Local preparation method of hard oxide film in inner cavity of complex empennage assembly

Through reasonable process flow and solution formula, the ablation and breakdown problems in the local preparation of hard oxide film in the cavity of complex tail components are solved, the processing efficiency and membrane performance are improved, and the hard oxide film layer of complex components is realized Regeneration and stability of membrane properties.

CN118910691APending Publication Date: 2024-11-08HENAN NORTHERN HONGYANG ELECTROMECHANICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410982501.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The hard oxide film in the cavity of the complex tail wing assembly is easily ablated and broken down during the local preparation process, resulting in the scrapping of the entire component. The traditional painting protection process is inefficient and is not suitable for complex components, making it difficult to achieve uniform regeneration of local film layers.

Method used

Adopt reasonable process flow and solution formula, including hot water soaking, effluent washing, hard anodizing, sealing treatment and recycling steps, and ensure conductivity and film quality by controlling process parameters such as voltage step power supply and temperature. Composite additives to improve the corrosion resistance and hardness of the film layer.

Benefits of technology

Improve processing efficiency, realize the regeneration of the hard oxide film layer in specific parts of complex components, ensure the stability and success rate of film layer performance, solve the problems of ablation and breakdown, and the efficiency of traditional paint protection is increased by 2~ 3 times, the success rate is more than 95%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910691A_ABST
    Figure CN118910691A_ABST
Patent Text Reader

Abstract

The invention discloses a local preparation method of a hard oxidation film in an inner cavity of a complex empennage assembly. The method comprises the steps of hanging tool loading, hot water soaking, bright dipping and washing, hard anodic oxidation, sealing treatment of the oxidized empennage assembly, recycling, pure water washing, water blowing, drying and performance inspection. According to the local preparation method of the hard oxidation film, through the method of reasonable process route, reasonable process parameter control, conductive threshold determination, stable voltage selection and soft start step power supply, starting over-current tripping is avoided, and the quality of the hard anodic oxidation film layer of the inner cavity of the empennage assembly can be optimally guaranteed; according to the invention, the regeneration of the hard oxidation film layer at the specific part of a complex part can be realized, the performance of the film layer at other parts is not influenced, the process problem that the whole empennage assembly is scrapped due to the fact that the film layer is extremely easy to ablate and break down in the production operation process is solved, the corrosion resistance of the film layer meets the relevant standard requirement, and the hardness of the film layer is not lower than 350HV0.05.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The patent of this invention relates to metal surface treatment technology, specifically to a method for locally preparing a hard oxide film in the inner cavity of a complex tail wing component. Background Art

[0002] Among the surface technologies of aluminum and aluminum alloys, anodizing is a widely and successfully applied technology. A thin oxide film is formed on the surface of aluminum and aluminum alloys by electrolytic oxidation, which changes the surface state and performance of aluminum and aluminum alloy parts. The hard anodized film of aluminum has high hardness, good lubrication effect, corrosion resistance and wear resistance, and is often used in aerospace and equipment aircraft aluminum alloy parts under friction.

[0003] Due to the problem of parts interference, a certain intelligent flight product needs to cut several planes on the inner wall of the installation groove of the complex inner cavity tail wing assembly after hard oxidation, and the cut plane parts also need to be repaired with local oxide film. The traditional repair process is paint protection, which has a long operation cycle and low processing efficiency. Affected by the size and complexity of the parts, parts with extremely complex inner cavities cannot be protected by paint and subsequent cleaning. The surface film of the parts is easily damaged during the removal of the protective paint, and the edge protective paint is prone to leakage. The tail wing assembly with complex structure, multiple blind holes and multiple installation slots is made of 7A04, which is an ultra-high strength aluminum alloy of the Al-Zn-Mg-Cu series. It has high quality requirements and high processing costs. The preparation of local film layers is very likely to cause ablation and breakdown, making the entire tail wing assembly scrapped. How to make the non-oxide film part form a uniform oxide film after reprocessing without affecting the film quality of other parts of the workpiece to ensure the functional requirements of the product has become a key problem that needs to be solved urgently. Summary of the invention

[0004] In view of the above problems, the purpose of the present invention is to provide a method for local preparation of hard oxide film in the inner cavity of a complex tail wing component. This method regenerates the hard oxide film layer in the inner cavity of a complex tail wing component through reasonable process flow, solution formulation and construction parameters. The corrosion resistance and hardness of the film layer are equivalent to those of a single film formation performance test.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is: a method for locally preparing a hard oxide film in the inner cavity of a complex tail component, comprising the following steps: (1) Upper hanger: The installation angle between the hanger and the tail assembly is 35-50 degrees. The conductivity between the hanger rods is kept good. Plastic pads are added at the connection between the hanger rod and the tail assembly, and plastic caps are added to seal the blind holes. (2) Hot water immersion: Immerse the mounted tail wing assembly in hot water at a temperature of 65°C-75°C for 1-2 minutes. Alumina reacts with water to form boehmite, which expands the oxide film to seal the pores, improves the sealing of the oxide film, and reduces the dissolution rate of the hard oxide film in subsequent processes. (3) Polishing and washing: immerse the tail wing assembly in a polishing solution for 30 seconds to dissolve the oxide film on the repaired surface of the tail wing assembly to expose the active metal interface, wash away the residual chemical agent on the surface of the workpiece, and prevent contamination of the hard anodizing tank liquid; the polishing solution is composed of: 250g / L-300g / L nitric acid, 10g / L-15g / L urea; (4) Hard anodizing: After washing with pure water, immerse the tail wing assembly in a hard anodizing tank. Turn on the refrigeration device, compressed air stirring device and pulse power supply. Select the stable voltage mode and soft start step-by-step power supply. The voltage of each piece is 5V for 5 minutes. The voltage is increased to 10V for 10 minutes. The voltage is increased to 17V for 20 minutes. The oxidation time is 35 minutes in total. The composition of the hard anodizing tank is as follows: concentrated sulfuric acid 200g / L-260g / L; citric acid 15g / L-25g / L; composite additives 10g / L-20g / L; temperature 1°C-5°C. (5) The oxidized tail wing assembly is sealed, and the sealing liquid composition is: 65g / L-75g / L potassium dichromate, the temperature is 85°C-90°C, and the duration is 15 minutes, so as to improve the corrosion resistance of the film layer of the hard oxide film; (6) Recovery: The sealing liquid is recovered for reuse, while reducing the Cr6 + content; (7) Pure water washing: The conductivity of the pure water used is not more than 50 μs / cm, and the immersion time is 30 seconds to clean the salt chemicals on the surface of the tail wing assembly and improve the film quality of the hard oxide film; (8) Blowing and drying: remove moisture from the surface of the tail wing assembly to eliminate water flow marks; (9) Performance test: The film thickness of the hard oxide film is required to be between 30 μm and 45 μm, and its appearance, corrosion resistance and hardness are tested in accordance with relevant standards.

[0006] Furthermore, the composite additive in step (4) is composed of a polyol mixture and an organic acid, wherein the polyol mixture is prepared by mixing two of sorbitol, neopentyl glycol, diethylene glycol and butanediol in a ratio of 1:1.

[0007] The organic acid is prepared by dissolving one of adipic acid, malic acid and succinic acid.

[0008] The composite additive is prepared by a polyol mixture: organic acid = 1:2, the polyol mixture content is 3g / L-7g / L, and the organic acid content is 6g / L-14g / L.

[0009] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) It solves the process problem that the hard oxide film in the cavity of the complex tail component is easily ablated and punctured during the local preparation process, which makes the entire tail component scrapped. (2) It realizes the process method innovation of regenerating the hard oxide film layer in the specific part of the complex component, and the film performance of other parts is not affected, and there is no overlap between the specific part and other parts. (3) Through a reasonable process route and reasonable control of process parameters, the conductive threshold is determined, the voltage is stabilized, and the soft start step power supply method is selected to avoid starting overcurrent tripping, which can optimally ensure the quality of the anodized film layer in the cavity of the tail component. (4) The processing efficiency is 2 to 3 times higher than that of traditional paint protection. Traditional paint protection is not suitable for complex components. The success rate of local film preparation is more than 95%, ensuring that the performance of the hard oxide film layer of the tail component is stable and good, and meeting the product design index requirements. The method of the present invention is not only suitable for the local preparation of the hard oxide film in the cavity of the complex tail component, but can also be extended to the regeneration of the hard oxide film layer of similar components. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 It is a process flow chart of the present invention; Figure 2 This is a diagram showing the effect of preparing a hard oxide film locally in the inner cavity of the tail wing assembly of the present invention. DETAILED DESCRIPTION

[0011] The technical solution of the present invention is clearly and completely described below in conjunction with the accompanying drawings and specific embodiments.

[0012] Reference Figure 1 As shown, a method for locally preparing a hard oxide film in the inner cavity of a complex tail wing component comprises the following steps: (1) Upper hanger: The installation angle between the hanger and the tail assembly is 35-50 degrees. The conductivity between the hanger rods is kept good. Plastic pads are added at the connection between the hanger rod and the tail assembly, and plastic caps are added to seal the blind holes. (2) Hot water immersion: Immerse the mounted tail wing assembly in hot water at a temperature of 65°C-75°C for 1-2 minutes. Alumina reacts with water to form boehmite, which expands the oxide film to seal the pores, improves the sealing of the oxide film, and reduces the dissolution rate of the hard oxide film in subsequent processes. (3) Polishing and washing: immerse the tail wing assembly in a polishing solution for 30 seconds to dissolve the oxide film on the repaired surface of the tail wing assembly to expose the active metal interface, wash away the residual chemical agent on the surface of the workpiece, and prevent contamination of the hard anodizing tank liquid; the polishing solution is composed of: 250g / L-300g / L nitric acid, 10g / L-15g / L urea; (4) Hard anodizing: After washing with pure water, immerse the tail wing assembly in a hard anodizing tank. Turn on the refrigeration device, compressed air stirring device and pulse power supply. Select the stable voltage mode and soft start step-by-step power supply. The voltage of each piece is 5V for 5 minutes. The voltage is increased to 10V for 10 minutes. The voltage is increased to 17V for 20 minutes. The oxidation time is 35 minutes in total. The composition of the hard anodizing tank is as follows: concentrated sulfuric acid 200g / L-260g / L; citric acid 15g / L-25g / L; composite additives 10g / L-20g / L; temperature 1°C-5°C. (5) The oxidized tail wing assembly is sealed, and the sealing liquid composition is: 65g / L-75g / L potassium dichromate, the temperature is 85°C-90°C, and the duration is 15 minutes, so as to improve the corrosion resistance of the film layer of the hard oxide film; (6) Recovery: The sealing liquid is recovered for reuse, while reducing the Cr6 content of a type of pollutant in the wastewater. + content; (7) Pure water washing: The conductivity of the pure water used is not more than 50 μs / cm, and the immersion time is 30 seconds to clean the salt chemicals on the surface of the tail wing assembly and improve the film quality of the hard oxide film; (8) Blowing and drying: remove moisture from the surface of the tail wing assembly to eliminate water flow marks; (9) Performance test: The film thickness of the hard oxide film is required to be between 30 μm and 45 μm, and its appearance, corrosion resistance and hardness are tested in accordance with relevant standards.

[0013] The composite additive in step (4) is composed of a polyol mixture and an organic acid, wherein the polyol mixture is prepared by mixing two of sorbitol, neopentyl glycol, diethylene glycol and butanediol in a ratio of 1:1.

[0014] The organic acid is prepared by dissolving one of adipic acid, malic acid and succinic acid.

[0015] The composite additive is prepared by a polyol mixture: organic acid = 1:2, the polyol mixture content is 3g / L-7g / L, and the organic acid content is 6g / L-14g / L.

[0016] A plastic pad is added at the connection between the hanging rod and the tail wing assembly to avoid overcurrent tripping during the hard anodizing in step (4), which can better protect the tail wing assembly from being burned due to the moment of rectifier startup; the blind hole is sealed with a plastic cap to prevent the blind hole seepage from being difficult to discharge and causing corrosion of the original oxide film layer. Example 1

[0017] The composition of the hard anodizing tank is as follows: concentrated sulfuric acid 200g / L; citric acid 15g / L; composite additive 10g / L; temperature is 1°C. Put the workpiece into the prepared hard anodizing tank, turn on the refrigeration device, compressed air stirring device and pulse power switch, select the stable voltage mode, soft start step power supply, each voltage is 5V, duration 5min→10V, duration 10min→17V, duration 20min, oxidation time is 35min in total. The rest of the steps are the same. Example 2

[0018] The composition of the hard anodizing tank is: concentrated sulfuric acid 230g / L; citric acid 20g / L; composite additives 15g / L; temperature is 3°C. Put the workpiece into the prepared hard anodizing tank, turn on the refrigeration device, compressed air stirring device and pulse power switch, select the stable voltage mode, soft start step power supply, each voltage is 5V, duration 5min→10V, duration 10min→17V, duration 20min, oxidation time is 35min in total. The rest of the steps are the same. Example 3

[0019] The composition of the hard anodizing tank is as follows: concentrated sulfuric acid 260g / L; citric acid 25g / L; composite additives 20g / L; temperature is 5°C. Put the workpiece into the prepared hard anodizing tank, turn on the refrigeration device, compressed air stirring device and pulse power switch, select the stable voltage mode, soft start step power supply, each voltage is 5V, duration 5min→10V, duration 10min→17V, duration 20min, oxidation time is 35min in total. The rest of the steps are the same. Implementation Effect

[0020] The above process is used for the tail wing component of a certain flight intelligent product. After hard anodizing treatment, the hardness and corrosion resistance test is carried out in accordance with the provisions of GB / T9790-1988 and WJ538-2007. The microhardness of the film layer formed in the inner cavity is not less than 350HV. 0.05 ,The drip corrosion resistance test is not less than 32min (under the test temperature of 22℃~26℃), and the target test results meet the tactical index requirements.

[0021] The process method described in the present invention solves the following problems: (1) It solves the process problem that the hard oxide film in the cavity of the complex tail component is easily ablated and punctured during the local preparation process, which makes the entire tail component scrapped. (2) It realizes the process method innovation of regenerating the hard oxide film layer in the specific part of the complex component, and the film performance of other parts is not affected, and there is no overlap between the specific part and other parts. (3) Through a reasonable process route and reasonable control of process parameters, the conductive threshold is determined, the voltage is stabilized, and the soft start step power supply method is selected to avoid starting overcurrent tripping, which can optimally ensure the quality of the anodized film layer in the cavity of the tail component. (4) The processing efficiency is improved by 2 to 3 times compared with traditional paint protection. Traditional paint protection is not suitable for complex parts. The success rate of local film preparation is more than 95%, ensuring that the performance of the hard oxide film layer of the tail component is stable and good, and meeting the product design index requirements.

[0022] The above invention is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention can be modified and varied. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.

Claims

1. A method for local preparation of hard oxide film in the inner cavity of a complex tail wing component. Features: The following steps are involved: (1) Upper hanger: The installation angle between the hanger and the tail assembly is 35-50 degrees. The conductivity between the hanger rods is kept good. Plastic pads are added at the connection between the hanger rod and the tail assembly, and plastic caps are added to seal the blind holes. (2) Hot water immersion: Immerse the mounted tail wing assembly in hot water at a temperature of 65°C-75°C for 1-2 minutes. Alumina reacts with water to form boehmite, which expands the oxide film to seal the pores, improves the sealing of the oxide film, and reduces the dissolution rate of the hard oxide film in subsequent processes. (3) Polishing and washing: immerse the tail wing assembly in a polishing solution for 30 seconds to dissolve the oxide film on the repaired surface of the tail wing assembly to expose the active metal interface, wash away the residual chemical agent on the surface of the workpiece, and prevent contamination of the hard anodizing tank liquid; the polishing solution is composed of: 250g / L-300g / L nitric acid, 10g / L-15g / L urea; (4) Hard anodizing: After washing with pure water, immerse the tail wing assembly in a hard anodizing tank. Turn on the refrigeration device, compressed air stirring device and pulse power supply. Select the stable voltage mode and soft start step-by-step power supply. The voltage of each piece is 5V for 5 minutes. The voltage is increased to 10V for 10 minutes. The voltage is increased to 17V for 20 minutes. The oxidation time is 35 minutes in total. The composition of the hard anodizing tank is as follows: concentrated sulfuric acid 200g / L-260g / L; citric acid 15g / L-25g / L; composite additives 10g / L-20g / L; temperature 1°C-5°C. (5) The oxidized tail wing assembly is sealed with sealing liquid. Composition: potassium dichromate 65g / L-75g / L, temperature 85℃-90℃, duration 15min, to improve the corrosion resistance of the hard oxide film; (6) Recovery: The sealing liquid is recovered for reuse, while reducing the Cr6 + content; (7) Pure water washing: The conductivity of the pure water used is not more than 50 μs / cm, and the immersion time is 30 seconds to clean the salt chemicals on the surface of the tail wing assembly and improve the film quality of the hard oxide film; (8) Blowing and drying: remove moisture from the surface of the tail wing assembly to eliminate water flow marks; (9) Performance test: The film thickness of the hard oxide film is required to be between 30 μm and 45 μm, and its appearance, corrosion resistance and hardness are tested in accordance with relevant standards.

2. The local preparation method of the hard oxide film according to claim 1, Features: The composite additive in step (4) is composed of a polyol mixture and an organic acid, wherein the polyol mixture is prepared by mixing two of sorbitol, neopentyl glycol, diethylene glycol and butanediol in a ratio of 1:

1.

3. The local preparation method of hard oxide film according to claim 2, Features: The organic acid is prepared by dissolving one of adipic acid, malic acid and succinic acid.

4. The method for preparing a local hard oxide film according to claim 3, Features: The composite additive is prepared by a polyol mixture: organic acid = 1:2, the polyol mixture content is 3g / L-7g / L, and the organic acid content is 6g / L-14g / L.