. An electrode according to claim 5, It is characterized in that The surface of the valve metal substrate is a roughened surface, which is prepared by one or more methods of grinding, sandblasting, etching, thermal spraying, anodizing, and micro-arc oxidation, and a ceramic oxide film is deposited on the roughened surface as an intermediate layer.
9. An electrode according to claim 5, It is characterized in that The electrocatalytic coating is applied by one or more methods including dipping, spin coating, brushing, roller coating or spraying. After the electrocatalytic coating is applied, it is necessary to heat at a temperature of 300 to 550° C. for not less than 20 minutes, and then repeat the coating, drying and sintering for a total of 5 to 30 times after cooling.
10. Use of an electrode according to claim 5, It is characterized in that The electrode is used as an anode in electrolytic copper foil, electrolytic chlorine production, PCB electroplating, hydrometallurgy, cathode protection, water treatment, and electrolytic hydrogen production.
Citation Information
Cited By
Organic additive oxidation resistant insoluble anode for PCB electroplating and preparation method thereof
CN121951657A
An insoluble anode for PCB electroplating against oxidation of organic additives and a preparation method thereof
CN121951657B