Lightweight high-strength high-impact polypropylene flat filament / continuous inorganic fiber fabric, woven composite material as well as preparation method and application of lightweight high-strength high-impact polypropylene flat filament / continuous inorganic fiber fabric

Through the hot pressing preparation of polypropylene flat wire/continuous inorganic fiber fabrics, combined with specific polymer combinations and structural design, the problems of mechanical properties and interface bonding strength of polypropylene composite materials are solved, achieving high-performance and environmentally friendly production, meeting lightweight Quality, high strength and high impact resistance.

CN118910783APending Publication Date: 2024-11-08CHINA PETROLEUM & CHEMICAL CORP +1

Patent Information

Application Number
CN202310506617.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-07
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing polypropylene composite materials are difficult to have high mechanical properties, strong interface bonding strength and light weight at the same time, and the production process is unsafe and environmentally friendly.

Method used

Polypropylene braided composite materials are prepared by hot pressing using polypropylene flat wire/continuous inorganic fiber fabrics. The composition of homopolymerized polypropylene and impact-resistant copolymerized polypropylene is used to combine random copolymerized polypropylene and thermal bonding enhancer to form multiple Layer structure to improve mechanical properties and interlayer peel strength and avoid the use of adhesives and volatile solvents during hot pressing.

Benefits of technology

The light weight, tensile strength, impact performance and interlayer peeling strength of polypropylene braided composite materials are achieved, and the safety and environmental protection of the production process are improved. The density is less than 1200Kg/m3 and the longitudinal tensile strength is ≥250Mpa. The interlayer peeling strength is ≥1N/mm, and the impact strength of the drop hammer is ≥150J.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004216068260000211
    Figure BDA0004216068260000211
  • Figure BDA0004216068260000221
    Figure BDA0004216068260000221
Patent Text Reader

Abstract

The invention relates to the field of polypropylene materials, in particular to a polypropylene flat filament / continuous inorganic fiber fabric, a woven composite material and a preparation method and application of the polypropylene flat filament / continuous inorganic fiber fabric. The polypropylene flat filament / continuous inorganic fiber fabric is a fabric formed by warp yarns and weft yarns in a plain weave, twill weave and / or satin weave structure, the warp yarns are polypropylene ribbon-like filaments, and the weft yarns comprise two groups of yarns, namely polypropylene ribbon-like filaments and continuous inorganic fiber reinforced polypropylene unidirectional prepreg tapes; wherein the structure of the polypropylene flat filament is BAB '; the layer A contains a polypropylene composition A, the layer B and the layer B'are the same or different and respectively and correspondingly contain a polypropylene composition B and a polypropylene composition B ', and the melting point of the polypropylene composition A is greater than that of the polypropylene composition B and that of the polypropylene composition B'. The polypropylene woven composite material is obtained through hot pressing of the fabric, and the polypropylene woven composite material has the advantages of light weight, good tensile property and impact resistance, and still has good interlayer peel strength when being prepared at a low hot pressing temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polyolefin braided composite materials, and more particularly to a lightweight, high-strength, high-impact polypropylene flat yarn / continuous inorganic fiber fabric, a braided composite material, and a preparation method and application thereof. Background Art

[0002] Polypropylene (PP) resin has low density, good heat resistance, no toxicity, and has the advantages of light weight and low cost, which makes it widely used. However, its mechanical properties (tensile strength, modulus) are low, and the molding shrinkage rate is large, which limits the use of polypropylene materials in structural parts. Usually, the polypropylene reinforcement method is to use continuous inorganic fiber materials, such as glass fiber, carbon fiber and other materials for filling, so that the fibers are continuously distributed in the polypropylene matrix. For example, CN 110734604 B discloses an organic sheet, which is formed by laminating and hot pressing continuous glass fiber reinforced polypropylene unidirectional prepreg tapes. The preparation method of the organic sheet comprises: impregnating a raw material melt containing polypropylene, a compatibilizer, and a polymer bonding aid with continuous glass fibers to obtain a continuous glass fiber reinforced polypropylene prepreg tape; after the continuous glass fiber reinforced polypropylene prepreg tape is cross-cut, it is layered according to the material thickness requirements, and the required organic sheet is pressed out by a continuous double-belt press device. CN 104553157B discloses a composite laminate and a preparation method thereof. The composite plate comprises, from top to bottom, an upper / lower surface layer of non-woven fabric and a core layer comprising several layers of continuous fiber reinforced thermoplastic prepreg tapes. The preparation method of the composite laminate comprises: stacking the upper and lower surface layers and the core layer, placing them in a hot press, and then placing them in a cold press for cold pressing to set the shape.

[0003] The mechanical properties of the continuous fiber reinforced polymer composite material prepared by the above method are greatly improved, but its ability to resist impact loads and interface bonding strength are still relatively poor. At present, the ability to resist impact loads is mainly improved by increasing the thickness of the composite, but this will greatly increase its weight. The improvement of interface bonding strength in the prior art is mainly achieved by introducing polymer bonding additives, while the addition of adhesives and / or volatile solvents makes the production process less safe and less environmentally friendly.

[0004] Therefore, how to provide a polypropylene flat yarn / continuous inorganic fiber composite material that has strong mechanical properties, high interface bonding strength and light weight, and improve the safety and environmental protection of the production process is a technical problem that needs to be solved at present. Summary of the invention

[0005] The purpose of the present invention is to overcome the technical defect that the existing continuous fiber reinforced polypropylene composite material is difficult to have strong mechanical properties, high interface bonding strength and light weight at the same time, and provide a lightweight, high-strength and high-impact polypropylene flat yarn / continuous inorganic fiber fabric, a woven composite material and a preparation method and application thereof. The polypropylene flat yarn / continuous inorganic fiber fabric of the present invention is subjected to hot pressing to obtain a polypropylene woven composite material. When less continuous inorganic fibers are used, a lighter polypropylene woven composite material is obtained. The polypropylene woven composite material has excellent mechanical properties and good interlayer peeling strength.

[0006] The first aspect of the present invention is to provide a polypropylene flat yarn / continuous inorganic fiber fabric, which is a fabric formed by warp yarn and weft yarn in a plain, twill and / or satin structure; the warp yarn is a polypropylene flat yarn, and the weft yarn includes two groups of yarns of a polypropylene flat yarn and a continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape; wherein the continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape contains random copolymerized polypropylene x, continuous inorganic fiber and a compatibilizer; wherein the polypropylene flat yarn includes a layer A and layers B and B' located on both sides of the layer A, and the structure is BAB'; the layer A contains a polypropylene composition A, and the polypropylene composition A includes homopolymerized polypropylene a and impact copolymerized polypropylene b; the layer B is the same as or different from the layer B', and each correspondingly contains a polypropylene composition B and a polypropylene composition B', wherein the polypropylene composition B and the polypropylene composition B' each include random copolymerized polypropylene x and a thermal bonding enhancer y; wherein the melting point of the polypropylene composition A is greater than the melting point of the polypropylene composition B and the polypropylene composition B'.

[0007] According to the present invention, the film layers B and B' on both sides of the film layer A are the same or different. In a preferred embodiment of the present invention, the film layers B and B' on both sides of the film layer A are the same.

[0008] According to some preferred technical solutions of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 50-99wt% of homopolypropylene a and 1-50wt% of impact copolymer polypropylene b; preferably, the polypropylene composition A comprises 70-90wt% of homopolypropylene a and 10-30wt% of impact copolymer polypropylene b.

[0009] According to some preferred technical solutions of the present invention, based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 70-99wt% of random copolymer polypropylene x and 1-30wt% of thermal adhesion enhancer y; preferably, the polypropylene composition B comprises 80-90wt% of random copolymer polypropylene x and 10-20wt% of thermal adhesion enhancer y.

[0010] According to some preferred technical solutions of the present invention, based on the total thickness of the polypropylene flat yarn, the thickness of layer A accounts for 51%-89% of the total thickness, preferably 71%-89%, and more preferably 71%-80%. The thicknesses of film layers B and B' on both sides of film layer A can be the same or different, preferably the same.

[0011] The present invention does not limit the thickness of the continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape and the polypropylene flat yarn, and can be selected in a wide range according to its actual application field. Preferably, the thickness of the continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape and the polypropylene flat yarn can be 10-1000 μm, preferably 30-500 μm, and more preferably 50-300 μm respectively.

[0012] According to the present invention, the thickness of the film layers A, B, B' can be controlled by the melt pump of the extruder during the processing.

[0013] In a preferred embodiment of the present invention, the melting point of the polypropylene composition A is greater than the melting points of the polypropylene composition B and the polypropylene composition B'; preferably, the melting point of the homopolymer polypropylene a in the polypropylene composition A is greater than the melting point of the random copolymer polypropylene x in the polypropylene compositions B and B'. The inventors of the present invention surprisingly found that the flat yarn prepared from the obtained polypropylene sheet and the inorganic fiber reinforced polypropylene unidirectional pre-impregnated warp weaving hot pressing to obtain a polypropylene woven composite material have more excellent mechanical properties and better interlayer peel strength. Even at a lower hot pressing temperature and a wider hot pressing temperature range, the obtained polypropylene woven composite material has a higher interlayer peel strength.

[0014] According to some preferred technical solutions of the present invention, the difference between the melting point of polypropylene composition A and the melting point of polypropylene composition B, and the difference between the melting point of polypropylene composition A and the melting point of polypropylene composition B' are each greater than or equal to 5°C, preferably greater than or equal to 10°C, and more preferably greater than or equal to 20°C.

[0015] According to some preferred technical solutions of the present invention, the melting point of the homopolymer polypropylene a in the polypropylene composition A is greater than the melting point of the random copolymer polypropylene x in the polypropylene composition B and the polypropylene composition B', and the temperature difference of the corresponding melting points is preferably greater than or equal to 10 degrees.

[0016] According to some preferred technical solutions of the present invention, the width of the polypropylene flat wire is 2-5 mm.

[0017] According to some preferred technical solutions of the present invention, the homopolypropylene a has the following characteristics:

[0018] The melting point is 160-170°C; and / or the melt flow rate of the homopolypropylene a at 230°C and 2.16kg load is 0.5-50g / 10min, preferably 1-20g / 10min, and more preferably 2.5-18g / 10min; and / or the isotacticity (mm) of the homopolypropylene a is not less than 96%.

[0019] According to some preferred technical solutions of the present invention, the impact-resistant copolymer polypropylene b has the following characteristics: a melting point of 150-170°C; and / or, the monomers of the impact-resistant copolymer polypropylene b and propylene copolymer are ethylene or butene, and the ethylene or butene content is 2-50%wt, preferably 3-20%wt, and more preferably 5-15%wt, and / or, the melt flow rate of the impact-resistant copolymer polypropylene b at 230°C and 2.16kg load is 0.5-50g / 10min, preferably 1-20g / 10min, and more preferably 2.5-18g / 10min; and / or, the impact strength of the impact-resistant copolymer polypropylene b is not less than 20KJ / m 2 .

[0020] According to the research conducted by the inventors, when the melt mass flow rate and polymer composition ratio of the polypropylene composition A are within the above preferred ranges, the impact-resistant copolymerized polypropylene b in the composition can absorb impact energy well, meet the requirements of impact performance, and make the sheet have good impact performance. At the same time, since the macromolecular segments in the homopolymerized polypropylene a are relatively regular, crystallization occurs during the preparation of the sheet, so the sheet also has good tensile properties.

[0021] According to some preferred technical solutions of the present invention, the random copolymer polypropylene x has the following characteristics: the melting point of the random copolymer polypropylene x is 120-140°C; and / or the melt flow rate of the random copolymer polypropylene x at 230°C and a load of 2.16 kg is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and further preferably 3-18 g / 10 min; and / or the random copolymer polypropylene x is a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer or a propylene-ethylene binary copolymer.

[0022] According to some preferred technical solutions of the present invention, the thermal adhesion enhancer y has: a melt flow rate of 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 1-18 g / 10 min at 190°C and a load of 2.16 kg; and / or, the thermal adhesion enhancer y is selected from one or more of polyolefin elastomers, EPDM rubber, SEBS, SBS, EVA and petroleum resins; preferably, the polyolefin elastomer is a copolymer elastomer of ethylene and propylene and / or alpha olefin; further preferably, the alpha olefin is a C4-C12 alpha olefin, more preferably 1-butene and / or 1-octene; and / or,

[0023] The petroleum resin is a hydrogenated petroleum resin of C5 and / or C9, preferably having a softening point of 100-150° C.; more preferably, the petroleum resin is a cyclopentadiene type resin.

[0024] According to the research conducted by the present inventors, when the melt mass flow rate and polymer composition ratio of the polypropylene compositions B and B' are within the preferred range, the low melting point random copolymer polypropylene x and thermal bonding enhancer y in the composition can significantly reduce the hot pressing temperature and broaden the hot pressing temperature window, and the thermal bonding enhancer y provides the sheet with good bonding properties, which can further improve the interlayer peeling strength.

[0025] According to some preferred technical solutions of the present invention, the layer A further contains a β-crystal nucleating agent; preferably,

[0026] The β-crystal nucleating agent is selected from at least one of condensed ring aromatic hydrocarbons, group IIA two-component complexes, aromatic diamides, rare earth compounds and cyclic dicarboxylates.

[0027] The content range of the β-crystal nucleating agent is relatively wide. Preferably, based on 100 parts by weight of the total amount of the polypropylene composition A, the content of the β-crystal nucleating agent in layer A is 0.01-0.5 parts by weight. For example, the content of the β-crystal nucleating agent may be 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, or 0.5 parts by weight.

[0028] According to the research of the present inventors, when the melt mass flow rate, polymer composition ratio and thickness distribution of the film layer A of the polypropylene composition A and the polypropylene combinations B and B' are within the preferred range, the sheet preparation process can be made smoother, thereby making the sheet have better uniformity, tensile strength, impact resistance and interlayer peeling strength.

[0029] According to some preferred technical solutions of the present invention, the polypropylene flat yarn is obtained by co-extrusion molding, casting or calendering, and stretching of polypropylene composition A, polypropylene composition B, and B' according to the BAB' structure to obtain a polypropylene sheet, which is then cut to obtain the polypropylene flat yarn.

[0030] In a preferred embodiment of the present invention, the preparation of the polypropylene composition A comprises melt blending the components including the homopolypropylene a and the impact copolymer polypropylene b. The conditions and equipment for melt blending the polypropylene composition A adopt the conditions and equipment for melt blending of polyolefins in the prior art, preferably, the melting temperature is 150-170° C., and the equipment is preferably a twin-screw extruder.

[0031] In a preferred embodiment of the present invention, the preparation of the polypropylene compositions B and B' comprises melt blending the components including the random copolymer polypropylene x and the thermal adhesion enhancer y. The conditions and equipment for melt blending the polypropylene compositions B and B' are the same as those for melt blending polyolefins in the prior art, preferably, the melting temperature is 110-150°C, and the equipment is preferably a twin-screw extruder.

[0032] The selection range of the co-extrusion and casting temperatures is relatively wide. In a preferred embodiment of the present invention, in step (1), the co-extrusion and casting temperatures are independently selected from 200-240°C; the temperature of the calendering roll is 50-70°C.

[0033] The selection range of stretching conditions is relatively wide. In a preferred embodiment of the present invention, the stretching conditions include: the stretching method is free stretching, and / or solid phase stretching, and / or multi-stage stretching; the stretching temperature is 90-165°C, preferably 90-140°C, and further preferably 90-119°C; the stretching ratio is 1-20 times, preferably 2-15 times.

[0034] In a preferred embodiment of the present invention, the longitudinal tensile strength of the stretched polypropylene sheet is greater than or equal to 30 MPa, more preferably 30 MPa-1 GPa; most preferably 300-800 MPa.

[0035] According to the present invention, the continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape contains random copolymerized polypropylene x, continuous inorganic fibers and a compatibilizer. According to some preferred technical solutions of the present invention, the continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape contains, by mass, 35-58wt% of random copolymerized polypropylene x, 40-60wt% of continuous inorganic fibers and 2-5wt% of a compatibilizer.

[0036] According to some preferred technical solutions of the present invention, the continuous inorganic fiber is selected from at least one of metal wire, carbon fiber, glass fiber and ceramic fiber.

[0037] According to some preferred technical solutions of the present invention, the compatibilizer is selected from one or more of polypropylene-maleic anhydride grafts and polypropylene-methyl methacrylate grafts.

[0038] According to some preferred technical solutions of the present invention, the density of the continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape is 1500-1800 Kg / m 3 , and / or, a thickness of 150-500 μm, and / or, a width of 2-3 mm.

[0039] According to some preferred technical schemes of the present invention, the continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape is prepared by the following method: random copolymer polypropylene x and a compatibilizer are mixed, melt-kneaded, and cast to obtain a melt, the melt is impregnated with the continuous inorganic fibers, and the continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape is obtained by cooling and shaping.

[0040] As an example, the preparation method of the continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape includes but is not limited to the following methods: after the random copolymer polypropylene x and the compatibilizer are evenly mixed, they are melt-kneaded by a twin-screw extruder, and the melt is conveyed into the impregnation mold through a casting mold; the continuous inorganic fiber is drawn out from the yarn frame unit, and after passing through a tension adjustment device, a wire spreading device, and a preheating device, it is introduced into the impregnation mold, impregnated with the melt, and the outlet mold is cooled and shaped to obtain a continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape.

[0041] The second aspect of the present invention is to provide a method for preparing the polypropylene flat yarn / continuous inorganic fiber fabric described in the first aspect, comprising: using the polypropylene flat yarn as warp yarn, using two groups of yarns including the polypropylene flat yarn and the continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape as weft yarn, weaving the warp yarn and the weft yarn in a plain, twill and / or satin structure to obtain the polypropylene flat yarn / continuous inorganic fiber fabric.

[0042] The third aspect of the present invention is a polypropylene woven composite material, comprising multiple layers of hot pressed polypropylene flat yarn / continuous inorganic fiber fabric described in the first aspect and / or polypropylene flat yarn / continuous inorganic fiber fabric prepared by the preparation method described in the second aspect.

[0043] As a specific example, more specifically, the polypropylene woven composite material comprises multiple layers of polypropylene flat yarn / continuous inorganic fiber fabric; the warp yarn of the polypropylene flat yarn / continuous inorganic fiber fabric is a polypropylene flat yarn; the weft yarn is two groups of yarns, a polypropylene flat yarn and a continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape, and the polypropylene flat yarn / continuous inorganic fiber fabric is formed with the above-mentioned warp yarn and weft yarn in a plain, twill and / or satin structure; the multiple layers of polypropylene flat yarn / continuous inorganic fiber fabric are hot pressed to obtain a polypropylene woven composite material; and the above-mentioned polypropylene flat yarn is the polypropylene flat yarn described above; the continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape is preferably the continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape described above, wherein the continuous inorganic fibers include but are not limited to metal wires, carbon fibers, glass fibers, ceramic fibers, etc.

[0044] According to some preferred technical solutions of the present invention, the multi-layer polypropylene flat yarn / continuous inorganic fiber fabric is stacked from top to bottom in the angle of 0-90° along the respective machine directions.

[0045] According to some preferred technical solutions of the present invention, the number of layers of the multi-layer polypropylene flat yarn / continuous inorganic fiber fabric is greater than or equal to 2 layers, more preferably 2-200 layers; most preferably 4-100 layers.

[0046] According to some preferred technical solutions of the present invention, the polypropylene woven composite material comprises a plurality of sequentially stacked polypropylene flat yarn / continuous inorganic fiber fabric unit groups; each polypropylene flat yarn / continuous inorganic fiber fabric unit group comprises at least one identical or different polypropylene flat yarn / continuous inorganic fiber fabric unit, and the polypropylene flat yarn in each polypropylene flat yarn / continuous inorganic fiber fabric unit comprises a core layer A i and located in the core layer A i The outer layer B on both sides i , B' i , structure B i A i B' i The structure of the polypropylene woven composite material is, from bottom to top, the nth group... the ith group... the second group, the first group, the second group... the ith group... the nth group, and the total number of stacked groups of polypropylene flat yarn / continuous inorganic fiber fabric unit groups is 2n-1; i and n are both integers not less than 2, and i≤n; wherein the core layer A of the polypropylene flat yarn in the polypropylene flat yarn / continuous inorganic fiber fabric unit i Containing polypropylene composition A i , outer layer B i With outer layer B' i The same or different, each corresponding to a polypropylene composition B i , polypropylene composition B' i , the polypropylene composition A i The melting point is greater than that of the polypropylene composition Bi , the polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than the average melting point of all outer layers in the i-1-th group.

[0047] According to some preferred technical solutions of the present invention, the polypropylene composition A i Melting point and polypropylene composition B i The difference in melting points, polypropylene composition A i The melting point of polypropylene composition B' i The difference in melting points is 5°C or more, preferably 10°C or more, and more preferably 20°C or more.

[0048] According to the present invention, the core layer of the polypropylene flat yarn in each polypropylene flat yarn / continuous inorganic fiber fabric unit can be the same material or different materials. There is no particular limitation on this in the present invention as long as the polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , polypropylene composition B' i The melting point can achieve better technical effects.

[0049] According to some preferred technical solutions of the present invention, the difference between the average value of the melting points of all outer layers of the polypropylene flat yarn in the i-th group and the average value of the melting points of all outer layers in the i-1th group are the same or different, and are each 1-40°C, preferably 1-10°C, and more preferably 1-5°C.

[0050] According to some preferred technical solutions of the present invention, each polypropylene flat yarn / continuous inorganic fiber fabric unit group independently includes 1 to 10, preferably 1 to 5 identical or different polypropylene flat yarn / continuous inorganic fiber fabric units. More preferably, 1 to 3 identical or different polypropylene sheet units, more preferably 1 polypropylene sheet unit. Preferably, the number of polypropylene flat yarn / continuous inorganic fiber fabric units included in each polypropylene flat yarn / continuous inorganic fiber fabric unit group is the same.

[0051] Preferably, but not necessarily, the melting point of any outer layer in each group is within ±10°C, within ±5°C, preferably within ±3°C, more preferably within ±1°C of the average melting point of all outer layers in the group.

[0052] In the embodiment where each polypropylene flat yarn / continuous inorganic fiber fabric unit group includes only one polypropylene flat yarn / continuous inorganic fiber fabric unit, for example, the structure of the polypropylene woven composite material can be sequentially as follows from bottom to top: B n A n B' n ……B i A i B'i ...B2A2B'2, B1A1B'1, B2A2B'2...B i A i B' i ……B n A n B' n , the total number of stacked layers of the polypropylene sheet unit is 2n-1; i and n are both integers not less than 2, and i≤n.

[0053] In the embodiment where each polypropylene flat yarn / continuous inorganic fiber fabric unit group includes 2 or more polypropylene flat yarn / continuous inorganic fiber fabric units, for example, the structure of the i-th polypropylene flat yarn / continuous inorganic fiber fabric unit group is B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip The structure of the polypropylene braided composite material can be sequentially as follows from bottom to top: n1 A n1 B' n1 , B n2 A n2 B' n2 ……B nq A nq B' nq )……(B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip )……(B 21 A 21 B' 21 , B 22 A 22 B' 22 ……B 2k A 2k B' 2k )(B 11 A 11 B' 11 , B 12 A 12 B' 12 ……B 1j A 1j B' 1j )(B 21 A 21 B'21 , B 22 A 22 B' 22 ……B 2k A 2k B' 2k )……(B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip )……(B n1 A n1 B' n1 , B n2 A n2 B' n2 ……B nq A nq B' nq ), the total number of stacked layers of polypropylene flat yarn / continuous inorganic fiber fabric units is j+2k+...2p+...2q; j, k, p, q are each independently an integer not less than 2, preferably an integer from 2 to 10, more preferably from 2 to 5, and more preferably from 2 to 3.

[0054] According to some preferred technical solutions of the present invention, the density of the polypropylene braided composite material is less than or equal to 1200Kg / m 3 , preferably less than or equal to 1150Kg / m 3 .

[0055] According to some preferred technical solutions of the present invention, the surface density of the polypropylene woven composite material is greater than or equal to 2000g / m 2 , more preferably 2000-50000g / m 2 ; Most preferably 15000-25000g / m 2 .

[0056] According to some preferred technical solutions of the present invention, the longitudinal tensile strength of the polypropylene woven composite material is greater than or equal to 250 MPa, more preferably 270-500 MPa; most preferably 270-400 MPa.

[0057] exist In a preferred embodiment of the present invention, the polypropylene woven composite material has at least one of the following characteristics:

[0058] Longitudinal tensile strength ≥250Mpa, preferably ≥270Mpa;

[0059] Interlayer peel strength ≥1N / mm, preferably ≥1.1N / mm;

[0060] The tensile strength is measured according to the method specified in GB / T1040.1-2018, and the interlayer peel strength is measured according to the method specified in GB / T2358-98. The corresponding specimens in the above two tests are the standard specimens required in the above-mentioned test standards.

[0061] When the polypropylene woven composite material is obtained by hot pressing 24 layers of polypropylene flat yarn / continuous inorganic fiber fabric and has a thickness of about 3.6 mm, the drop weight impact strength is ≥150J, preferably ≥160J.

[0062] The drop weight impact strength is measured according to the method specified in GB / T14153-1993, and the thickness of the sample is the thickness of the prepared product.

[0063] The fourth aspect of the present invention is to provide a method for preparing the polypropylene woven composite material described in the third aspect, the preparation method comprising laminating and hot-pressing multiple layers of the polypropylene flat yarn / continuous inorganic fiber fabric, and then cooling and shaping to form the polypropylene woven composite material.

[0064] Preferably, the temperature of the hot pressing fusion is 115-170°C, preferably 115-159°C, and more preferably 140-159°C.

[0065] Preferably, the pressure of the hot pressing fusion is 2-10Mpa.

[0066] Preferably, the preheating time of the hot pressing fusion is 5-600s, and the hot pressing time is 1-600s, preferably 10-500s.

[0067] Preferably, the cooling and shaping pressure is 2-8 MPa, and the cooling and shaping time is 30-700 s.

[0068] In a preferred embodiment of the present invention, adjacent layers of the polypropylene flat yarn / continuous inorganic fiber fabric are placed at 0-90° along their respective machine directions, wherein the machine direction is the stretching direction (MD).

[0069] In a more preferred embodiment of the present invention, the method for preparing the lightweight, high-strength, high-impact polypropylene woven composite material comprises the following steps:

[0070] Step a: co-extrude polypropylene composition A, polypropylene composition B, and polypropylene composition B' according to the BAB' structure and cast or calender to obtain a co-extruded polypropylene sheet; preferably, the extrusion casting or calendering temperature is 200-240°C, and the temperature of the calendering roller is 50-70°C. The co-extruded polypropylene sheet is stretched at a certain temperature to obtain a stretched polypropylene sheet; preferably, the stretching temperature is 90-165°C, preferably 90-140°C, and more preferably 90-119°C; the stretching ratio is 1-15 times, preferably 2-9 times; the stretched polypropylene sheet is slit to prepare a polypropylene flat wire, preferably, the width of the polypropylene flat wire is 2-5mm.

[0071] Step b: After the random copolymer polypropylene x and the compatibilizer are uniformly mixed, they are melt-kneaded by a twin-screw extruder, and the melt is conveyed into an impregnation mold through a casting mold; the continuous inorganic fiber is led out from the creel unit, and after passing through a tension adjustment device, a wire spreading device, and a preheating device, it is introduced into the impregnation mold and impregnated with the melt. The outlet mold is cooled and shaped to obtain a continuous glass continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape.

[0072] Step c: winding the polypropylene flat yarn and the inorganic fiber reinforced polypropylene unidirectional prepreg tape separately for weaving; forming the polypropylene flat yarn / continuous inorganic fiber fabric in plain, twill and / or satin structure on a loom with a double-sided multi-shuttle box mechanism with the prepared warp yarn and weft yarn.

[0073] Step d: hot-press and fuse the multi-layer polypropylene flat yarn / continuous inorganic fiber fabric, and then cool and shape to form a polypropylene woven composite material. Preferably, in step d, the hot-pressing conditions are: hot-pressing temperature 115-170°C, preferably 115-159°C, and more preferably 140-159°C; hot-pressing pressure 2-10Mpa, preheating time 5-600s, hot-pressing time 1-600s, preferably 10-500s, cooling pressure 2-8Mpa, cooling time 30s-700s; preferably, adjacent polypropylene fabrics in the polypropylene composite material can be placed at 0-90° between the warp and the warp.

[0074] According to the present invention, in a preferred specific embodiment, the pressure is preferably maintained continuously during the hot pressing and cooling process without being reduced. The hot pressing process is carried out continuously, and preferably a continuous hot pressing composite material molding equipment consisting of a preheating machine, a crawler-type continuous flat hot press, a crawler-type continuous flat cooling press, a sheet cutting machine and a sheet stacking machine arranged in sequence is used; preferably, the crawler-type continuous flat hot press has a preheating unit, an independent heating and pressurizing unit, an air cooling unit and a lifting mechanism.

[0075] During the preparation, the polypropylene flat yarn / continuous inorganic fiber fabric is stacked in sequence and then preheated by a preheater. The preheated samples are sequentially hot-pressed and fused by a crawler-type flat hot press, and then cooled and shaped by a crawler-type continuous flat cooling press to form a polypropylene woven composite material, i.e., a stacked hot-pressed product. Afterwards, the product is sliced ​​by a sheet cutter as needed, and then the hot-pressed product is stacked and arranged by a sheet stacker. The hot-pressing temperature is controlled by a preheating unit, an independent heating and pressing unit, and an air-cooling unit in the crawler-type flat hot press, and the hot-pressing pressure is controlled by a lifting mechanism. According to the research of the inventors, when the preparation process parameters are within a preferred range, the polypropylene woven composite material is preferably prepared using the device, and the polypropylene woven composite material has better tensile strength, impact resistance, and interlayer peeling strength.

[0076] A fifth aspect of the present invention is an application of the polypropylene woven composite material described in the third aspect or the polypropylene woven composite material obtained by the preparation method described in the fourth aspect in the fields of sports protection, automobile manufacturing, military materials and consumer goods.

[0077] According to a specific embodiment of the present invention, the material fields include luggage and transportation industry, shoemaking industry, automobile manufacturing industry, sports equipment manufacturing industry, audio equipment manufacturing industry and military field.

[0078] Compared with the prior art, the present invention has the following beneficial effects:

[0079] (1) The polypropylene woven composite material of the present invention has light weight, good tensile strength, impact resistance and interlayer peeling strength;

[0080] The polypropylene braided composite material has the following characteristics:

[0081] Density ≤1200Kg / m 3 , preferably ≤1150Kg / m 3 ; Longitudinal tensile strength ≥250Mpa, preferably ≥270Mpa; interlayer peel strength ≥1N / mm, preferably ≥1.1N / mm; when the polypropylene woven composite material is obtained by hot pressing 24 layers of polypropylene flat wire / continuous inorganic fiber fabric, and the thickness is about 3.6mm, the drop hammer impact strength is ≥150J, preferably ≥160J.

[0082] (2) The present invention prepares the polypropylene braided composite by a hot pressing bonding method, and does not use any adhesives and volatile solvents during the production process, so the production process is safe and environmentally friendly.

[0083] (3) The polypropylene woven composite material of the present invention can be prepared at a relatively low hot pressing temperature and within a relatively wide hot pressing temperature range, which effectively reduces the energy consumption of the equipment and the damage to the composite material caused by high-temperature operation. At the same time, when prepared at a relatively low hot pressing temperature, it still has good interlayer peeling strength. DETAILED DESCRIPTION

[0084] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0085] In the following examples and comparative examples:

[0086] The extrusion calender and stretching equipment were purchased from Tianjin Hengrui Company, and the model was HRPC-800 three-layer co-extrusion plastic stretching sheet production line.

[0087] The properties of the polypropylene woven composite material, polypropylene composition and sheet material were tested according to the following method. The test results of the polypropylene woven composite material are shown in Table 1:

[0088] (1) Melt flow rate (MFR): measured according to the method specified in GB / T 3682.2-2018, where the test temperature for homopolymer polypropylene and impact copolymer polypropylene is 230°C and the load is 2.16 kg; the test temperature for thermal bonding enhancer is 190°C and the load is 2.16 kg;

[0089] (2) Melting point: measured according to the method specified in GB / T 28724-2012;

[0090] (3) Tensile strength: measured according to the method specified in GB / T1040.1-2018;

[0091] (4) Drop weight impact strength: measured according to the method specified in GB / T14153-1993;

[0092] (5) Interlayer peel strength: measured according to the method specified in QB / T2358-98;

[0093] (6) Density: measured according to the method specified in GB / T 1033.1-2008;

[0094] (7) Surface density: measured according to the method specified in ASTM D1622-2020;

[0095] In the following examples, the β-crystal nucleating agent with the brand name VP101B is sourced from Beijing Research Institute of Chemical Industry of Sinopec Corporation; the sources of some raw materials are described in the examples, and the other raw materials are commercially available unless otherwise specified.

[0096] Example 1

[0097] This example is used to illustrate the preparation of the polypropylene woven composite material, polypropylene composition, three-layer co-extruded polypropylene sheet, continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape, and polypropylene flat yarn / continuous inorganic fiber fabric provided by the present invention.

[0098] (1) Preparation of polypropylene composition A:

[0099] Component a is a homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 160°C, a melt flow rate of 3.2g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry (under 23°C test conditions, the impact strength is 23KJ / m 2 ), ethylene content is 11%wt, melt flow rate is 2.0g / 10min, and melting point is 155℃.

[0100] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 80 parts by weight, and the mass fraction Wb of component b is 20 parts by weight. 0.05 parts by weight of β-crystal nucleating agent with the grade of VP101B is added. Then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 200-230°C. After the screw is melt-mixed, extruded, granulated and dried, a polypropylene composition pellet is obtained. The melt mass flow rate MFRA is detected to be 4.6 / 10min; the melting point of the polypropylene composition A is 157°C.

[0101] (2) Preparation of polypropylene composition B:

[0102] Component x is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 140°C and a melt flow rate of 6.6 g / 10 min; component y is a polyolefin elastomer with a grade of 6102, purchased from Exxon, which is an ethylene-propylene copolymer with an ethylene content of 16%wt and a melt flow rate of 1.4 g / 10 min at 190°C and a load of 2.16 kg;

[0103] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 85 parts by weight, the mass fraction Wy of component y is 15 parts by weight, and the other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained, and the melt mass flow rate MFRB is 5.2 g / 10 min, and the melting point is 138° C.;

[0104] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0105] The pellets of polypropylene composition A and polypropylene composition B obtained in the above steps (1) and (2) are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion calendering machine, and the polypropylene composition B is added to the upper and lower surface layer extruders of the multi-layer extrusion casting machine.

[0106] After the pellets are co-extruded and compounded out from the die of the extruder, they are sequentially passed through a calendering roller and a traction roller, and then subjected to solid phase stretching, edge cutting and winding, thereby obtaining the sheet.

[0107] The temperature of the extrusion casting was 230°C, and the temperature of the calendering roller was 55°C. The temperature during the solid phase stretching process was 135°C, the stretching rate was 2m / min, and the stretching ratio was 7 times. After stretching, the film was rolled up to form a polypropylene sheet (composite film), which consisted of an upper surface layer (film layer B), a core layer (film layer A) and a lower surface layer (film layer B).

[0108] The thickness of the polypropylene sheet (composite film) is 150 μm, wherein the thickness of the film layer A accounts for 80% of the total thickness of the sheet.

[0109] (4) Preparation of polypropylene flat yarn:

[0110] The three-layer co-extruded polypropylene sheet obtained in the above step (3) is cut by a high-speed slitting machine with multiple blades to obtain oriented polypropylene flat yarns with a width of 3 mm.

[0111] (5) Preparation of continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape:

[0112] Component x is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 140°C and a melt flow rate of 6.6 g / 10 min; the compatibilizer is a polypropylene-maleic anhydride grafted polymer (PP-g-MAH) with a brand name of CMG5701, purchased from Jiayirong Company; the continuous inorganic fiber is a glass fiber with a brand name of SE4805-2400tex, purchased from Owens Corning Company.

[0113] The components prepared above are weighed according to the proportion, wherein the mass fraction of component x is 35 parts by weight, the mass fraction of the compatibilizer is 5 parts by weight, and the mass fraction of the glass fiber is 60 parts by weight. The random copolymer polypropylene x and the compatibilizer are evenly mixed, melt-kneaded by a twin-screw extruder, and the melt is conveyed into an impregnation mold through a casting mold; the continuous glass fiber is led out from the creel unit, passed through a tension regulating device, a wire spreading device, and a preheating device, and then introduced into the impregnation mold, and impregnated with the melt. The outlet mold is cooled and shaped to obtain a continuous glass fiber reinforced polypropylene unidirectional prepreg tape with a thickness of 155 μm and a width of 3 mm.

[0114] (6) Preparation of polypropylene flat yarn / continuous inorganic fiber fabric:

[0115] The polypropylene flat yarn obtained in step (4) and the continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape obtained in step (5) are respectively wound at a ratio of 1:1 for weaving; the prepared warp yarn and weft yarn are formed into a polypropylene flat yarn / continuous inorganic fiber fabric in a plain weave structure on a loom with a double-sided multi-shuttle box mechanism;

[0116] (7) Preparation of polypropylene woven composite materials:

[0117] The polypropylene flat yarn / continuous inorganic fiber fabric obtained in the above step (6) is laminated and hot-pressed and fused, and then cooled and shaped to form a polypropylene woven composite material. The polypropylene woven composite material includes 24 layers of polypropylene flat yarn / continuous inorganic fiber fabric. The polypropylene flat yarn / continuous inorganic fiber fabric is placed at 90° between the warp and the warp. The hot pressing conditions used are: temperature 150°C, hot pressing pressure 5Mpa, preheating time 180s, hot pressing time 180s, and cooling time 600s. The thickness of the prepared polypropylene woven composite material is 3.6mm, and the surface density is shown in Table 1.

[0118] Example 2

[0119] This example is used to illustrate the preparation of the polypropylene woven composite material, polypropylene composition, three-layer co-extruded polypropylene sheet, continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape, and polypropylene flat yarn / continuous inorganic fiber fabric provided by the present invention.

[0120] (1) Preparation of polypropylene composition A:

[0121] Component a is homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 165°C, a melt flow rate of 8.1g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry, with an impact strength of 25KJ / m under 23°C test conditions. 2 , ethylene content is 8%wt, melt flow rate is 3.2g / 10min, and melting point is 155℃.

[0122] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 70 parts by weight, and the mass fraction Wb of component b is 30 parts by weight. 0.05 parts by weight of a β-crystal nucleating agent with the grade VP101B is added. Then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 200-230°C. After the screw is melt-mixed, extruded, granulated and dried, a polypropylene composition pellet is obtained. The melt mass flow rate MFRA is detected to be 7.3 / 10min, and the melting point of the polypropylene composition A is 161°C.

[0123] (2) Preparation of polypropylene composition B:

[0124] Component x is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 134°C, an ethylene-propylene-butene terpolymer, and a melt flow rate of 5.2 g / 10 min; component y is a polyolefin elastomer produced by Sinopec Beijing Research Institute of Chemical Industry, an ethylene-propylene copolymer, with an ethylene content of 15% wt, a melting point of 105°C, and a melt flow rate of 9 g / 10 min at 190°C and a load of 2.16 kg;

[0125] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 80 parts by weight, the mass fraction Wy of component y is 20 parts by weight, and the other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained, and its melt mass flow rate MFRB is detected to be 9.6 g / 10 min. The melting point of the polypropylene composition B is 130°C.

[0126] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0127] The preparation process is the same as step (3) of Example 1.

[0128] (4) Preparation of polypropylene flat yarn:

[0129] The preparation process is the same as step (4) of Example 1.

[0130] (5) Preparation of continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape:

[0131] The preparation process is the same as step (5) of Example 1.

[0132] (6) Preparation of polypropylene flat yarn / continuous inorganic fiber fabric:

[0133] The preparation process is the same as step (6) of Example 1.

[0134] (7) Preparation of polypropylene woven composite materials:

[0135] The preparation process is the same as step (7) of Example 1.

[0136] The thickness of the prepared polypropylene woven composite material is close to that of Example 1.

[0137] Example 3

[0138] This example is used to illustrate the preparation of the polypropylene woven composite material, polypropylene composition, three-layer co-extruded polypropylene sheet, continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape, and polypropylene flat yarn / continuous inorganic fiber fabric provided by the present invention.

[0139] (1) Preparation of polypropylene composition A:

[0140] The preparation process is the same as step (1) of Example 1.

[0141] (2) Preparation of polypropylene composition B:

[0142] The preparation process is the same as step (2) of Example 1.

[0143] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0144] The preparation process is the same as step (3) of Example 1.

[0145] (4) Preparation of polypropylene flat yarn:

[0146] The preparation process is the same as step (4) of Example 1.

[0147] (5) Preparation of continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape:

[0148] The main preparation process is the same as step (5) of Example 1, wherein the mass fraction of component x is 58 weight parts, the mass fraction of the compatibilizer is 2 weight parts, and the mass fraction of glass fiber is 40 weight parts, to obtain a continuous glass fiber reinforced polypropylene unidirectional prepreg tape with a thickness of 147 μm and a width of 3 mm.

[0149] (6) Preparation of polypropylene flat yarn / continuous inorganic fiber fabric:

[0150] The preparation process is the same as step (6) of Example 1.

[0151] (7) Preparation of polypropylene woven composite materials:

[0152] The preparation process is the same as step (7) of Example 1.

[0153] The thickness of the prepared polypropylene woven composite material is close to that in Example 1, and the surface density is shown in Table 1.

[0154] Example 4

[0155] This example is used to illustrate the preparation of the polypropylene woven composite material, polypropylene composition, three-layer co-extruded polypropylene sheet, continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape, and polypropylene flat yarn / continuous inorganic fiber fabric provided by the present invention.

[0156] (1) Preparation of polypropylene composition A:

[0157] Same as Example 1, wherein the mass fraction Wa of component a is 90 parts by weight, and the mass fraction Wb of component b is 10 parts by weight. 0.05 parts by weight of a β-crystal nucleating agent with a grade of VP101B is added. A pellet of polypropylene composition A is obtained, and its melt mass flow rate MFRA is detected to be 6.8 / 10min, and the melting point of polypropylene composition A is 158°C.

[0158] (2) Preparation of polypropylene composition B:

[0159] The same as Example 1, wherein the mass fraction Wx of component x is 90 parts by weight, the mass fraction Wy of component y is 10 parts by weight, and finally the polypropylene composition B pellets are obtained. The melt mass flow rate MFRB is 8.7 g / 10 min, and the melting point of the polypropylene composition B is 139°C.

[0160] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0161] The preparation process is the same as step (3) of Example 1.

[0162] (4) Preparation of polypropylene flat yarn:

[0163] The preparation process is the same as step (4) of Example 1.

[0164] (5) Preparation of continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape:

[0165] The preparation process is the same as step (5) of Example 1.

[0166] (6) Preparation of polypropylene flat yarn / continuous inorganic fiber fabric:

[0167] The preparation process is the same as step (6) of Example 1.

[0168] (7) Preparation of polypropylene woven composite materials:

[0169] The preparation process is the same as step (7) of Example 1.

[0170] The thickness of the prepared polypropylene woven composite material is close to that of Example 1.

[0171] Example 5

[0172] This example is used to illustrate the preparation of the polypropylene woven composite material, polypropylene composition, three-layer co-extruded polypropylene sheet, continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape, and polypropylene flat yarn / continuous inorganic fiber fabric provided by the present invention.

[0173] (1) Preparation of polypropylene composition A:

[0174] The preparation process is the same as step (1) of Example 1.

[0175] (2) Preparation of polypropylene composition B:

[0176] The preparation process is the same as step (2) of Example 1.

[0177] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0178] The main steps are the same as those of Example 1. The thickness of the polypropylene sheet is 150 μm, wherein the thickness of the film layer A accounts for 90% of the total thickness of the sheet.

[0179] (4) Preparation of polypropylene flat yarn:

[0180] The preparation process is the same as step (4) of Example 1.

[0181] (5) Preparation of continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape:

[0182] The preparation process is the same as step (5) of Example 1.

[0183] (6) Preparation of polypropylene flat yarn / continuous inorganic fiber fabric:

[0184] The preparation process is the same as step (6) of Example 1.

[0185] (7) Preparation of polypropylene woven composite materials:

[0186] The preparation process is the same as step (7) of Example 1.

[0187] The thickness of the prepared polypropylene woven composite material is close to that of Example 1.

[0188] Example 6

[0189] This example is used to illustrate the preparation of the polypropylene woven composite material, polypropylene composition, three-layer co-extruded polypropylene sheet, continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape, and polypropylene flat yarn / continuous inorganic fiber fabric provided by the present invention.

[0190] (1) Preparation of polypropylene composition A:

[0191] The preparation process is the same as step (1) of Example 1.

[0192] (2) Preparation of polypropylene composition B:

[0193] The preparation process is the same as step (2) of Example 1.

[0194] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0195] The main steps are the same as those in Example 1. The thickness of the polypropylene sheet is 150 μm, wherein the thickness of the film layer A accounts for 70% of the total thickness of the sheet.

[0196] (4) Preparation of polypropylene flat yarn:

[0197] The preparation process is the same as step (4) of Example 1.

[0198] (5) Preparation of continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape:

[0199] The preparation process is the same as step (5) of Example 1.

[0200] (6) Preparation of polypropylene flat yarn / continuous inorganic fiber fabric:

[0201] The preparation process is the same as step (6) of Example 1.

[0202] (7) Preparation of polypropylene woven composite materials:

[0203] The preparation process is the same as step (7) of Example 1.

[0204] The thickness of the prepared polypropylene woven composite material is close to that of Example 1.

[0205] Example 7

[0206] This example is used to illustrate the preparation of the polypropylene woven composite material, polypropylene composition, three-layer co-extruded polypropylene sheet, continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape, and polypropylene flat yarn / continuous inorganic fiber fabric provided by the present invention.

[0207] (1) Preparation of polypropylene composition A:

[0208] The preparation process is the same as step (1) of Example 1.

[0209] (2) Preparation of polypropylene composition B:

[0210] The preparation process is the same as step (2) of Example 1.

[0211] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0212] The preparation process is the same as step (3) of Example 1.

[0213] (4) Preparation of polypropylene flat yarn:

[0214] The preparation process is the same as step (4) of Example 1.

[0215] (5) Preparation of continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape:

[0216] The preparation process is the same as step (5) of Example 1.

[0217] (6) Preparation of polypropylene flat yarn / continuous inorganic fiber fabric:

[0218] The preparation process is the same as step (6) of Example 1. The prepared warp yarns and weft yarns are woven into a polypropylene flat yarn / continuous inorganic fiber fabric with a satin structure on a loom with a double-sided multi-shuttle box mechanism.

[0219] (7) Preparation of polypropylene woven composite materials:

[0220] The preparation process is the same as step (7) of Example 1.

[0221] The thickness of the prepared polypropylene woven composite material is close to that of Example 1.

[0222] Example 8

[0223] This example is used to illustrate the preparation of the polypropylene woven composite material, polypropylene composition, three-layer co-extruded polypropylene sheet, continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape, and polypropylene flat yarn / continuous inorganic fiber fabric provided by the present invention.

[0224] (1) Preparation of polypropylene composition A:

[0225] The preparation process is the same as step (1) of Example 1.

[0226] (2) Preparation of polypropylene composition B:

[0227] The preparation process is the same as step (2) of Example 1.

[0228] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0229] The main preparation process is the same as step (3) of Example 1. The stretching ratio of the sheet is 10 times. The thickness of the polypropylene sheet (composite film) is 135 μm.

[0230] (4) Preparation of polypropylene flat yarn:

[0231] The preparation process is the same as step (4) of Example 1.

[0232] (5) Preparation of continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape:

[0233] The preparation process is the same as step (5) of Example 1.

[0234] (6) Preparation of polypropylene flat yarn / continuous inorganic fiber fabric:

[0235] The preparation process is the same as step (6) of Example 1.

[0236] (7) Preparation of polypropylene woven composite materials:

[0237] The preparation process is the same as step (7) of Example 1.

[0238] The thickness of the prepared polypropylene woven composite material is 3.35 mm, and the surface density is shown in Table 1.

[0239] Example 9

[0240] This example is used to illustrate the preparation of the polypropylene woven composite material, the polypropylene composition, the three-layer co-extruded polypropylene sheet, the continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape, and the polypropylene / continuous inorganic fiber fabric provided by the present invention.

[0241] (1) Preparation of polypropylene composition A:

[0242] The preparation process is the same as step (1) of Example 1.

[0243] (2) Preparation of polypropylene composition B:

[0244] The preparation process is the same as step (2) of Example 1.

[0245] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0246] The preparation process is the same as step (3) of Example 1.

[0247] (4) Preparation of polypropylene flat yarn:

[0248] The preparation process is the same as step (4) of Example 1.

[0249] (5) Preparation of continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape:

[0250] The preparation process is the same as step (5) of Example 1.

[0251] (6) Preparation of polypropylene flat yarn / continuous inorganic fiber fabric:

[0252] The preparation process is the same as step (6) of Example 1.

[0253] (7) Preparation of polypropylene woven composite materials:

[0254] The main preparation process is the same as step (7) of Example 1. The polypropylene flat yarn / continuous inorganic fiber fabric is placed at an angle of 45° between the warp directions.

[0255] The thickness of the prepared polypropylene woven composite material is close to that of Example 1.

[0256] Example 10

[0257] This example is used to illustrate the preparation of the polypropylene woven composite material, polypropylene composition, three-layer co-extruded polypropylene sheet, continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape, and polypropylene flat yarn / continuous inorganic fiber fabric provided by the present invention.

[0258] (1) Preparation of polypropylene composition A:

[0259] The preparation process is the same as step (1) of Example 1.

[0260] (2) Preparation of polypropylene composition B:

[0261] The preparation process is the same as step (2) of Example 1.

[0262] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0263] The preparation process is the same as step (3) of Example 1.

[0264] (4) Preparation of polypropylene flat yarn:

[0265] The preparation process is the same as step (4) of Example 1.

[0266] (5) Preparation of continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape:

[0267] The preparation process is the same as step (5) of Example 1.

[0268] (6) Preparation of polypropylene flat yarn / continuous inorganic fiber fabric:

[0269] The preparation process is the same as step (6) of Example 1.

[0270] (7) Preparation of polypropylene woven composite materials:

[0271] The main preparation process is the same as step (7) of Example 1. The polypropylene flat yarn / continuous inorganic fiber fabric is placed in a direction of 0° between the warp directions.

[0272] The thickness of the prepared polypropylene woven composite material is close to that of Example 1.

[0273] Embodiment 11

[0274] This example is used to illustrate the preparation of the polypropylene woven composite material, polypropylene composition, three-layer co-extruded polypropylene sheet, continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape, and polypropylene flat yarn / continuous inorganic fiber fabric provided by the present invention.

[0275] (1) Preparation of polypropylene composition A:

[0276] The preparation process is the same as step (1) of Example 1.

[0277] (2) Preparation of polypropylene composition B:

[0278] The preparation process is the same as step (2) of Example 1.

[0279] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0280] The preparation process is the same as step (3) of Example 1.

[0281] (4) Preparation of polypropylene flat yarn:

[0282] The preparation process is the same as step (4) of Example 1.

[0283] (5) Preparation of continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape:

[0284] The preparation process is the same as step (5) of Example 1.

[0285] (6) Preparation of polypropylene flat yarn / continuous inorganic fiber fabric:

[0286] The preparation process is the same as step (6) of Example 1.

[0287] (7) Preparation of polypropylene woven composite materials:

[0288] The main steps are the same as those in Example 1. The hot pressing temperature is 155° C., the hot pressing pressure is 10 MPa, the preheating time is 300 s, the hot pressing time is 300 s, and the cooling time is 700 s. The thickness of the prepared polypropylene woven composite material is 3.51 mm, and the surface density is shown in Table 1.

[0289] Example 12

[0290] This example is used to illustrate the preparation of the polypropylene woven composite material, polypropylene composition, three-layer co-extruded polypropylene sheet, continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape, and polypropylene flat yarn / continuous inorganic fiber fabric provided by the present invention.

[0291] (1) Preparation of polypropylene composition A:

[0292] The preparation process is the same as step (1) of Example 1.

[0293] (2) Preparation of polypropylene composition B:

[0294] The preparation process is the same as step (2) of Example 1.

[0295] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0296] The preparation process is the same as step (3) of Example 1.

[0297] (4) Preparation of polypropylene flat yarn:

[0298] The preparation process is the same as step (4) of Example 1.

[0299] (5) Preparation of continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape:

[0300] The preparation process is the same as step (5) of Example 1.

[0301] (6) Preparation of polypropylene flat yarn / continuous inorganic fiber fabric:

[0302] The preparation process is the same as step (6) of Example 1.

[0303] (7) Preparation of polypropylene woven composite materials:

[0304] The polypropylene flat yarn / continuous inorganic fiber fabric obtained in the above step (6) is laminated and hot-pressed and fused, and then cooled and shaped to form a polypropylene woven composite material. The polypropylene woven composite material includes 48 layers of polypropylene flat yarn / continuous inorganic fiber fabric. The polypropylene flat yarn / continuous inorganic fiber fabric is placed at 90° between the warp and the warp. The hot pressing conditions used are: hot pressing temperature of 155°C, hot pressing pressure of 10Mpa, preheating time of 300s, hot pressing time of 300s, and cooling time of 700s. The thickness of the prepared polypropylene woven composite material is 7.1mm, and the surface density is shown in Table 1.

[0305] Example 13

[0306] This example is used to illustrate the preparation of the polypropylene woven composite material, polypropylene composition, three-layer co-extruded polypropylene sheet, continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape, and polypropylene flat yarn / continuous inorganic fiber fabric provided by the present invention.

[0307] (1) Preparation of polypropylene composition A:

[0308] The preparation process is the same as step (1) of Example 1.

[0309] (2) Preparation of polypropylene composition B:

[0310] The preparation process is the same as step (2) of Example 1. The difference is that component B i and x i The materials are as follows:

[0311] Component x1 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 110°C; component x2 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 115°C; component x3 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 120°C; component x4 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 125°C; component x5 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry , which is an ethylene-propylene-butene terpolymer with a melting point of 130°C; component x6 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 135°C; component x7 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 138°C; component x8 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 140°C; component x9 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 143°C; component x 10 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 145°C; component x 11 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 148°C; component x 12 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 150°C; among them, components x1-x 12 The molecular weight distribution Mw / Mn is between 7 and 10, and the components x1-x 12 The melt flow rate is 1-20g / 10min.

[0312] Finally, the polypropylene composition B is obtained. i Granules (i.e. x i +y=B i , i=1, 2, 3, 4, 5, 6, 7, 8, 9, 11, 12), after testing, the melting point of B1 is 110℃, the melting point of B2 is 113℃, the melting point of B3 is 117℃, the melting point of B4 is 123℃, the melting point of B5 is 127℃, the melting point of B6 is 133℃, the melting point of B7 is 135℃, the melting point of B8 is 137℃, the melting point of B9 is 140℃, and the melting point of B 10 The melting point of B is 142°C. 11 The melting point of B is 146℃. 12 The melting point is 148°C.

[0313] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0314] The preparation process is the same as step (3) of Example 1.

[0315] (4) Preparation of polypropylene flat yarn:

[0316] The preparation process is the same as step (4) of Example 1.

[0317] (5) Preparation of continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape:

[0318] The preparation process is the same as step (5) of Example 1.

[0319] (6) Preparation of polypropylene flat yarn / continuous inorganic fiber fabric:

[0320] The preparation process is the same as step (6) of Example 1.

[0321] (7) Preparation of polypropylene woven composite materials:

[0322] The preparation process is the same as step (7) of Example 1.

[0323] The polypropylene flat yarn / continuous inorganic fiber fabric obtained in the above step (6) is laminated and hot-pressed to fuse, and then cooled and shaped to form a polypropylene woven composite material. The polypropylene woven composite material includes 23 layers of polypropylene flat yarn / continuous inorganic fiber fabric. The polypropylene flat yarn / continuous inorganic fiber fabric is laminated in sequence, from bottom to top, in the order of B 12 A 12 B 12… B9A9B 9… B3A3B3, B2A2B2, B1A1B1, B2A2B2, B3A3B3,…B9A9B9…B 12 A 12 B 12 The polypropylene flat yarn / continuous inorganic fiber fabric is placed at 90° between the warp and the warp. The hot pressing conditions used are: temperature 150℃, hot pressing pressure 5Mpa, preheating time 180s, hot pressing time 120s, and cooling time 600s. The thickness of the prepared polypropylene woven composite material is 3.39mm, and the surface density is shown in Table 1.

[0324] Embodiment 14

[0325] This example is used to illustrate the preparation of the polypropylene woven composite material, polypropylene composition, three-layer co-extruded polypropylene sheet, continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape, and polypropylene flat yarn / continuous inorganic fiber fabric provided by the present invention.

[0326] (1) Preparation of polypropylene composition A:

[0327] The preparation process is the same as step (1) of Example 1.

[0328] (2) Preparation of polypropylene composition B:

[0329] The preparation process is the same as step (2) of Example 1. The difference is that component B i and x i The materials are as follows:

[0330] The main preparation process is the same as step (2) of Example 1. The difference is that component B i and x i The materials are as follows:

[0331] Components x1-x3 are random copolymer polypropylenes produced by Sinopec Beijing Research Institute of Chemical Industry, which are ethylene-propylene-butene terpolymers with a melting point of 120°C; components x4-x6 are random copolymer polypropylenes produced by Sinopec Beijing Research Institute of Chemical Industry, which are ethylene-propylene-butene terpolymers with a melting point of 130°C; components x7-x9 are random copolymer polypropylenes produced by Sinopec Beijing Research Institute of Chemical Industry, which are ethylene-propylene-butene terpolymers with a melting point of 140°C; components x 10 -x 12 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, an ethylene-propylene-butene terpolymer with a melting point of 150°C; wherein the molecular weight distribution Mw / Mn of components x1-x9 is all between 7-10, and the melt flow rate of components x1-x9 is all between 1-20g / 10min.

[0332] Finally, the polypropylene composition B is obtained. i Granules (i.e. x i +y=B i , i=1, 2, 3, 4, 5, 6, 7, 8, 9...12), after testing, the melting point of B1-B3 is 117℃, the melting point of B4-B6 is 127℃, and the melting point of B7-B9 is 137℃. 10 -B 12 The melting point is 148°C.

[0333] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0334] The preparation process is the same as step (3) of Example 1.

[0335] (4) Preparation of polypropylene flat yarn:

[0336] The preparation process is the same as step (4) of Example 1.

[0337] (5) Preparation of continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape:

[0338] The preparation process is the same as step (5) of Example 1.

[0339] (6) Preparation of polypropylene flat yarn / continuous inorganic fiber fabric:

[0340] The preparation process is the same as step (6) of Example 1.

[0341] (7) Preparation of polypropylene woven composite materials:

[0342] The preparation process is the same as step (7) of Example 1.

[0343] The polypropylene flat yarn / continuous inorganic fiber fabric obtained in the above step (6) is laminated and hot-pressed to fuse, and then cooled and shaped to form a polypropylene woven composite material. The polypropylene woven composite material includes 23 layers of polypropylene flat yarn / continuous inorganic fiber fabric. The polypropylene flat yarn / continuous inorganic fiber fabric is laminated in sequence, from bottom to top, in the order of B 12 A 12 B 12… B9A9B 9… B3A3B3, B2A2B2, B1A1B1, B2A2B2, B3A3B3,…B9A9B9…B 12 A 12 B 12 The polypropylene flat yarn / continuous inorganic fiber fabric is placed at 90° between the warp and the warp. The hot pressing conditions used are: temperature 150℃, hot pressing pressure 5Mpa, preheating time 180s, hot pressing time 120s, and cooling time 600s. The thickness of the prepared polypropylene woven composite material is 3.41mm, and the surface density is shown in Table 1.

[0344] Comparative Example 1

[0345] A continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape was prepared according to the method of Example 1. However, only the continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape was used as the warp and weft to prepare a polypropylene flat yarn / continuous inorganic fiber fabric. A polypropylene woven composite material was prepared according to the method of Example 1.

[0346] The thickness of the prepared polypropylene woven composite material is 3.65 mm, and the surface density is shown in Table 1.

[0347] Comparative Example 2

[0348] A continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape was prepared according to the method of Example 1. However, only the continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape was used as the weft to prepare a polypropylene flat yarn / continuous inorganic fiber fabric. A polypropylene woven composite material was prepared according to the method of Example 1.

[0349] The thickness of the prepared polypropylene woven composite material is 3.59 mm, and the surface density is shown in Table 1.

[0350] Comparative Example 3

[0351] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1. Only polypropylene composition A was used for extrusion casting into a single-layer film with a thickness of 150 μm. A continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape and a polypropylene / continuous inorganic fiber fabric were prepared according to the method of Example 1.

[0352] The thickness of the prepared polypropylene / woven composite material is close to that of Example 1.

[0353] Comparative Example 4

[0354] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1. Only the polypropylene composition B was used for extrusion casting into a single-layer film with a thickness of 150 μm. A continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape and a polypropylene / continuous inorganic fiber fabric were prepared according to the method of Example 1.

[0355] The thickness of the prepared polypropylene / woven composite material is close to that of Example 1.

[0356] Comparative Example 5

[0357] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1, except that the polypropylene composition A contained only component b. A continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape and a polypropylene / continuous inorganic fiber fabric were prepared according to the method of Example 1.

[0358] The thickness of the prepared polypropylene / woven composite material is close to that of Example 1.

[0359] Comparative Example 6

[0360] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1, except that the polypropylene composition B contained only component y. A continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape and a polypropylene / continuous inorganic fiber fabric were prepared according to the method of Example 1.

[0361] The thickness of the prepared polypropylene / woven composite material is close to that of Example 1.

[0362] Comparative Example 7

[0363] A three-layer co-extruded polypropylene sheet was prepared according to the method of Example 1, except that the thickness of the film layer A accounted for 95% of the total thickness of the sheet. A continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape and a polypropylene / continuous inorganic fiber fabric were prepared according to the method of Example 1.

[0364] The thickness of the prepared polypropylene / woven composite material is close to that of Example 1.

[0365] Comparative Example 8

[0366] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1, except that the thickness of the film layer A accounted for 50% of the total thickness of the sheet. A continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape and a polypropylene / continuous inorganic fiber fabric were prepared according to the method of Example 1.

[0367] The thickness of the prepared polypropylene / woven composite material is close to that of Example 1.

[0368] Comparative Example 9

[0369] A coextruded polypropylene sheet was prepared according to the method of Example 13, except that component B i and x i The materials are as follows:

[0370] Component x 12 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 110°C; component x 11 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 115°C; component x 10It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 120°C; component x9 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 125°C; component x8 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 130°C; component x7 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 135°C; component x6 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 138°C; component x5 is The random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry is an ethylene-propylene-butene terpolymer with a melting point of 140°C; component x4 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 143°C; component x3 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 145°C; component x2 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 148°C; component x1 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 150°C; among them, components x1-x 12 The molecular weight distribution Mw / Mn is between 7 and 10, and the components x1-x 12 The melt flow rate is 1-20g / 10min.

[0371] Finally, the polypropylene composition B is obtained. i Granules (i.e. x i +y=B i , i = 1, 2, 3, 4, 5, 6, 7, 8, 9, 11, 12), after testing, B 12 The melting point of B is 110℃. 11 The melting point of B is 113℃. 10 The melting point of B is 117℃, the melting point of B9 is 123℃, the melting point of B8 is 127℃, the melting point of B7 is 133℃, the melting point of B6 is 135℃, the melting point of B5 is 137℃, the melting point of B4 is 140℃, the melting point of B3 is 142℃, the melting point of B2 is 146℃ and the melting point of B1 is 148℃.

[0372] Experimental example

[0373] The polypropylene woven composite materials obtained in the above examples and comparative examples were tested according to the following method. The test results are shown in Table 1.

[0374] (1) Tensile strength: Prepare samples and measure them according to the method specified in GB / T1040.1-2018;

[0375] (2) Interlayer peel strength: Sample preparation and measurement shall be carried out according to the method specified in QB / T2358-98.

[0376] (3) Drop hammer impact strength: measured according to the method specified in GB / T14153-1993. The thicknesses of the polypropylene woven composite materials obtained in Examples 1-11 and Comparative Examples 3-8 are similar, about 3.6 mm, and are all within the range of 3.6 mm±1 mm.

[0377] Table 1

[0378]

[0379]

[0380] From the results of the examples in Table 1, it can be concluded that the polypropylene woven composite material prepared according to the present invention has light weight, good tensile properties and impact resistance, and has good interlayer peeling strength at a lower hot pressing temperature. The density of the polypropylene woven composite material of the present invention is ≤1200Kg / m 3 , longitudinal (MD) tensile strength ≥ 250Mpa, interlayer peel strength ≥ 1N / mm; the polypropylene woven composite material is obtained by hot pressing 24 layers of polypropylene / continuous inorganic fiber fabric, and when the thickness is about 3.6mm, the drop hammer impact strength is ≥ 150J.

[0381] It can be seen from the preferred embodiments 1-3 that the density of the polypropylene woven composite material prepared by the present invention is ≤1150Kg / m 3 , longitudinal (MD) tensile strength ≥ 270Mpa, interlayer peel strength ≥ 1.1N / mm; the polypropylene woven composite material is obtained by hot pressing 24 layers of polypropylene / continuous inorganic fiber fabric, and when the thickness is about 3.6mm, the drop hammer impact strength is ≥ 160J.

[0382] It can be seen from Comparative Examples 1-2 that the polypropylene woven composite material prepared by only using continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape as warp or weft woven fabric and laminating and hot pressing cannot achieve the density, tensile strength and impact performance of the polypropylene woven composite material in the embodiment.

[0383] It can be seen from Comparative Examples 3-8 that using only a single-layer sheet structure or using an interlayer ratio outside the scope of the embodiment will lead to a decrease in the performance of the laminated polypropylene sheet or fabric, resulting in a significant decrease in the tensile strength, impact performance or interlayer peel strength of the obtained polypropylene woven composite material.

[0384] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

[0385] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

Claims

1. A polypropylene flat yarn / continuous inorganic fiber fabric, which is a fabric formed by warp yarns and weft yarns in a plain, twill and / or satin structure; The warp yarn is a polypropylene flat yarn, and the weft yarn includes two groups of yarns, a polypropylene flat yarn and a continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape; in, The continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape contains random copolymer polypropylene x, continuous inorganic fibers and a compatibilizer; The polypropylene flat yarn comprises a layer A and layers B and B' located on both sides of the layer A, and the structure is BAB'; Layer A contains a polypropylene composition A, and the polypropylene composition A includes homopolymer polypropylene a and impact copolymer polypropylene b; layer B and layer B' are the same or different, and each contains a polypropylene composition B and a polypropylene composition B', wherein the polypropylene composition B and the polypropylene composition B' each include a random copolymer polypropylene x and a thermal bonding enhancer y; The melting point of the polypropylene composition A is greater than the melting points of the polypropylene composition B and the polypropylene composition B'.

2. The polypropylene flat yarn / continuous inorganic fiber fabric according to claim 1, characterized in that: Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 50-99wt% of homopolypropylene a and 1-50wt% of impact copolymer polypropylene b; preferably, the polypropylene composition A comprises 70-90wt% of homopolypropylene a and 10-30wt% of impact copolymer polypropylene b; and / or, Based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 70-99 wt% of random copolymer polypropylene x and 1-30 wt% of thermal adhesion enhancer y; preferably, the polypropylene composition B comprises 80-90 wt% of random copolymer polypropylene x and 10-20 wt% of thermal adhesion enhancer y.

3. The polypropylene flat yarn / continuous inorganic fiber fabric according to claim 1, characterized in that: Based on the total thickness of the polypropylene flat yarn, the thickness of the layer A accounts for 51%-89% of the total thickness, preferably 71%-89%, and more preferably 71%-80%; The melting point of the homopolymer polypropylene a in the polypropylene composition A is greater than the melting point of the random copolymer polypropylene x in the polypropylene composition B and the polypropylene composition B', and the temperature difference of the corresponding melting points is preferably greater than or equal to 10 degrees; and / or, The difference between the melting point of the polypropylene composition A and the melting point of the polypropylene composition B, and the difference between the melting point of the polypropylene composition A and the melting point of the polypropylene composition B' are each greater than or equal to 5°C, preferably greater than or equal to 10°C, more preferably greater than or equal to 20°C; and / or, And / or, the polypropylene flat yarn is obtained by co-extrusion molding, casting or calendering, and stretching the polypropylene composition A, the polypropylene composition B, and the polypropylene composition B' according to the BAB' structure to obtain a polypropylene sheet, and then slitting to obtain the polypropylene flat yarn.

4. The polypropylene flat yarn / continuous inorganic fiber fabric according to claim 1, characterized in that: The melting point of the homopolypropylene a is 160-170° C.; and / or, The homopolypropylene a has a melt flow rate of 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min at 230° C. and 2.16 kg load; and / or The isotacticity (mm) of the homopolypropylene a is not less than 96%.

5. The polypropylene flat yarn / continuous inorganic fiber fabric according to claim 1, characterized in that: The melting point of the impact-resistant copolymer polypropylene b is 150-170° C.; and / or, The monomer of the impact-resistant copolymer polypropylene b and propylene copolymer is ethylene or butene, and the content of ethylene or butene is 2-50%wt, preferably 3-20%wt, and more preferably 5-15%wt, and / or, The impact copolymer polypropylene b has a melt flow rate of 0.5-50 g / 10 min at 230° C. and a load of 2.16 kg, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or, The impact strength of the impact-resistant copolymer polypropylene b is not less than 20KJ / m 2 .

6. The polypropylene flat yarn / continuous inorganic fiber fabric according to claim 1, characterized in that: The melting point of the random copolymer polypropylene x is 120-140° C.; and / or, The random copolymer polypropylene x has a melt flow rate of 0.5-50 g / 10 min at 230° C. and a load of 2.16 kg, preferably 1-20 g / 10 min, and more preferably 3-18 g / 10 min; and / or, The random copolymer polypropylene x is a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer or a propylene-ethylene binary copolymer.

7. The polypropylene flat yarn / continuous inorganic fiber fabric according to claim 1, characterized in that: The melt flow rate of the thermal adhesion enhancer y at 190° C. and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 1-18 g / 10 min; and / or, The thermal adhesion enhancer y is selected from one or more of polyolefin elastomer, EPDM rubber, SEBS, SBS, EVA and petroleum resin; preferably, The polyolefin elastomer is a copolymer elastomer of ethylene and propylene and / or alpha olefin; further preferably, the alpha olefin is a C4-C12 alpha olefin, more preferably 1-butene and / or 1-octene; and / or, The petroleum resin is a hydrogenated petroleum resin of C5 and / or C9, preferably having a softening point of 100-150° C.; more preferably, the petroleum resin is a cyclopentadiene type resin.

8. The polypropylene flat yarn / continuous inorganic fiber fabric according to claim 1, characterized in that: The layer A also contains a β-crystalline nucleating agent; preferably, The β-crystal nucleating agent is at least one selected from the group consisting of condensed aromatic hydrocarbons, group IIA two-component complexes, aromatic diamides, rare earth compounds and cyclic dicarboxylates; and / or, Based on 100 parts by weight of the total amount of the polypropylene composition A, the content of the β-crystal nucleating agent in layer A is 0.01-0.5 parts by weight.

9. The polypropylene flat yarn / continuous inorganic fiber fabric according to any one of claims 1 to 8, characterized in that: The continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape contains, by mass, 35-58 wt% of random copolymer polypropylene x, 40-60 wt% of continuous inorganic fibers and 2-5 wt% of a compatibilizer; and / or, The continuous inorganic fiber is selected from at least one of metal wire, carbon fiber, glass fiber and ceramic fiber; and / or, The compatibilizer is selected from one or more of polypropylene-maleic anhydride grafts and polypropylene-methyl methacrylate grafts; and / or, The density of the continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape is 1500-1800 Kg / m 3 , and / or, a thickness of 150-500 μm, and / or, a width of 2-3 mm; preferably, The continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape is prepared by the following method: random copolymer polypropylene x and a compatibilizer are mixed, melt-kneaded, and cast to obtain a melt, the melt is impregnated with the continuous inorganic fiber, and the continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape is obtained by cooling and shaping.

10. A method for preparing the polypropylene flat yarn / continuous inorganic fiber fabric according to any one of claims 1 to 9, comprising: The polypropylene flat yarn is used as warp yarn, and two groups of yarns including polypropylene flat yarn and continuous inorganic fiber reinforced polypropylene unidirectional prepreg tape are used as weft yarn. The warp yarn and the weft yarn are woven in a plain, twill and / or satin structure to obtain the polypropylene flat yarn / continuous inorganic fiber fabric.

11. A polypropylene woven composite material, comprising multiple layers of hot pressed polypropylene flat yarn / continuous inorganic fiber fabric according to any one of claims 1 to 9 and / or polypropylene flat yarn / continuous inorganic fiber fabric prepared by the preparation method according to claim 10.

12. The polypropylene braided composite material according to claim 11, characterized in that: The multi-layer polypropylene flat yarn / continuous inorganic fiber fabric is stacked from top to bottom in the direction of 0-90° along the respective machine directions; and / or, The number of layers of the multi-layer polypropylene flat yarn / continuous inorganic fiber fabric is greater than or equal to 2 layers, more preferably 2-200 layers; most preferably 4-100 layers; and / or, The density of polypropylene braided composite material is less than or equal to 1200Kg / m 3 , preferably less than or equal to 1150Kg / m 3 and / or, The surface density of the polypropylene woven composite material is greater than or equal to 2000g / m 2 , more preferably 2000-50000g / m 2 ; Most preferably 15000-25000g / m 2 and / or, The longitudinal tensile strength of the polypropylene woven composite material is greater than or equal to 250 MPa, more preferably 270-500 MPa, and most preferably 270-400 MPa.

13. The polypropylene braided composite material according to claim 11, characterized in that: The polypropylene woven composite material comprises a plurality of sequentially stacked polypropylene flat yarn / continuous inorganic fiber fabric unit groups; each polypropylene flat yarn / continuous inorganic fiber fabric unit group comprises at least one identical or different polypropylene flat yarn / continuous inorganic fiber fabric unit, and the polypropylene flat yarn in each polypropylene flat yarn / continuous inorganic fiber fabric unit comprises a core layer A i and located in the core layer A i The outer layer B on both sides i , B' i , structure B i A i B' i The structure of the polypropylene woven composite material is, from bottom to top, the nth group... the ith group... the second group, the first group, the second group... the ith group... the nth group, and the total number of stacked groups of polypropylene flat yarn / continuous inorganic fiber fabric unit groups is 2n-1; i and n are both integers not less than 2, and i≤n; Among them, the core layer A of the polypropylene flat yarn in the polypropylene flat yarn / continuous inorganic fiber fabric unit i Containing polypropylene composition A i , outer layer B i With outer layer B' i The same or different, each corresponding to a polypropylene composition B i , polypropylene composition B' i , The polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , the polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than the average melting point of all outer layers in the i-1-th group.

14. The polypropylene braided composite material according to claim 13, characterized in that: Polypropylene composition A i Melting point and polypropylene composition B i The difference in melting points, polypropylene composition A i The melting point of polypropylene composition B' i The difference in melting points of each is greater than or equal to 5°C, preferably greater than or equal to 10°C, more preferably greater than or equal to 20°C; and / or, The difference between the average melting point of all outer layers of the polypropylene flat yarn in the i-th group and the average melting point of all outer layers in the i-1th group is the same or different, and each is 1-40°C, preferably 1-10°C, more preferably 1-5°C; and / or, Each group of polypropylene tape yarn / continuous inorganic fiber fabric units independently comprises 1 to 10, preferably 1 to 5, identical or different polypropylene tape yarn / continuous inorganic fiber fabric units.

15. The method for preparing the polypropylene woven composite material according to any one of claims 11 to 14, the method comprising laminating and hot-pressing a plurality of layers of the polypropylene flat yarn / continuous inorganic fiber fabric, and then cooling and shaping the laminate to form the polypropylene woven composite material; preferably, The temperature of the hot pressing fusion is 115-170°C, preferably 115-159°C, and more preferably 140-159°C; and / or, The pressure of the hot pressing fusion is 2-10Mpa; and / or, The preheating time of the hot pressing fusion is 5-600s, and the hot pressing time is 1-600s, preferably 10-500s; and / or, The cooling and shaping pressure is 2-8Mpa, and the cooling and shaping time is 30s-700s.

16. Use of the polypropylene woven composite material according to any one of claims 11 to 14 or the polypropylene woven composite material obtained by the preparation method according to claim 15 in the fields of sports protection, automobile manufacturing, military materials and consumer products.

Citation Information

Patent Citations

  • Continuous fiber reinforced thermoplastic prepreg tape braided fabric and continuous fiber reinforced thermoplastic prepreg tape plate preparation method

    CN102615839A

  • Continuous fiber-reinforced thermoplastic resin product and preparation method thereof

    CN104416912A

  • Method for manufacturing flat yarn and method for manufacturing cloth laminate

    JP2014019981A

Cited By

  • Low-temperature impact-resistant self-reinforced polypropylene bionic composite material as well as preparation method and application thereof

    CN120038996A