Alkali-resistant aluminum alloy and preparation process thereof
By forming a multi-layer structure on the surface of the aluminum alloy, including a porous alumina layer and a silica sealing layer, the problem of corrosion of aluminum alloy in an alkaline environment is solved, its alkali resistance and service life are improved, and its appearance is maintained quality.
Patent Information
- Application Number
- CN202410972050.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
Aluminum alloys are susceptible to corrosion in alkaline environments. The existing anodizing technology causes damage and decolorization of the surface film layer under the action of alkaline detergents, affecting service life and appearance.
Using a multi-layer structure alkali-resistant aluminum alloy, including a porous alumina layer and a silica sealing layer, the porous layer is formed through anodizing process, and primary and secondary sealing are carried out to enhance the corrosion resistance and wear resistance of the surface. sex.
It significantly improves the tolerance of aluminum alloy to alkaline environment, extends service life, maintains appearance quality, reduces maintenance and replacement needs, and enhances market competitiveness.
Smart Images

Figure CN118910690A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy materials, in particular to an alkali-resistant aluminum alloy and a preparation process thereof. Background Art
[0002] Aluminum alloys are widely used in various industrial fields due to their excellent physical and chemical properties. However, during the use of aluminum alloys, their surfaces are easily affected by the environment, such as corrosion and wear, which will seriously affect their service life and performance.
[0003] To solve this problem, researchers have adopted a variety of surface treatment technologies, among which anodizing is a commonly used surface treatment method. It can form a dense aluminum oxide film on the surface of aluminum alloy, thereby improving its corrosion resistance and wear resistance. However, the aluminum oxide film has a high porosity and strong adsorption capacity. It is easy to adsorb pollutants in the environment, affecting the appearance of the film. It is also susceptible to corrosion by corrosive anions, causing damage to the film.
[0004] Although the existing technology has improved the alkali resistance of aluminum alloy anodized surface to a certain extent, there are still some problems. Aluminum oxide will react with hydroxide in an alkaline environment. Therefore, when aluminum alloy anodized workpieces used in kitchen appliances encounter alkaline cleaners (such as green umbrella, Vigor, etc.), the surface film layer will be damaged, causing discoloration and other undesirable phenomena.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] One of the objects of the present invention is to provide an alkali-resistant aluminum alloy to alleviate at least one of the above-mentioned technical problems in the prior art.
[0007] A second object of the present invention is to provide a process for preparing an alkali-resistant aluminum alloy.
[0008] In order to solve the above-mentioned technical problems, the present invention particularly adopts the following technical solutions:
[0009] A first aspect of the present invention provides an alkali-resistant aluminum alloy, comprising an aluminum alloy substrate and a multilayer structure formed on the surface of the aluminum alloy substrate;
[0010] The multilayer structure comprises a porous layer and a sealing layer which are stacked;
[0011] The sealing layer comprises a first sealing layer and a second sealing layer which are stacked;
[0012] The second sealing layer is made of silicon dioxide.
[0013] Furthermore, the material of the porous layer is porous alumina.
[0014] Preferably, the thickness of the porous layer is 0.5 μm to 10 μm.
[0015] Preferably, the first sealing layer is made of aluminum oxide.
[0016] Preferably, the thickness of the first sealing layer is 1 μm to 3 μm.
[0017] Furthermore, the thickness of the second sealing layer is 3 μm to 5 μm.
[0018] Furthermore, the multilayer structure comprises a porous layer, a coloring layer and a sealing layer;
[0019] The colored layer is formed in the microporous structure inside the porous layer;
[0020] The sealing layer is formed on the surface of the colored layer or the surface of the porous layer.
[0021] Preferably, the material of the aluminum alloy substrate includes 5 series aluminum alloy or 6 series aluminum alloy.
[0022] The second aspect of the present invention provides a preparation process of the alkali-resistant aluminum alloy, specifically, the porous layer is generated on the surface of the aluminum alloy substrate by an anodizing process, and the porous layer is sealed once and twice to obtain the alkali-resistant aluminum alloy.
[0023] Furthermore, the process of the primary sealing includes:
[0024] The aluminum alloy substrate with the porous layer is subjected to a hydration reaction in deionized water to obtain a first sealing layer.
[0025] Preferably, the temperature of the hydration reaction is 95°C to 98°C.
[0026] Preferably, the hydration reaction time is 5 min to 10 min.
[0027] Furthermore, the secondary sealing process includes:
[0028] The aluminum alloy substrate with the first sealing layer is immersed in a sealing liquid for sealing, and then solidified to obtain the second sealing layer.
[0029] Preferably, the sealing temperature is 20°C to 40°C.
[0030] Preferably, the sealing time is 3 minutes to 10 minutes.
[0031] The sealing liquid is a water-based sealing liquid or a solvent-based sealing liquid.
[0032] Furthermore, the water-based sealing liquid includes 5wt.% to 15wt.% of phenyltrimethoxysilane, 5wt.% to 15wt.% of silica sol, 3wt.% to 8wt.% of tetraethyl orthosilicate, 5wt.% to 10wt.% of (3-epoxypropyl)propyltrimethoxysilane, and the balance is deionized water.
[0033] Preferably, the curing temperature is 80°C to 150°C.
[0034] Preferably, the curing time is 5 min to 20 min.
[0035] Furthermore, the solvent-based sealing liquid includes 20wt.% to 35wt.% of methylphenyl silicone resin, 15wt.% to 25wt.% of acrylic modified silicone resin, 5wt.% to 10wt.% of silica sol, 2wt.% to 3wt.% of leveling agent, 1wt.% to 2wt.% of alkylphenol polyoxyethylene ether, and the balance is ethylene glycol butyl ether.
[0036] Preferably, the curing temperature is 120°C to 150°C.
[0037] Preferably, the curing time is 20 min to 40 min.
[0038] Furthermore, the preparation process of the alkali-resistant aluminum alloy also includes a coloring process before sealing after the porous layer is generated.
[0039] Preferably, the aluminum alloy substrate with the porous layer is placed in a dyeing liquid for dyeing to obtain the colored layer.
[0040] Preferably, the coloring time is 5 min to 10 min.
[0041] Preferably, the dyeing liquid is an inorganic dyeing liquid or an organic dyeing liquid.
[0042] Furthermore, before the anodizing process is performed, a pre-treatment process of the aluminum alloy substrate is also included.
[0043] Preferably, the pre-treatment process includes degreasing, alkali treatment, primary neutralization, polishing and secondary neutralization performed in sequence.
[0044] Compared with the prior art, the present invention has at least the following beneficial effects:
[0045] The alkali-resistant aluminum alloy provided by the present invention has a multi-layer corrosion-resistant structure arranged on the surface of the aluminum alloy substrate, which not only enhances the stability of the aluminum alloy surface, but also the outer second sealing layer prevents the corrosion of the aluminum alloy substrate by alkaline substances, thereby improving its tolerance to alkaline environment, extending the service life of the alkali-resistant aluminum alloy and maintaining the appearance quality, reducing the need for maintenance and replacement, improving user experience, and also improving the overall value and market competitiveness of the product.
[0046] The preparation process provided by the present invention forms a uniform and highly ordered porous layer through an anodic oxidation process, which provides a good foundation for the subsequent sealing step and ensures the uniformity and adhesion of the first sealing layer and the second sealing layer. After the porous layer is sealed once, the micropores on the surface are effectively filled, reducing the penetration path of the corrosive medium. Further secondary sealing operations, especially using silicon dioxide as a sealing material, improve the surface hardness, wear resistance and alkali resistance of the alkali-resistant aluminum alloy, meeting the rated application requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0048] Figure 1 It is a structural schematic diagram of the alkali-resistant aluminum alloy of the present invention. DETAILED DESCRIPTION
[0049] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution in the embodiment of the present invention will be clearly and completely described below in combination with the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, but not all of the embodiments. The components of the embodiment of the present invention can be arranged and designed in various different configurations.
[0050] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0051] A first aspect of the present invention provides an alkali-resistant aluminum alloy, comprising an aluminum alloy substrate and a multilayer structure formed on the surface of the aluminum alloy substrate;
[0052] The multilayer structure comprises a porous layer and a sealing layer which are stacked;
[0053] The sealing layer comprises a first sealing layer and a second sealing layer which are stacked;
[0054] The second sealing layer is made of silicon dioxide.
[0055] The alkali-resistant aluminum alloy provided by the present invention has a multi-layer corrosion-resistant structure arranged on the surface of the aluminum alloy substrate, which not only enhances the stability of the aluminum alloy surface, but also the outer second sealing layer prevents the corrosion of the aluminum alloy substrate by alkaline substances, thereby improving its tolerance to alkaline environment, extending the service life of the alkali-resistant aluminum alloy and maintaining the appearance quality, reducing the need for maintenance and replacement, improving user experience, and also improving the overall value and market competitiveness of the product.
[0056] The present invention sets the material of the second sealing layer to silicon dioxide because silicon dioxide has excellent resistance to a variety of chemical substances, especially alkaline substances. This significantly improves the corrosion resistance of aluminum alloys in alkaline environments and extends their service life. At the same time, silicon dioxide has a high hardness and can effectively improve the hardness of the aluminum alloy multilayer structure, thereby enhancing its wear resistance. This makes aluminum alloy products more durable and reduces damage caused by daily wear. Silicon dioxide forms a uniform and continuous second sealing layer, effectively sealing the porous structure of the porous layer, reducing the penetration of corrosive media, and improving the sealing effect.
[0057] In addition, silicon dioxide can withstand high temperatures without changing its properties, maintaining the stability of the material's performance. It is also a naturally occurring material that is non-toxic and environmentally friendly. Using silicon dioxide as a sealing material not only meets environmental requirements but also has a low cost. Silicon dioxide as the second sealing layer material can give the aluminum alloy surface a smooth and uniform appearance, enhancing the market competitiveness and attractiveness of alkali-resistant aluminum alloys.
[0058] Furthermore, the material of the porous layer is porous alumina.
[0059] Compared with aluminum alloy, alumina is chemically inactive and not easy to react with external substances. As a protective barrier for aluminum alloy substrate, it is also easier to prepare. Due to the porous structure of porous alumina, its surface area is large, which provides better mechanical anchoring for the subsequent preparation of sealing layer and enhances the adhesion between the porous layer and the sealing layer.
[0060] Preferably, the thickness of the porous layer is 0.5 μm to 10 μm.
[0061] Typically but not limiting, the thickness of the porous layer may be, for example, 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, or any value within the range of 0.5 μm to 10 μm.
[0062] Preferably, the first sealing layer is made of aluminum oxide.
[0063] Preferably, the thickness of the first sealing layer is 1 μm to 3 μm.
[0064] The thickness of the first sealing layer within the above range can ensure that the porous layer is fully sealed.
[0065] Typically but not limiting, the thickness of the first sealing layer may be 1 μm, 2 μm or 3 μm, or any value within the range of 1 μm to 3 μm.
[0066] Furthermore, the thickness of the second sealing layer is 3 μm to 5 μm.
[0067] The thickness of the second sealing layer is within the above range, which can provide sufficient protection and improve the overall durability of the multi-layer structure.
[0068] Typically but not limiting, the thickness of the second sealing layer may be 3 μm, 4 μm or 5 μm, or any value within the range of 3 μm to 5 μm.
[0069] In one embodiment of the present invention, the structural schematic diagram of the alkali-resistant aluminum alloy is as follows Figure 1 As shown, the alkali-resistant aluminum alloy includes an aluminum alloy substrate and a multilayer structure; the multilayer structure includes a porous layer, a coloring layer and a sealing layer; the coloring layer is formed in the microporous structure inside the porous layer; the sealing layer is formed on the surface of the coloring layer or the surface of the porous layer.
[0070] Preferably, the material of the aluminum alloy substrate includes 5 series aluminum alloy or 6 series aluminum alloy.
[0071] The coloring layer is mainly used to improve the appearance of alkali-resistant aluminum alloys, giving them a colorful appearance to meet the needs of different occasions. The coloring layer not only improves the appearance quality of alkali-resistant aluminum alloys, but also increases the functionality and market adaptability of the product, which can meet a wider range of market needs and usage environments.
[0072] The second aspect of the present invention provides a preparation process of the alkali-resistant aluminum alloy, specifically, the porous layer is generated on the surface of the aluminum alloy substrate by an anodizing process, and the porous layer is sealed once and twice to obtain the alkali-resistant aluminum alloy.
[0073] The preparation process provided by the present invention forms a uniform and highly ordered porous layer through an anodic oxidation process, which provides a good foundation for the subsequent sealing step and ensures the uniformity and adhesion of the first sealing layer and the second sealing layer. After the porous layer is sealed once, the micropores on the surface are effectively filled, reducing the penetration path of the corrosive medium. Further secondary sealing operations, especially using silicon dioxide as a sealing material, improve the surface hardness, wear resistance and alkali resistance of the alkali-resistant aluminum alloy, meeting the rated application requirements.
[0074] At the same time, the preparation process of the present invention ensures the consistency and reliability of the product through standardized anodizing and sealing process flow, and each batch of alkali-resistant aluminum alloy can meet the same high quality standards and is suitable for large-scale industrial production. The anodizing and sealing processes use environmentally friendly chemicals, such as silicon dioxide, which is not only environmentally friendly but also reduces production costs, improves the durability of the alkali-resistant aluminum alloy, and reduces long-term maintenance and replacement costs.
[0075] Furthermore, the process of the primary sealing includes:
[0076] The aluminum alloy substrate with the porous layer is subjected to a hydration reaction in deionized water to obtain a first sealing layer. During the hydration reaction, aluminum oxide reacts with water to generate Al 2 O 3 ·H 2 After O, the volume expands and the membrane pores are blocked, which plays a role of sealing the pores.
[0077] Preferably, the temperature of the hydration reaction is 95°C to 98°C.
[0078] Typically but not limiting, the temperature of the hydration reaction may be 95°C, 96°C, 97°C or 98°C, or any value within the range of 95°C to 98°C.
[0079] Preferably, the hydration reaction time is 5 min to 10 min.
[0080] Typically but not limiting, the hydration reaction time may be 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes or 10 minutes, or any value within the range of 5 min to 10 min.
[0081] Furthermore, the secondary sealing process includes:
[0082] The aluminum alloy substrate with the first sealing layer is immersed in a sealing liquid for sealing, and then solidified to obtain the second sealing layer.
[0083] Preferably, the sealing temperature is 20°C to 40°C.
[0084] Typically but not limiting, the sealing temperature may be, for example, 20°C, 24°C, 28°C, 32°C, 36°C or 40°C, or any value within the range of 20°C to 40°C.
[0085] Preferably, the sealing time is 3 minutes to 10 minutes.
[0086] Typically but not limiting, the sealing time may be, for example, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min, or any value within the range of 3 min to 10 min.
[0087] The invention provides two formulas of sealing liquids, one is a water-based sealing liquid, and the other is a solvent-based sealing liquid.
[0088] The water-based sealing liquid includes 5wt.% to 15wt.% of phenyltrimethoxysilane, 5wt.% to 15wt.% of silica sol, 3wt.% to 8wt.% of tetraethyl orthosilicate, 5wt.% to 10wt.% of (3-epoxypropyl)propyltrimethoxysilane, and the balance is deionized water.
[0089] In the water-based sealing fluid, ethyl orthosilicate undergoes a hydrolysis reaction in an aqueous environment to generate silicic acid and ethanol. Subsequently, the hydroxyl groups between the generated silicic acid molecules combine with each other to form silicon-oxygen bonds and release water molecules. This process forms the basic structure of silica. As the condensation reaction proceeds, the silica particles gradually aggregate and form a three-dimensional network structure together with the silica sol, namely silica gel. Silane acts as a coupling agent in this process, promoting the reaction of hydroxyl groups on the surface of the aluminum alloy and in the silica gel to form stable silicon-oxygen bonds, thereby enhancing the bonding force between the silica layer and the substrate. Finally, the water and residual organic matter in the gel are removed by heating or natural evaporation to form a uniform and dense silica layer.
[0090] Typically but not limiting, in the water-based sealing liquid, phenyltrimethoxysilane can be, for example, 5wt.%, 6wt.%, 7wt.%, 8wt.%, 9wt.%, 10wt.%, 11wt.%, 12wt.%, 13wt.%, 14wt.% or 15wt.%, or any value within the range of 5wt.% to 15wt.%; the silica sol can be, for example, 5wt.%, 6wt.%, 7wt.%, 8wt.%, 9wt.%, 10wt.%, 11wt.%, 12wt.%, 13wt.%, 14wt.% or 15wt.%. .%, 14wt.% or 15wt.%, and can also be any value in the range of 5wt.% to 15wt.%; tetraethyl orthosilicate can be, for example, 3wt.%, 4wt.%, 5wt.%, 6wt.%, 7wt.% or 8wt.%, and can also be any value in the range of 3wt.% to 8wt.%; (3-epoxypropyl)propyltrimethoxysilane can be, for example, 5wt.%, 6wt.%, 7wt.%, 8wt.%, 9wt.% or 10wt.%, and can also be any value in the range of 5wt.% to 10wt.%.
[0091] Preferably, the curing temperature is 80°C to 150°C.
[0092] Typically but not limiting, the curing temperature of the aqueous sealing liquid can be, for example, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C, or any value within the range of 80°C to 150°C.
[0093] Preferably, the curing time is 5 min to 20 min.
[0094] Typically but not restrictively, the curing time of the water-based sealing liquid can be, for example, 5 min, 7 min, 9 min, 11 min, 13 min, 15 min, 17 min, 19 min or 20 min, or any value within the range of 5 min to 20 min.
[0095] The solvent-based sealing liquid comprises 20 wt.% to 35 wt.% of methylphenyl silicone resin, 15 wt.% to 25 wt.% of acrylic modified silicone resin, 5 wt.% to 10 wt.% of silica sol, 2 wt.% to 3 wt.% of leveling agent, 1 wt.% to 2 wt.% of alkylphenol polyoxyethylene ether, and the balance is ethylene glycol butyl ether.
[0096] In solvent-based sealing fluid, silica sol is a dispersion of already formed silica particles, which directly serves as a source of silica in the process. When coated on the surface of aluminum alloy and after a proper drying or curing process, the silica particles in the sol will aggregate and form a continuous silica layer. Methyl phenyl silicone resin and acrylic modified silicone resin not only provide additional silicon elements in the coating, but also form a stable three-dimensional network structure through their own cross-linking reaction. This structure helps to enhance the mechanical strength and corrosion resistance of the second sealing layer and provide additional support for the silica layer. Ethylene glycol butyl ether, as a solvent, can adjust the viscosity and fluidity of the solvent-based sealing fluid to ensure that the silica sol and other resin components are evenly coated on the surface of the aluminum alloy. It can also act as an evaporation rate controller during the drying process, affecting the drying dynamics, thereby affecting the microstructure and properties of the coating. Leveling agents help solvent-based sealing fluids form a smooth and uniform coating on the surface of aluminum alloys and reduce coating defects. Alkylphenol polyoxyethylene ether, as a surfactant, improves the stability and wettability of the solvent-based sealing liquid, making the coating more uniform. It may also participate in the self-assembly behavior during the drying process and affect the nanoscale structure of the second sealing layer.
[0097] Compared with water-based sealing liquid, solvent-based sealing liquid has a more stable formula, good construction performance and high surface paint film quality.
[0098] Typically but not limiting, in the solvent-based sealing liquid, the methylphenyl silicone resin can be, for example, 20wt.%, 21wt.%, 23wt.%, 25wt.%, 27wt.%, 29wt.%, 31wt.%, 33wt.% or 35wt.%, or any value within the range of 20wt.% to 35wt.%; the acrylic modified silicone resin can be, for example, 15wt.%, 16wt.%, 17wt.%, 18wt.%, 19wt.%, 20wt.%, 21wt.%, 22wt.%, 23wt.%, 24wt.% or 25wt.%, or any value within the range of 15wt.% to 25wt.%. the silica sol may be, for example, 5wt.%, 6wt.%, 7wt.%, 8wt.%, 9wt.% or 10wt.%, or any value within the range of 5wt.% to 10wt.%; the leveling agent may be, for example, 2wt.%, 2.2wt.%, 2.4wt.%, 2.6wt.%, 2.8wt.% or 3wt.%, or any value within the range of 2wt.% to 3wt.%; the alkylphenol polyoxyethylene ether may be, for example, 1wt.%, 1.2wt.%, 1.4wt.%, 1.6wt.%, 1.8wt.% or 2.0wt.%, or any value within the range of 1wt.% to 2wt.%.
[0099] Preferably, the curing temperature is 120°C to 150°C.
[0100] Typically but not limiting, the curing temperature of the solvent-based sealing liquid may be, for example, 120°C, 130°C, 140°C or 150°C, or any value within the range of 120°C to 150°C.
[0101] Preferably, the curing time is 20 min to 40 min.
[0102] Typically but not limiting, the curing time of the solvent-based sealing liquid may be, for example, 20 min, 25 min, 30 min, 35 min or 40 min, or any value within the range of 20 min to 40 min.
[0103] Furthermore, the preparation process of the alkali-resistant aluminum alloy also includes a coloring process before sealing after the porous layer is generated.
[0104] Preferably, the aluminum alloy substrate with the porous layer is placed in a dyeing liquid for dyeing to obtain the colored layer.
[0105] Preferably, the coloring time is 5 min to 10 min.
[0106] Typically but not limiting, the coloring time may be, for example, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min, or any value within the range of 5 min to 10 min.
[0107] Preferably, the dyeing liquid is an inorganic dyeing liquid or an organic dyeing liquid.
[0108] Furthermore, before the anodizing process is performed, a pre-treatment process of the aluminum alloy substrate is also included.
[0109] Preferably, the pre-treatment process includes degreasing, alkali treatment, primary neutralization, polishing and secondary neutralization performed in sequence.
[0110] In the following, some embodiments of the present invention are described in detail in conjunction with the embodiments. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.
[0111] The aluminum alloy workpieces used in the following examples and comparative examples were all pre-treated, and the pre-treatment included the following steps:
[0112] 1. Degreasing: At room temperature, soak the aluminum alloy workpiece in an acidic degreasing agent (2% to 3% sulfuric acid or phosphoric acid) for 3 to 5 minutes.
[0113] 2. Alkali treatment: At a temperature of 40 to 80°C, immerse the degreased workpiece in a 3% to 8% concentration of sodium hydroxide solution for 5 to 15 seconds to remove the naturally generated aluminum oxide film on the surface of the aluminum alloy workpiece and the residual acid from degreasing.
[0114] 3. Primary neutralization: At room temperature, soak the aluminum alloy workpiece in 10% to 20% nitric acid solution for 10 to 30 seconds to remove impurities remaining after alkaline corrosion and neutralize the alkali solution remaining after alkaline corrosion.
[0115] 4. Polishing: Immerse the aluminum alloy workpiece in chemical polishing liquid. Through the chemical ion reaction between aluminum and chemical polishing liquid, different degrees of deep polishing will occur on the uneven parts of the aluminum alloy surface, producing a gloss effect on the surface of the aluminum part, making the surface of the aluminum part have a smooth mirror effect.
[0116] 5. Secondary neutralization: The aluminum alloy workpiece is immersed in an aqueous solution formed by potassium permanganate and sulfuric acid to remove stains on the surface after the chemical polishing solution, thereby obtaining the aluminum alloy substrate used in the examples and comparative examples.
[0117] Example 1
[0118] This embodiment provides an alkali-resistant aluminum alloy, and the preparation process steps are as follows:
[0119] 1. Anodize the aluminum alloy substrate in a sulfuric acid solution to form a porous aluminum oxide film on its surface. Then dye it in a dye for 10 minutes.
[0120] 2. The dyed aluminum alloy substrate was placed in deionized water at 96° C. for hydration reaction for 5 minutes to obtain the first sealing layer.
[0121] 3. Immerse the aluminum alloy after the first sealing in a water-based sealing liquid for sealing. The sealing time is 10 minutes and the sealing temperature is 30°C.
[0122] Water-based sealing liquid composition: 5% phenyltrimethoxysilane, 5% nano-SiO 2 Sol, 3% ethyl orthosilicate, 5% (3-epoxypropyloxy)propyltrimethoxysilane, and the balance is deionized water.
[0123] 4. Then, the aluminum alloy substrate with the multilayer structure is placed in an oven and baked at 80° C. for 15 minutes to obtain the alkali-resistant aluminum alloy.
[0124] Example 2
[0125] This embodiment provides an alkali-resistant aluminum alloy, and the preparation process steps are as follows:
[0126] 1. Same as the step in Example 1.
[0127] 2. The dyed aluminum alloy substrate was placed in deionized water at 96° C. for hydration reaction for 8 minutes to obtain the first sealing layer.
[0128] 3. Immerse the aluminum alloy after the first sealing into a water-based sealing liquid for sealing. The sealing time is 5 minutes and the sealing temperature is 30°C.
[0129] Water-based sealing liquid composition: 10% phenyltrimethoxysilane, 10% nano-SiO 2 Sol, 5% ethyl orthosilicate, 7% (3-epoxypropyloxy)propyltrimethoxysilane, and the balance is deionized water.
[0130] 4. Then, the aluminum alloy substrate with the multilayer structure is placed in an oven and baked at 100° C. for 30 minutes to obtain the alkali-resistant aluminum alloy.
[0131] Example 3
[0132] This embodiment provides an alkali-resistant aluminum alloy, and the preparation process steps are as follows:
[0133] 1. Same as the step in Example 1.
[0134] 2. The dyed aluminum alloy substrate was placed in deionized water at 96° C. for hydration reaction for 10 minutes to obtain a first sealing layer.
[0135] 3. Immerse the aluminum alloy after the first sealing into a water-based sealing liquid for sealing. The sealing time is 3 minutes and the sealing temperature is 30°C.
[0136] Water-based sealing liquid composition: 15% phenyltrimethoxysilane, 15% nano-SiO 2 Sol, 8% ethyl orthosilicate, 10% (3-epoxypropyloxy)propyltrimethoxysilane, and the balance is deionized water.
[0137] 4. Then, the aluminum alloy substrate with the multilayer structure is placed in an oven and baked at 150° C. for 20 min to obtain the alkali-resistant aluminum alloy.
[0138] Example 4
[0139] This embodiment provides an alkali-resistant aluminum alloy, and the preparation process steps are as follows:
[0140] 1. Same as the step in Example 1.
[0141] 2. The dyed aluminum alloy substrate was placed in deionized water at 96° C. for hydration reaction for 10 minutes to obtain a first sealing layer.
[0142] 3. Immerse the aluminum alloy after the first sealing into a water-based sealing liquid for sealing. The sealing time is 8 minutes and the sealing temperature is 30°C.
[0143] Water-based sealing liquid composition: 5% phenyltrimethoxysilane, 10% nano-SiO 2 Sol, 5% ethyl orthosilicate, 5% (3-epoxypropyloxy)propyltrimethoxysilane, and the balance is deionized water.
[0144] 4. Then, the aluminum alloy substrate with the multilayer structure is placed in an oven and baked at 120° C. for 15 min to obtain the alkali-resistant aluminum alloy.
[0145] Example 5
[0146] This embodiment provides an alkali-resistant aluminum alloy, and the preparation process steps are as follows:
[0147] 1. Same as the step in Example 1.
[0148] 2. The dyed aluminum alloy substrate was placed in deionized water at 96° C. for hydration reaction for 5 minutes to obtain the first sealing layer.
[0149] 3. Immerse the aluminum alloy after the first sealing into a water-based sealing liquid for sealing. The sealing time is 5 minutes and the sealing temperature is 30°C.
[0150] Water-based sealing liquid composition: 10% phenyltrimethoxysilane, 15% nano-SiO 2 Sol, 3% ethyl orthosilicate, 5% (3-epoxypropyloxy)propyltrimethoxysilane, and the balance is deionized water.
[0151] 4. Then, the aluminum alloy substrate with the multilayer structure is placed in an oven and baked at 100° C. for 40 minutes to obtain the alkali-resistant aluminum alloy.
[0152] Example 6
[0153] This embodiment provides an alkali-resistant aluminum alloy, and the preparation process steps are as follows:
[0154] 1. Same as the step in Example 1.
[0155] 2. The dyed aluminum alloy substrate was placed in deionized water at 96° C. for hydration reaction for 10 minutes to obtain a first sealing layer.
[0156] 3. Immerse the aluminum alloy after the first sealing into a water-based sealing liquid for sealing. The sealing time is 8 minutes and the sealing temperature is 30°C.
[0157] Water-based sealing liquid composition: 5% phenyltrimethoxysilane, 15% nano-SiO 2 Sol, 8% ethyl orthosilicate, 10% (3-epoxypropyloxy)propyltrimethoxysilane, and the balance is deionized water.
[0158] 4. Then, the aluminum alloy substrate with the multilayer structure is placed in an oven and baked at 100° C. for 20 minutes to obtain the alkali-resistant aluminum alloy.
[0159] Example 7
[0160] This embodiment provides an alkali-resistant aluminum alloy, and the preparation process steps are as follows:
[0161] 1. Same as the step in Example 1.
[0162] 2. The dyed aluminum alloy substrate was placed in deionized water at 96° C. for hydration reaction for 5 minutes to obtain the first sealing layer.
[0163] 3. Immerse the aluminum alloy after the first sealing in a water-based sealing liquid for sealing. The sealing time is 10 minutes and the sealing temperature is 30°C.
[0164] Water-based sealing liquid composition: 15% phenyltrimethoxysilane, 15% nano-SiO 2 Sol, 8% ethyl orthosilicate, 10% (3-epoxypropyloxy)propyltrimethoxysilane, and the balance is deionized water.
[0165] 4. Then, the aluminum alloy substrate with the multilayer structure is placed in an oven and baked at 180° C. for 20 min to obtain the alkali-resistant aluminum alloy.
[0166] Example 8
[0167] This embodiment provides an alkali-resistant aluminum alloy, and the preparation process steps are as follows:
[0168] 1. Same as the step in Example 1.
[0169] 2. The dyed aluminum alloy substrate was placed in deionized water at 96° C. for hydration reaction for 1 minute to obtain the first sealing layer.
[0170] 3. Immerse the aluminum alloy after the first sealing into a water-based sealing liquid for sealing. The sealing time is 3 minutes and the sealing temperature is 30°C.
[0171] Water-based sealing liquid composition: 15% phenyltrimethoxysilane, 15% nano-SiO 2 Sol, 8% ethyl orthosilicate, 10% (3-epoxypropyloxy)propyltrimethoxysilane, and the balance is deionized water.
[0172] 4. Then, the aluminum alloy substrate with the multilayer structure is placed in an oven and baked at 150° C. for 20 min to obtain the alkali-resistant aluminum alloy.
[0173] Example 9
[0174] This embodiment provides an alkali-resistant aluminum alloy, and the preparation process steps are as follows:
[0175] 1. Same as the step in Example 1.
[0176] 2. The dyed aluminum alloy substrate was placed in deionized water at 96° C. for hydration reaction for 10 minutes to obtain a first sealing layer.
[0177] 3. Immerse the aluminum alloy after the first sealing into a water-based sealing liquid for sealing. The sealing time is 3 minutes and the sealing temperature is 30°C.
[0178] Water-based sealing liquid composition: 20% phenyltrimethoxysilane, 15% nano-SiO 2 Sol, 5% ethyl orthosilicate, 8% (3-epoxypropyloxy)propyltrimethoxysilane, and the balance is deionized water.
[0179] 4. Then, the aluminum alloy substrate with the multilayer structure is placed in an oven and baked at 150° C. for 20 min to obtain the alkali-resistant aluminum alloy.
[0180] Comparative Example 1
[0181] This comparative example provides an aluminum alloy. The difference from Example 1 is that step 2 is omitted, and the remaining steps are the same as those in Example 1, which will not be repeated here.
[0182] Comparative Example 2
[0183] This comparative example provides an aluminum alloy. The difference from Example 1 is that step 3 is omitted, and the remaining steps are the same as those in Example 1, which will not be repeated here.
[0184] Test Example 1
[0185] The aluminum alloys obtained in the examples and comparative examples were observed for appearance and tested using an alkaline kitchen detergent.
[0186] Spray the sample with a strong kitchen stain remover (Green Umbrella), wipe it with a rag / gauze at a force of 10N for 30s, and observe whether the coating cracks or peels off from the bottom plate. The test results are shown in Table 1 below.
[0187] Table 1
[0188]
[0189]
[0190] The aluminum alloys obtained in Examples 1-6 and Example 10 had good appearance, and showed no obvious discoloration in the alkaline kitchen detergent resistance test.
[0191] In Example 7, due to the high baking temperature, the color of the pigment in the coloring layer changed under high temperature. In Example 8, the primary sealing time was too short, and part of the pigment dissolved in the water-based sealing liquid during the secondary sealing process, causing the color to become lighter. In Example 9, due to the high solid content of the water-based sealing liquid, the coating after curing had undesirable phenomena such as paint blasting, and discoloration in the alkali resistance test.
[0192] After the process of comparative example 1 was completed, the color changed because the pigment was dissolved by the sealing liquid; in the alkali resistance test of comparative example 2, poor decolorization occurred.
[0193] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. An alkali-resistant aluminum alloy, characterized in that: It includes an aluminum alloy substrate and a multilayer structure formed on the surface of the aluminum alloy substrate; The multilayer structure comprises a porous layer and a sealing layer which are stacked; The sealing layer comprises a first sealing layer and a second sealing layer which are stacked; The second sealing layer is made of silicon dioxide.
2. The alkali-resistant aluminum alloy according to claim 1, characterized in that: The material of the porous layer is porous aluminum oxide; Preferably, the thickness of the porous layer is 0.5 μm to 10 μm; Preferably, the material of the first sealing layer is aluminum oxide; Preferably, the thickness of the first sealing layer is 1 μm to 3 μm.
3. The alkali-resistant aluminum alloy according to claim 1, characterized in that: The thickness of the second sealing layer is 3 μm to 5 μm.
4. The alkali-resistant aluminum alloy according to any one of claims 1 to 3, characterized in that: The multilayer structure comprises a porous layer, a coloring layer and a sealing layer; The colored layer is formed in the microporous structure inside the porous layer; The sealing layer is formed on the surface of the colored layer or the surface of the porous layer; Preferably, the material of the aluminum alloy substrate includes 5 series aluminum alloy or 6 series aluminum alloy.
5. A process for preparing the alkali-resistant aluminum alloy according to any one of claims 1 to 4, characterized in that: The porous layer is generated on the surface of the aluminum alloy substrate by an anodic oxidation process, and the porous layer is sealed once and twice to obtain the alkali-resistant aluminum alloy.
6. The preparation process according to claim 5, characterized in that: The process of one-time sealing includes: The aluminum alloy substrate with the porous layer is subjected to a hydration reaction in deionized water to obtain a first sealing layer; Preferably, the temperature of the hydration reaction is 95°C to 98°C; Preferably, the hydration reaction time is 5 min to 10 min.
7. The preparation process according to claim 5, characterized in that: The secondary sealing process includes: The aluminum alloy substrate with the first sealing layer is immersed in a sealing liquid for sealing, and then cured to obtain the second sealing layer; Preferably, the sealing temperature is 20°C to 40°C; Preferably, the sealing time is 3 minutes to 10 minutes.
8. The preparation process according to claim 7, characterized in that: The sealing liquid is a water-based sealing liquid or a solvent-based sealing liquid; Preferably, the water-based sealing liquid comprises 5wt.% to 15wt.% of phenyltrimethoxysilane, 5wt.% to 15wt.% of silica sol, 3wt.% to 8wt.% of tetraethyl orthosilicate, 5wt.% to 10wt.% of (3-epoxypropyl)propyltrimethoxysilane, and the balance is deionized water; Preferably, the curing temperature is 80°C to 150°C; Preferably, the curing time is 5 min to 20 min.
9. The preparation process according to claim 8, characterized in that: The solvent-based sealing liquid comprises 20 wt.% to 35 wt.% of methylphenyl silicone resin, 15 wt.% to 25 wt.% of acrylic modified silicone resin, 5 wt.% to 10 wt.% of silica sol, 2 wt.% to 3 wt.% of leveling agent, 1 wt.% to 2 wt.% of alkylphenol polyoxyethylene ether, and the balance is ethylene glycol butyl ether; Preferably, the curing temperature is 120°C to 150°C; Preferably, the curing time is 20 min to 40 min.
10. The preparation process according to any one of claims 5 to 9, characterized in that: Before the anodizing process is performed, the method further includes a pre-treatment process of the aluminum alloy substrate; Preferably, the pre-treatment process includes degreasing, alkali treatment, primary neutralization, polishing and secondary neutralization performed in sequence.