Degradable high-elasticity polylactic acid composite fiber and preparation method thereof

Through the preparation method of modified composite fibers of polylactic acid and nanocellulose and other materials, the difficulties in optimizing degradation performance of polylactic acid fibers are solved, and the coordinated improvement of high elasticity and high degradation performance is achieved, which is suitable for a wide range of applications of environmentally friendly products.

CN118910761APending Publication Date: 2024-11-08SHENZHEN ESUN IND +1
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411087029.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-08

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a degradable high-elasticity polylactic acid composite fiber and a preparation method thereof, and belongs to the technical field of polylactic acid fiber preparation, the degradable high-elasticity polylactic acid composite fiber comprises modified polylactic acid, nano cellulose, citrate, nano zinc oxide, polyethylene glycol and polyvinyl alcohol; the preparation method comprises the following steps: mixing modified polylactic acid with nano cellulose, citrate, nano zinc oxide, polyethylene glycol and polyvinyl alcohol in a high-speed mixer to obtain a spinning material; melting the obtained spinning material, and spinning by a spinning machine to obtain fibers; cooling and curing the obtained fiber, and stretching; and winding and collecting the stretched fibers to form finished fibers. The modified polylactic acid is prepared, the polylactic acid fiber with high degradation performance is prepared by adopting the modified polylactic acid and a specific polylactic acid fiber spinning material formula, and meanwhile, the high elasticity of the product is guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polylactic acid fiber preparation, and specifically relates to a degradable high-elastic polylactic acid composite fiber and a preparation method thereof. Background Art

[0002] With the increasing awareness of environmental protection, the environmental problems of traditional synthetic fibers have gradually become prominent, and degradable materials have become the key to solving this problem. Polylactic acid (PLA) fiber, as a biodegradable material, has attracted much attention in recent years. However, pure PLA fiber still needs to be improved in some aspects, such as elasticity and heat resistance. Therefore, the development of high-performance degradable polylactic acid composite fibers has become the focus of research.

[0003] The preparation method of degradable polylactic acid composite fiber is mainly to improve its performance by compounding PLA with other biocompatible materials. These composite materials can be elastomers, plasticizers or other biodegradable materials. Through specific preparation processes, such as melt blending, spinning, etc., degradable polylactic acid composite fibers with good elasticity and other required properties can be obtained. This technology is environmentally friendly. The composite fiber inherits the biodegradability of PLA and can be completely decomposed in the natural environment, reducing pollution to the environment. Through composite modification, the elasticity, heat resistance, mechanical properties, etc. of the fiber have been significantly improved, broadening its application range. With the increasing demand of consumers for environmentally friendly products, degradable polylactic acid composite fibers have broad application prospects in the fields of textiles, packaging, and medical treatment. Especially in occasions requiring high elasticity and environmental performance, such as sportswear, medical dressings, etc., this composite fiber will have huge market competitiveness.

[0004] Although polylactic acid fiber itself is degradable, the pursuit of higher degradation performance may affect the elasticity of the fiber. This is because some methods to improve degradation performance, such as adding specific biodegradation agents or changing the fiber structure, may affect the molecular chain structure and degree of cross-linking of the fiber, thereby affecting its elasticity. Therefore, how to improve its degradation performance while maintaining the elasticity of the fiber is a difficulty in current research. The degradation rate of polylactic acid fiber is affected by many factors, such as temperature, humidity, and microbial species. Under certain conditions, the degradation rate may be too fast or too slow, which will affect the service life and performance of the fiber. Therefore, how to accurately control the degradation rate of polylactic acid composite fibers is also a problem that needs to be solved.

[0005] In summary, degradable polylactic acid composite fibers and their preparation methods have significant advantages in terms of environmental protection and performance. However, how to optimize the degradation performance while maintaining the elasticity of the fibers is still the focus of current research. With the continuous advancement of technology and the promotion of the market, it is believed that this technology will continue to improve and play a greater role in the future. Summary of the invention

[0006] In order to solve the above problems, the present invention mainly optimizes from the perspective of formulation and material modification, and provides a degradable high-elastic polylactic acid composite fiber and a preparation method thereof. The specific scheme is as follows:

[0007] Firstly, the present invention provides a degradable high-elastic polylactic acid composite fiber, comprising modified polylactic acid, nano cellulose, citrate, nano zinc oxide, polyethylene glycol and polyvinyl alcohol.

[0008] Preferably, the components in the composite fiber are calculated by weight as follows: 100 parts of modified polylactic acid, 1-3 parts of nanocellulose, 3-5 parts of citrate, 2-4 parts of nano zinc oxide, 2-4 parts of polyethylene glycol, and 2-4 parts of polyvinyl alcohol.

[0009] Preferably, the nanocellulose fibers have a diameter of 3-25 nm and a fiber length of 50-500 nm.

[0010] The present invention also provides a method for preparing the above-mentioned degradable high-elastic polylactic acid composite fiber, comprising the following steps:

[0011] S1, taking modified polylactic acid, nanocellulose, citrate, nano zinc oxide, polyethylene glycol, and polyvinyl alcohol and mixing them in a high-speed mixer to obtain a spinning material;

[0012] S2, melting the obtained spinning material, and spinning it through a spinning machine to obtain fibers;

[0013] S3. After the obtained fiber is cooled and solidified, it is stretched; the stretched fiber is wound and collected to form a finished fiber.

[0014] Preferably, in step S3, the melting temperature is 160-200° C., the spinning temperature is 185-195° C., and the spinning speed is 800-1000 m / min.

[0015] Preferably, the stretching ratio in step S4 is 2.5-3.5 times, and the stretching temperature is 80-90°C.

[0016] Preferably, the preparation method of the modified polylactic acid comprises: dissolving the modifiers glutamic acid and chitosan in acidic water, adding polylactic acid, adjusting the pH and then heating for reaction, washing with water and drying after the reaction is completed to obtain the modified polylactic acid.

[0017] Preferably, in the modified polylactic acid preparation method, the mass ratio of glutamic acid to polylactic acid is 1:100.

[0018] Preferably, in the modified polylactic acid preparation method, the mass ratio of chitosan to polylactic acid is 5:100.

[0019] Preferably, in the modified polylactic acid preparation method, the pH of the acidic water is 5.5; and the pH is adjusted to 5.5.

[0020] Preferably, in the modified polylactic acid preparation method, the heating reaction is a stirring reaction, the reaction temperature is 50° C., and the reaction time is 4 hours.

[0021] Beneficial Effects

[0022] The invention prepares modified polylactic acid, adopts the modified polylactic acid and a specific polylactic acid fiber spinning material formula, prepares polylactic acid fiber with high degradation performance, and at the same time ensures the high elasticity of the product. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0024] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.

[0025] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified. The details are as follows:

[0026] Polylactic acid particles: NatureWorks 4032D PLA, molecular weight 150,000 g / mol;

[0027] Nanocellulose: Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., fiber diameter: 15-25nm (nanoscale), fiber length: 200-300nm;

[0028] Chitosan (CAS 9012-76-4, 99%): Jiangsu Duoyang Bioengineering Technology Co., Ltd.;

[0029] L-Glutamic acid: Manufacturer: Xi'an Tianmao Chemical Co., Ltd., high-grade pure GR;

[0030] Citrate esters: tributyl citrate, dibutyl citrate;

[0031] Nano zinc oxide: Kramar, 99.9%, 30±10nm;

[0032] Polyethylene glycol: polyethylene glycol 400 (PEG-400), Shanghai Zhanyun Chemical Co., Ltd.;

[0033] Polyvinyl alcohol: Ron's reagent, low viscosity type.

[0034] Example 1 A method for preparing a degradable high-elastic polylactic acid composite fiber:

[0035] S1, dissolving the modifiers glutamic acid and chitosan in acidic water, adding polylactic acid, adjusting the pH and heating to react, washing with water and drying after the reaction to obtain modified polylactic acid;

[0036] S2, taking the modified polylactic acid obtained in step S1 and mixing it with nano cellulose, citrate, nano zinc oxide, polyethylene glycol and polyvinyl alcohol to obtain a spinning material;

[0037] S3, melting the obtained spinning material, and spinning it through a spinning machine to obtain fibers;

[0038] S4. After the obtained fiber is cooled and solidified, it is stretched; the stretched fiber is wound and collected to form a finished fiber.

[0039] The mass ratio of glutamic acid to polylactic acid in step S1 is 1:100.

[0040] The mass ratio of chitosan to polylactic acid in step S1 is 5:100.

[0041] The acidic water in step S1 has a pH of 5.5; the pH is adjusted to 5.5.

[0042] In step S1, the heating reaction was carried out and the stirring reaction was carried out at a temperature of 50° C. and a reaction time of 4 h.

[0043] The components in the composite fiber are calculated by weight as follows: 100 parts of modified polylactic acid, 1 part of nanocellulose, 3 parts of citrate, 2 parts of nano zinc oxide, 2 parts of polyethylene glycol, and 2 parts of polyvinyl alcohol.

[0044] In step S3, the melting temperature is 160° C., the spinning temperature is 185° C., and the spinning speed is 800 m / min.

[0045] The stretching ratio in step S4 is 2.5 times and the stretching temperature is 80°C.

[0046] Example 2 A method for preparing a degradable high-elastic polylactic acid composite fiber:

[0047] S1, dissolving the modifiers glutamic acid and chitosan in acidic water, adding polylactic acid, adjusting the pH and heating to react, washing with water and drying after the reaction to obtain modified polylactic acid;

[0048] S2, taking the modified polylactic acid obtained in step S1 and mixing it with nano cellulose, citrate, nano zinc oxide, polyethylene glycol and polyvinyl alcohol to obtain a spinning material;

[0049] S3, melting the obtained spinning material, and spinning it through a spinning machine to obtain fibers;

[0050] S4. After the obtained fiber is cooled and solidified, it is stretched; the stretched fiber is wound and collected to form a finished fiber.

[0051] The mass ratio of glutamic acid to polylactic acid in step S1 is 3:100.

[0052] The mass ratio of chitosan to polylactic acid in step S1 is 9:100.

[0053] The acidic water in step S1 has a pH of 5.5; the pH is adjusted to 5.5.

[0054] In step S1, the heating reaction was carried out and the stirring reaction was carried out at a temperature of 50° C. and a reaction time of 4 h.

[0055] The components in the composite fiber are calculated by weight as follows: 100 parts of modified polylactic acid, 1 part of nanocellulose, 3 parts of citrate, 2 parts of nano zinc oxide, 2 parts of polyethylene glycol, and 2 parts of polyvinyl alcohol.

[0056] In step S3, the melting temperature is 160° C., the spinning temperature is 185° C., and the spinning speed is 800 m / min.

[0057] The stretching ratio in step S4 is 2.5 times and the stretching temperature is 80°C.

[0058] Example 3 A method for preparing a degradable high-elastic polylactic acid composite fiber:

[0059] S1, dissolving the modifiers glutamic acid and chitosan in acidic water, adding polylactic acid, adjusting the pH and heating to react, washing with water and drying after the reaction to obtain modified polylactic acid;

[0060] S2, taking the modified polylactic acid obtained in step S1 and mixing it with nano cellulose, citrate, nano zinc oxide, polyethylene glycol and polyvinyl alcohol to obtain a spinning material;

[0061] S3, melting the obtained spinning material, and spinning it through a spinning machine to obtain fibers;

[0062] S4. After the obtained fiber is cooled and solidified, it is stretched; the stretched fiber is wound and collected to form a finished fiber.

[0063] The mass ratio of glutamic acid to polylactic acid in step S1 is 2:100.

[0064] The mass ratio of chitosan to polylactic acid in step S1 is 7:100.

[0065] The acidic water in step S1 has a pH of 5.5; the pH is adjusted to 5.5.

[0066] In step S1, the heating reaction was carried out and the stirring reaction was carried out at a temperature of 50° C. and a reaction time of 4 h.

[0067] The components in the composite fiber are calculated by weight as follows: 100 parts of modified polylactic acid, 1 part of nanocellulose, 3 parts of citrate, 2 parts of nano zinc oxide, 2 parts of polyethylene glycol, and 2 parts of polyvinyl alcohol.

[0068] In step S3, the melting temperature is 160° C., the spinning temperature is 185° C., and the spinning speed is 800 m / min.

[0069] The stretching ratio in step S4 is 2.5 times and the stretching temperature is 80°C.

[0070] Example 4 A method for preparing a degradable high-elastic polylactic acid composite fiber:

[0071] S1, dissolving the modifiers glutamic acid and chitosan in acidic water, adding polylactic acid, adjusting the pH and heating to react, washing with water and drying after the reaction to obtain modified polylactic acid;

[0072] S2, taking the modified polylactic acid obtained in step S1 and mixing it with nano cellulose, citrate, nano zinc oxide, polyethylene glycol and polyvinyl alcohol to obtain a spinning material;

[0073] S3, melting the obtained spinning material, and spinning it through a spinning machine to obtain fibers;

[0074] S4. After the obtained fiber is cooled and solidified, it is stretched; the stretched fiber is wound and collected to form a finished fiber.

[0075] The mass ratio of glutamic acid to polylactic acid in step S1 is 2:100.

[0076] The mass ratio of chitosan to polylactic acid in step S1 is 7:100.

[0077] The acidic water in step S1 has a pH of 5.5; the pH is adjusted to 5.5.

[0078] In step S1, the heating reaction was carried out and the stirring reaction was carried out at a temperature of 50° C. and a reaction time of 4 h.

[0079] The components in the composite fiber are calculated by weight as follows: 100 parts of modified polylactic acid, 3 parts of nanocellulose, 5 parts of citrate, 4 parts of nano zinc oxide, 4 parts of polyethylene glycol, and 4 parts of polyvinyl alcohol.

[0080] In step S3, the melting temperature is 160° C., the spinning temperature is 185° C., and the spinning speed is 800 m / min.

[0081] The stretching ratio in step S4 is 2.5 times and the stretching temperature is 80°C.

[0082] Example 5 A method for preparing a degradable high-elastic polylactic acid composite fiber:

[0083] S1, dissolving the modifiers glutamic acid and chitosan in acidic water, adding polylactic acid, adjusting the pH and heating to react, washing with water and drying after the reaction to obtain modified polylactic acid;

[0084] S2, taking the modified polylactic acid obtained in step S1 and mixing it with nano cellulose, citrate, nano zinc oxide, polyethylene glycol and polyvinyl alcohol to obtain a spinning material;

[0085] S3, melting the obtained spinning material, and spinning it through a spinning machine to obtain fibers;

[0086] S4. After the obtained fiber is cooled and solidified, it is stretched; the stretched fiber is wound and collected to form a finished fiber.

[0087] The mass ratio of glutamic acid to polylactic acid in step S1 is 2:100.

[0088] The mass ratio of chitosan to polylactic acid in step S1 is 7:100.

[0089] The acidic water in step S1 has a pH of 5.5; the pH is adjusted to 5.5.

[0090] In step S1, the heating reaction was carried out and the stirring reaction was carried out at a temperature of 50° C. and a reaction time of 4 h.

[0091] The components in the composite fiber are calculated by weight as follows: 100 parts of modified polylactic acid, 2 parts of nanocellulose, 4 parts of citrate, 3 parts of nano zinc oxide, 3 parts of polyethylene glycol, and 3 parts of polyvinyl alcohol.

[0092] In step S3, the melting temperature is 160° C., the spinning temperature is 185° C., and the spinning speed is 800 m / min.

[0093] The stretching ratio in step S4 is 2.5 times and the stretching temperature is 80°C.

[0094] Example 6 A method for preparing a degradable high-elastic polylactic acid composite fiber:

[0095] S1, dissolving the modifiers glutamic acid and chitosan in acidic water, adding polylactic acid, adjusting the pH and heating to react, washing with water and drying after the reaction to obtain modified polylactic acid;

[0096] S2, taking the modified polylactic acid obtained in step S1 and mixing it with nano cellulose, citrate, nano zinc oxide, polyethylene glycol and polyvinyl alcohol to obtain a spinning material;

[0097] S3, melting the obtained spinning material, and spinning it through a spinning machine to obtain fibers;

[0098] S4. After the obtained fiber is cooled and solidified, it is stretched; the stretched fiber is wound and collected to form a finished fiber.

[0099] The mass ratio of glutamic acid to polylactic acid in step S1 is 2:100.

[0100] The mass ratio of chitosan to polylactic acid in step S1 is 7:100.

[0101] The acidic water in step S1 has a pH of 6.0; the pH is adjusted to 6.0.

[0102] In step S1, the heating reaction and stirring reaction are performed at a temperature of 60° C. and a reaction time of 6 h.

[0103] The components in the composite fiber are calculated by weight as follows: 100 parts of modified polylactic acid, 2 parts of nanocellulose, 4 parts of citrate, 3 parts of nano zinc oxide, 3 parts of polyethylene glycol, and 3 parts of polyvinyl alcohol.

[0104] In step S3, the melting temperature is 200° C., the spinning temperature is 195° C., and the spinning speed is 1000 m / min.

[0105] The stretching ratio in step S4 is 3.5 times and the stretching temperature is 90°C.

[0106] Example 7 A method for preparing a degradable high-elastic polylactic acid composite fiber:

[0107] S1, dissolving the modifiers glutamic acid and chitosan in acidic water, adding polylactic acid, adjusting the pH and heating to react, washing with water and drying after the reaction to obtain modified polylactic acid;

[0108] S2, taking the modified polylactic acid obtained in step S1 and mixing it with nano cellulose, citrate, nano zinc oxide, polyethylene glycol and polyvinyl alcohol to obtain a spinning material;

[0109] S3, melting the obtained spinning material, and spinning it through a spinning machine to obtain fibers;

[0110] S4. After the obtained fiber is cooled and solidified, it is stretched; the stretched fiber is wound and collected to form a finished fiber.

[0111] The mass ratio of glutamic acid to polylactic acid in step S1 is 2:100.

[0112] The mass ratio of chitosan to polylactic acid in step S1 is 7:100.

[0113] The acidic water in step S1 has a pH of 6.0; the pH is adjusted to 5.5.

[0114] In step S1, the heating reaction was carried out and the stirring reaction was carried out at a temperature of 55° C. and a reaction time of 5 h.

[0115] The components in the composite fiber are calculated by weight as follows: 100 parts of modified polylactic acid, 2 parts of nanocellulose, 4 parts of citrate, 3 parts of nano zinc oxide, 3 parts of polyethylene glycol, and 3 parts of polyvinyl alcohol.

[0116] In step S3, the melting temperature is 180° C., the spinning temperature is 190° C., and the spinning speed is 900 m / min.

[0117] The stretching ratio in step S4 is 3.0 times and the stretching temperature is 85°C.

[0118] Comparative Example 1: A method for preparing a degradable high-elastic polylactic acid composite fiber (without glutamic acid modification):

[0119] S1, dissolving the modifier chitosan in acidic water, adding polylactic acid, adjusting the pH and heating for reaction, washing with water and drying after the reaction to obtain modified polylactic acid;

[0120] S2, taking the modified polylactic acid obtained in step S1 and mixing it with nano cellulose, citrate, nano zinc oxide, polyethylene glycol and polyvinyl alcohol to obtain a spinning material;

[0121] S3, melting the obtained spinning material, and spinning it through a spinning machine to obtain fibers;

[0122] S4. After the obtained fiber is cooled and solidified, it is stretched; the stretched fiber is wound and collected to form a finished fiber.

[0123] The mass ratio of chitosan to polylactic acid in step S1 is 7:100.

[0124] The acidic water in step S1 has a pH of 6.0; the pH is adjusted to 5.5.

[0125] In step S1, the heating reaction was carried out and the stirring reaction was carried out at a temperature of 55° C. and a reaction time of 5 h.

[0126] The components in the composite fiber are calculated by weight as follows: 100 parts of modified polylactic acid, 2 parts of nanocellulose, 4 parts of citrate, 3 parts of nano zinc oxide, 3 parts of polyethylene glycol, and 3 parts of polyvinyl alcohol.

[0127] In step S3, the melting temperature is 180° C., the spinning temperature is 190° C., and the spinning speed is 900 m / min.

[0128] The stretching ratio in step S4 is 3.0 times and the stretching temperature is 85°C.

[0129] Comparative Example 2: A method for preparing a degradable high-elastic polylactic acid composite fiber (without adding chitosan for modification):

[0130] S1, dissolving the modifier glutamic acid in acidic water, adding polylactic acid, adjusting the pH and heating to react, washing with water and drying after the reaction to obtain modified polylactic acid;

[0131] S2, taking the modified polylactic acid obtained in step S1 and mixing it with nano cellulose, citrate, nano zinc oxide, polyethylene glycol and polyvinyl alcohol to obtain a spinning material;

[0132] S3, melting the obtained spinning material, and spinning it through a spinning machine to obtain fibers;

[0133] S4. After the obtained fiber is cooled and solidified, it is stretched; the stretched fiber is wound and collected to form a finished fiber.

[0134] The mass ratio of glutamic acid to polylactic acid in step S1 is 2:100.

[0135] The acidic water in step S1 has a pH of 6.0; the pH is adjusted to 5.5.

[0136] In step S1, the heating reaction was carried out and the stirring reaction was carried out at a temperature of 55° C. and a reaction time of 5 h.

[0137] The components in the composite fiber are calculated by weight as follows: 100 parts of modified polylactic acid, 2 parts of nanocellulose, 4 parts of citrate, 3 parts of nano zinc oxide, 3 parts of polyethylene glycol, and 3 parts of polyvinyl alcohol.

[0138] In step S3, the melting temperature is 180° C., the spinning temperature is 190° C., and the spinning speed is 900 m / min.

[0139] The stretching ratio in step S4 is 3.0 times and the stretching temperature is 85°C.

[0140] Comparative Example 3: A method for preparing a degradable high-elastic polylactic acid composite fiber (without adding nanocellulose for modification):

[0141] S1, dissolving the modifiers glutamic acid and chitosan in acidic water, adding polylactic acid, adjusting the pH and heating to react, washing with water and drying after the reaction to obtain modified polylactic acid;

[0142] S2, taking the modified polylactic acid obtained in step S1 and mixing it with citrate, nano zinc oxide, polyethylene glycol and polyvinyl alcohol to obtain a spinning material;

[0143] S3, melting the obtained spinning material, and spinning it through a spinning machine to obtain fibers;

[0144] S4. After the obtained fiber is cooled and solidified, it is stretched; the stretched fiber is wound and collected to form a finished fiber.

[0145] The mass ratio of glutamic acid to polylactic acid in step S1 is 2:100.

[0146] The mass ratio of chitosan to polylactic acid in step S1 is 7:100.

[0147] The acidic water in step S1 has a pH of 6.0; the pH is adjusted to 5.5.

[0148] In step S1, the heating reaction was carried out and the stirring reaction was carried out at a temperature of 55° C. and a reaction time of 5 h.

[0149] The components in the composite fiber are calculated by weight as follows: 100 parts of modified polylactic acid, 4 parts of citrate, 3 parts of nano zinc oxide, 3 parts of polyethylene glycol, and 3 parts of polyvinyl alcohol.

[0150] In step S3, the melting temperature is 180° C., the spinning temperature is 190° C., and the spinning speed is 900 m / min.

[0151] The stretching ratio in step S4 is 3.0 times and the stretching temperature is 85°C.

[0152] Comparative Example 4: A method for preparing a degradable high-elastic polylactic acid composite fiber (without adding chitosan modification and nanocellulose):

[0153] S1, dissolving the modifier glutamic acid in acidic water, adding polylactic acid, adjusting the pH and heating to react, washing with water and drying after the reaction to obtain modified polylactic acid;

[0154] S2, taking the modified polylactic acid obtained in step S1 and mixing it with citrate, nano zinc oxide, polyethylene glycol and polyvinyl alcohol to obtain a spinning material;

[0155] S3, melting the obtained spinning material, and spinning it through a spinning machine to obtain fibers;

[0156] S4. After the obtained fiber is cooled and solidified, it is stretched; the stretched fiber is wound and collected to form a finished fiber.

[0157] The mass ratio of glutamic acid to polylactic acid in step S1 is 2:100.

[0158] The acidic water in step S1 has a pH of 6.0; the pH is adjusted to 5.5.

[0159] In step S1, the heating reaction was carried out and the stirring reaction was carried out at a temperature of 55° C. and a reaction time of 5 h.

[0160] The components in the composite fiber are calculated by weight as follows: 100 parts of modified polylactic acid, 4 parts of citrate, 3 parts of nano zinc oxide, 3 parts of polyethylene glycol, and 3 parts of polyvinyl alcohol.

[0161] In step S3, the melting temperature is 180° C., the spinning temperature is 190° C., and the spinning speed is 900 m / min.

[0162] The stretching ratio in step S4 is 3.0 times and the stretching temperature is 85°C.

[0163] Comparative Example 5: A method for preparing a degradable high-elastic polylactic acid composite fiber (without adding glutamic acid modification and nanocellulose):

[0164] S1, dissolving the modifier chitosan in acidic water, adding polylactic acid, adjusting the pH and heating for reaction, washing with water and drying after the reaction to obtain modified polylactic acid;

[0165] S2, taking the modified polylactic acid obtained in step S1 and mixing it with citrate, nano zinc oxide, polyethylene glycol and polyvinyl alcohol to obtain a spinning material;

[0166] S3, melting the obtained spinning material, and spinning it through a spinning machine to obtain fibers;

[0167] S4. After the obtained fiber is cooled and solidified, it is stretched; the stretched fiber is wound and collected to form a finished fiber.

[0168] The mass ratio of chitosan to polylactic acid in step S1 is 7:100.

[0169] The acidic water in step S1 has a pH of 6.0; the pH is adjusted to 5.5.

[0170] In step S1, the heating reaction was carried out and the stirring reaction was carried out at a temperature of 55° C. and a reaction time of 5 h.

[0171] The components in the composite fiber are calculated by weight as follows: 100 parts of modified polylactic acid, 4 parts of citrate, 3 parts of nano zinc oxide, 3 parts of polyethylene glycol, and 3 parts of polyvinyl alcohol.

[0172] In step S3, the melting temperature is 180° C., the spinning temperature is 190° C., and the spinning speed is 900 m / min.

[0173] The stretching ratio in step S4 is 3.0 times and the stretching temperature is 85°C.

[0174] Comparative Example 6 A method for preparing a degradable high-elastic polylactic acid composite fiber (without adding glutamic acid and chitosan for modification, step S1 is used as a parallel control):

[0175] S1, adding polylactic acid into acidic water, adjusting the pH and heating for reaction, washing with water and drying after the reaction to obtain modified polylactic acid;

[0176] S2, taking the modified polylactic acid obtained in step S1 and mixing it with nano cellulose, citrate, nano zinc oxide, polyethylene glycol and polyvinyl alcohol to obtain a spinning material;

[0177] S3, melting the obtained spinning material, and spinning it through a spinning machine to obtain fibers;

[0178] S4. After the obtained fiber is cooled and solidified, it is stretched; the stretched fiber is wound and collected to form a finished fiber.

[0179] The mass ratio of glutamic acid to polylactic acid in step S1 is 2:100.

[0180] The mass ratio of chitosan to polylactic acid in step S1 is 7:100.

[0181] The acidic water in step S1 has a pH of 6.0; the pH is adjusted to 5.5.

[0182] In step S1, the heating reaction was carried out and the stirring reaction was carried out at a temperature of 55° C. and a reaction time of 5 h.

[0183] The components in the composite fiber are calculated by weight as follows: 100 parts of modified polylactic acid, 2 parts of nanocellulose, 4 parts of citrate, 3 parts of nano zinc oxide, 3 parts of polyethylene glycol, and 3 parts of polyvinyl alcohol.

[0184] In step S3, the melting temperature is 180° C., the spinning temperature is 190° C., and the spinning speed is 900 m / min.

[0185] The stretching ratio in step S4 is 3.0 times and the stretching temperature is 85°C.

[0186] Comparative Example 7 A method for preparing a degradable high-elastic polylactic acid composite fiber (without adding glutamic acid and chitosan for modification, and step S1 is not performed):

[0187] S1, mixing polylactic acid with nanocellulose, citrate, nano zinc oxide, polyethylene glycol and polyvinyl alcohol to obtain a spinning material;

[0188] S2, melting the obtained spinning material, and spinning it through a spinning machine to obtain fibers;

[0189] S3. After the obtained fiber is cooled and solidified, it is stretched; the stretched fiber is wound and collected to form a finished fiber.

[0190] The components in the composite fiber are calculated by weight as follows: 100 parts of polylactic acid, 2 parts of nanocellulose, 4 parts of citrate, 3 parts of nano zinc oxide, 3 parts of polyethylene glycol, and 3 parts of polyvinyl alcohol.

[0191] In step S2, the melting temperature is 180° C., the spinning temperature is 190° C., and the spinning speed is 900 m / min.

[0192] The stretching ratio in step S3 is 3.0 times and the stretching temperature is 85°C.

[0193] Comparative Example 8 A method for preparing a degradable high-elastic polylactic acid composite fiber (without modifying the raw materials, but performing mixing optimization):

[0194] S1, mixing polylactic acid with glutamic acid, chitosan, nanocellulose, citrate, nano zinc oxide, polyethylene glycol and polyvinyl alcohol to obtain a spinning material;

[0195] S2, melting the obtained spinning material, and spinning it through a spinning machine to obtain fibers;

[0196] S3. After the obtained fiber is cooled and solidified, it is stretched; the stretched fiber is wound and collected to form a finished fiber.

[0197] The mass ratio of glutamic acid to polylactic acid in step S1 is 2:100.

[0198] The mass ratio of chitosan to polylactic acid in step S1 is 7:100.

[0199] The components in the composite fiber are calculated by weight as follows: 100 parts of polylactic acid, 2 parts of nanocellulose, 4 parts of citrate, 3 parts of nano zinc oxide, 3 parts of polyethylene glycol, and 3 parts of polyvinyl alcohol.

[0200] In step S2, the melting temperature is 180° C., the spinning temperature is 190° C., and the spinning speed is 900 m / min.

[0201] The stretching ratio in step S3 is 3.0 times and the stretching temperature is 85°C.

[0202] Blank control 1: A method for preparing a degradable high-elastic polylactic acid composite fiber (without modifying the raw materials, without adding nanocellulose, and step S1 as a control):

[0203] S1, adding polylactic acid into acidic water, adjusting the pH and then heating for reaction, washing with water and drying after the reaction to obtain polylactic acid;

[0204] S2, mixing the polylactic acid obtained in step S1 with citrate, nano zinc oxide, polyethylene glycol, and polyvinyl alcohol to obtain a spinning material;

[0205] S3, melting the obtained spinning material, and spinning it through a spinning machine to obtain fibers;

[0206] S4. After the obtained fiber is cooled and solidified, it is stretched; the stretched fiber is wound and collected to form a finished fiber.

[0207] The components in the composite fiber are calculated by weight as follows: 100 parts of polylactic acid, 4 parts of citrate, 3 parts of nano zinc oxide, 3 parts of polyethylene glycol, and 3 parts of polyvinyl alcohol.

[0208] In step S3, the melting temperature is 180° C., the spinning temperature is 190° C., and the spinning speed is 900 m / min.

[0209] The stretching ratio in step S4 is 3.0 times and the stretching temperature is 85°C.

[0210] Blank control 2: A method for preparing a degradable high-elastic polylactic acid composite fiber (without modifying the raw materials, without adding nanocellulose, and without operating step S1):

[0211] S1, mixing polylactic acid with citrate, nano zinc oxide, polyethylene glycol and polyvinyl alcohol to obtain a spinning material;

[0212] S2, melting the obtained spinning material, and spinning it through a spinning machine to obtain fibers;

[0213] S3. After the obtained fiber is cooled and solidified, it is stretched; the stretched fiber is wound and collected to form a finished fiber.

[0214] The components in the composite fiber are calculated by weight as follows: 100 parts of polylactic acid, 4 parts of citrate, 3 parts of nano zinc oxide, 3 parts of polyethylene glycol, and 3 parts of polyvinyl alcohol.

[0215] In step S2, the melting temperature is 180° C., the spinning temperature is 190° C., and the spinning speed is 900 m / min.

[0216] The stretching ratio in step S3 is 3.0 times and the stretching temperature is 85°C.

[0217] Performance testing: Composting degradation rate: The degradation rate of the sample is evaluated according to the method of measuring the released carbon dioxide in the national standard GB / T 19277.1-2011 "Determination of the final aerobic biodegradability of materials under controlled composting conditions using the method of measuring the released carbon dioxide". Elastic modulus: According to GB / T 19341-2003 standard. Strength: According to GB / T 34239-2017 standard.

[0218] The compost used in the experimental evaluation was prepared according to the above standard GB / T 19277.1-2011. Accurately weighed samples of the same mass of the embodiment and the comparative example were mixed with the same fixed mass of compost as the sample group; the sample containing only compost was the blank control group 3. The carbon dioxide absorption bottle was titrated at regular intervals to calculate the amount of carbon dioxide released and thus the biodegradation rate. The specific calculation method is: the amount of carbon dioxide collected in the absorption bottle of the titrated sample group is converted into the corresponding carbon content W1, the carbon content W2 calculated by subtracting the carbon dioxide released by the blank group is divided by the total carbon content W0 in the sample to obtain the biodegradation rate. The calculation formula is as follows:

[0219]

[0220] After testing, the tensile strength of the fibers obtained in all the above embodiments and comparative examples is greater than 50 MPa, which meets the application requirements. The composting degradation rate data is shown in Table 1.

[0221] Table 1 Test results of sample composting degradation rate

[0222]

[0223]

[0224] From the experimental data, it can be seen that the two modifiers added in the polylactic acid modification step and the nanocellulose added in the melt mixing step have a synergistic effect on the improvement of the degradability of the polylactic acid fiber, and this synergistic effect is also reflected in the simultaneous guarantee of fiber elasticity. If this synergistic effect is lost (any one or two of the three are missing), then even if the degradability is improved, the elastic parameters are lower than those of ordinary polylactic acid fibers. In addition, while optimizing elasticity, the raw materials we use (especially chitosan) also bring excellent antibacterial properties to the product, thus expanding the application range of the product of the present invention to a certain extent.

[0225] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

[0226] The present invention and its implementation methods are described above, and such description is not restrictive, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it, without departing from the purpose of the invention, they can design methods and embodiments similar to the technical solution without creativity, which should all fall within the protection scope of the present invention.

Claims

1. A degradable and highly elastic polylactic acid composite fiber, Features: Including modified polylactic acid, nano cellulose, citrate, nano zinc oxide, polyethylene glycol, and polyvinyl alcohol.

2. The degradable high-elastic polylactic acid composite fiber according to claim 1, Features: The components in the composite fiber are calculated by weight as follows: 100 parts of modified polylactic acid, 1-3 parts of nanocellulose, 3-5 parts of citrate, 2-4 parts of nano zinc oxide, 2-4 parts of polyethylene glycol, and 2-4 parts of polyvinyl alcohol.

3. The degradable high-elastic polylactic acid composite fiber according to claim 1 or 2, Features: The diameter of the nanocellulose fiber is 3-25 nm, and the fiber length is 50-500 nm.

4. A method for preparing the degradable high-elastic polylactic acid composite fiber according to any one of claims 1 to 3, Features: The following steps are involved: S1, taking modified polylactic acid, nanocellulose, citrate, nano zinc oxide, polyethylene glycol, and polyvinyl alcohol and mixing them in a high-speed mixer to obtain a spinning material; S2, melting the obtained spinning material, and spinning it through a spinning machine to obtain fibers; S3. After the obtained fiber is cooled and solidified, it is stretched; the stretched fiber is wound and collected to form a finished fiber.

5. The method for preparing the degradable high-elastic polylactic acid composite fiber according to claim 4, Features: In step S3, the melting temperature is 160-200° C., the spinning temperature is 185-195° C., and the spinning speed is 800-1000 m / min.

6. The method for preparing the degradable high-elastic polylactic acid composite fiber according to claim 4, Features: The stretching ratio in step S4 is 2.5-3.5 times, and the stretching temperature is 80-90°C.

7. The method for preparing the degradable high-elastic polylactic acid composite fiber according to claim 4, Features: The preparation method of the modified polylactic acid comprises: dissolving modifiers glutamic acid and chitosan in acidic water, adding polylactic acid, adjusting pH and then heating for reaction, washing with water and drying after the reaction is finished to obtain the modified polylactic acid.

8. The method for preparing the degradable high-elastic polylactic acid composite fiber according to claim 7, Features: In the modified polylactic acid preparation method, the mass ratio of glutamic acid to polylactic acid is 1:100; in the modified polylactic acid preparation method, the mass ratio of chitosan to polylactic acid is 5:

100.

9. The method for preparing the degradable high-elastic polylactic acid composite fiber according to claim 7, Features: In the modified polylactic acid preparation method, the pH of the acidic water is 5.5; the pH is adjusted to 5.5; in the modified polylactic acid preparation method, the heating reaction is a stirring reaction, the reaction temperature is 50° C., and the reaction time is 4 hours.

Citation Information

Cited By

  • Environment-friendly degradable polylactic acid straw and preparation process thereof

    CN120137370A

  • Environment-friendly degradable wet tissue and preparation method thereof

    CN120330952A

  • PLA biodegradable antibacterial fabric and preparation method thereof

    CN122791630A