Cellulose solid electrolyte for lithium ion battery as well as preparation method and application of cellulose solid electrolyte
Through the preparation method of cellulose solid electrolyte, the safety and performance problems of traditional lithium-ion battery electrolytes are solved, efficient lithium-ion conduction and low-cost industrial production are achieved, and the development of the next generation of lithium-ion batteries is promoted.
Patent Information
- Application Number
- CN202411508465.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-28
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The liquid electrolytes of traditional lithium-ion batteries have problems such as flammable explosion, liquid leakage and serious side reactions. In addition, solid electrolyte materials have low room temperature conductivity, poor mechanical properties and high cost, making it difficult to achieve large-scale application.
The preparation method of cellulose solid electrolyte is adopted to remove residual moisture through an optimized process and introduce lithium salts in a directional manner. Combined with an interface optimizer, an efficient ion transmission channel is formed, which improves the conduction efficiency of lithium ions and reduces the overall quality of the battery.
It significantly improves the conduction efficiency of lithium ions, improves the mechanical performance and safety of the battery, reduces costs, and realizes the widespread application of high-performance lithium ion batteries.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of lithium ion battery solid electrolytes, and more specifically, relates to a cellulose solid electrolyte for lithium ion batteries and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries occupy an important position in the modern energy field and are widely used in various scenarios such as digital products, energy storage devices and electric vehicles. However, traditional liquid lithium-ion batteries face problems such as flammability, leakage and serious side reactions, which limit their application in fields with high safety requirements. As an alternative, solid-state electrolytes have become a research hotspot for the next generation of lithium-ion batteries due to their high safety and wide electrochemical stability window. However, traditional solid-state electrolyte materials such as sulfides, although they have good room temperature conductivity, have defects such as limited material sources, high costs, and insufficient mechanical properties, making it difficult to achieve large-scale application.
[0003] To solve this problem, the present invention proposes a method for preparing a cellulose solid electrolyte and its application in lithium-ion batteries. By optimizing the preparation process, the method can remove residual moisture while retaining the internal channels of cellulose, and at the same time introduce lithium salts in a directional manner, thereby achieving the coexistence of ion transmission channels and transmission sites, thereby significantly improving the conduction efficiency of lithium ions. In addition, the process is simple, low-cost, and easy to achieve industrial production, making this type of cellulose solid electrolyte have broad application prospects in the next generation of high-performance lithium-ion batteries. Summary of the invention
[0004] In order to solve the above-mentioned deficiencies and shortcomings of the prior art, the purpose of the present invention is to provide a preparation method and application of a cellulose solid electrolyte for lithium ion batteries, which can solve the problems of low room temperature conductivity, poor mechanical properties, high cost, etc. of traditional solid electrolytes.
[0005] Another object of the present invention is to provide a method for preparing the above-mentioned cellulose solid electrolyte.
[0006] Another object of the present invention is to provide applications of the above-mentioned cellulose solid electrolyte.
[0007] The object of the present invention is achieved by the following technical scheme: a cellulose solid electrolyte for lithium ion batteries, the cellulose solid electrolyte comprising a cellulose matrix, a lithium salt and an interface optimizer, and the mass ratio thereof is 5.0-9.0:0.5-2.0:0.5-3.0.
[0008] The cellulose is an insoluble macromolecular polysaccharide with a molecular weight of 100 Da to 20,000 Da; the lithium salt is any one of lithium hexafluorophosphate (LiPF6), lithium bis(trifluoromethanesulfonyl imide) (LiTFSI), lithium bis(fluorosulfonyl imide) (LiFSI), and lithium tetrafluoroborate (LiBF4); the interface optimizer is a mixed solvent composed of lithium salt and any one or more of fluoroethylene carbonate (FEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), ethylene glycol dimethyl ether (DME), and dioxolane (DOL), preferably lithium bis(trifluoromethanesulfonyl imide) (LiTFSI) and fluoroethylene carbonate (FEC) are mixed in a mass ratio of 1.0:2.1 to 2.9.
[0009] Cellulose is a macromolecular polysaccharide with a molecular weight of 100 Da~20,000 Da. It has high strength, high toughness and is insoluble.
[0010] Preferably, the lithium salt is LiTFSI and the interface optimizer is FEC.
[0011] Specifically, the mass ratio of cellulose, lithium salt and interface optimizer is 7.5-8.5:0.7-1.3:0.7-1.3. Preferably, the mass ratio of cellulose, lithium salt and interface optimizer is 8:1:1.
[0012] A method for preparing a cellulose solid electrolyte for lithium-ion batteries comprises the steps of uniformly dispersing cellulose in deionized water, performing solvent exchange to remove water after forming a membrane, and finally introducing lithium salt in a directional manner by soaking in a lithium salt-interface optimizer mixed solution.
[0013] The preparation method of the cellulose solid electrolyte comprises the following steps:
[0014] a) adding cellulose into water and stirring to form a uniform dispersion; b) pouring the above solution into a sand core funnel, filtering it to form a film to obtain a cellulose membrane, and controlling the amount of solution added to make the membrane thickness between 20 μm and 100 μm; c) placing the cellulose film in an oven and heating it for 30-40 minutes to remove some of the moisture; d) immersing the cellulose membrane from which some water has been removed in N,N-dimethylformamide for solvent exchange, replacing the N,N-dimethylformamide every 24 hours, and repeating the replacement three times to completely remove the water; e) The cellulose membrane after solvent exchange is used as a matrix and immersed in a mixed solution of lithium salt and interface optimizer to introduce lithium salt in a directional manner, and then post-treated to obtain the result.
[0015] The concentration of lithium salt in the mixed solution in step e) is 1.2 mol / L to 1.9 mol / L.
[0016] The post-treatment includes removing and drying the liquid on the surface of the cellulose membrane.
[0017] An application of the cellulose solid electrolyte for lithium-ion batteries is used in lithium-ion batteries. The use of the electrolyte can reduce the overall mass of the battery, thereby increasing the energy density of the battery.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1. The present invention uses cellulose to form a membrane by suction filtration, and then dries the surface of the obtained electrolyte membrane (dries part of the water), which solves the problem that the wet membrane has no strength, cannot be self-supported, and the internal channels of the dry membrane collapse.
[0020] 2. The present invention removes moisture inside the cellulose electrolyte membrane by solvent exchange. This process can remove moisture while maintaining the channel structure inside the membrane, thus preventing residual water from corroding the battery.
[0021] 3. The method used in the present invention can fill a very small amount of interface optimizer with flame retardant function into the grain boundaries inside the solid electrolyte, thereby giving the electrolyte excellent flame retardant properties while constructing a continuous ion conduction network.
[0022] 4. The abundant oxygen atoms in the cellulose electrolyte membrane of the present invention can be complexed with the lithium salt, so that the lithium salt is introduced in a directional manner during the soaking process, thereby achieving the purpose of uniformly dispersing and anchoring the lithium salt.
[0023] 5. The raw material used in the present invention is natural cellulose, whose high strength and low density properties help to alleviate the impact of lithium dendrites and reduce the overall mass of the battery, thereby improving the energy density and safety performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a battery cycle performance diagram of the cellulose solid electrolyte prepared in Example 1 and a lithium iron phosphate positive electrode.
[0025] Figure 2 This is a flow chart for preparing the electrolyte in Example 1.
[0026] Figure 3 Figure 2 shows the cycling performance of a lithium-lithium symmetric battery assembled using a cellulose solid electrolyte. DETAILED DESCRIPTION
[0027] The following is combined with Figure 2The preparation flow chart of further illustrates the content of the present invention through specific examples, but should not be construed as limiting the present invention. Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0028] Example 1
[0029] 1. Add cellulose to water and stir to form a uniform dispersion.
[0030] 2. Pour the above solution into a sand core funnel and filter it to form a film. Control the amount of solution added so that the film thickness is 100 μm.
[0031] 3. Place the above cellulose film in an oven and heat it at 60 °C for 30 min to remove some moisture.
[0032] 4. Remove the partially dried membrane completely and immerse it in DMF. Replace the DMF every 24 hours and repeat this process three times to completely remove moisture.
[0033] 5. The solvent-exchanged cellulose membrane was immersed in a mixed solution of lithium salt and interface optimizer. After 48 hours, the surface liquid was removed and wiped dry. At this time, the liquid content in the cellulose membrane was 10%. The lithium salt and interface optimizer were LiTFSI and FEC, respectively. The weight ratio of LiTFSI and FEC was 1.0:2.5, and the lithium salt concentration was 1.5 mol / L.
[0034] 6. Mix the lithium iron phosphate positive electrode material, conductive additive and binder in a mass ratio of 8:1:1, then add N-methylpyrrolidone (NMP) and stir evenly to obtain a positive electrode slurry with a certain fluidity. Apply the above positive electrode slurry on aluminum foil, and then transfer it to a 100 ℃ oven to dry NMP. Cut the dried electrode into a disc with a diameter of 12 mm to obtain a lithium iron phosphate positive electrode.
[0035] 7. Lithium-ion batteries were assembled in a glove box filled with argon gas, and the battery shell used was a 2032-type button cell assembly.
[0036] The first discharge specific capacity is 163.5 mAh / g, and the discharge specific capacity after 100 cycles is 149.7 mAh / g, with a capacity retention rate of 91.6%.
[0037] Example 2
[0038] 1. Add cellulose to water and stir to form a uniform dispersion.
[0039] 2. Pour the above solution into a sand core funnel and filter it to form a film. Control the amount of solution added so that the film thickness is 100 μm.
[0040] 3. Place the above cellulose film in an oven and heat it at 60 °C for 30 min to remove some moisture.
[0041] 4. Remove the partially dried membrane completely and immerse it in DMF. Replace the DMF every 24 hours and repeat this process three times to completely remove moisture.
[0042] 5. The solvent-exchanged cellulose membrane was immersed in a mixed solution of lithium salt and interface optimizer. After 48 hours, the surface liquid was removed and wiped dry. At this time, the liquid content in the cellulose membrane was 10%. The lithium salt and interface optimizer were LiTFSI and FEC, respectively. The weight ratio of LiTFSI and FEC was 1.0:2.9, and the lithium salt concentration was 1.5 mol / L.
[0043] 6. Mix the lithium iron phosphate positive electrode material, conductive additive and binder in a mass ratio of 7.5:0.7:0.7, then add N-methylpyrrolidone (NMP) and stir evenly to obtain a positive electrode slurry with a certain fluidity. Apply the above positive electrode slurry on aluminum foil, and then transfer it to a 100 ℃ oven to dry NMP. Cut the dried electrode into a disc with a diameter of 12 mm to obtain a lithium iron phosphate positive electrode.
[0044] 7. Lithium-ion batteries were assembled in a glove box filled with argon gas, and the battery shell used was a 2032-type button cell assembly.
[0045] The first discharge specific capacity is 163.0 mAh / g, and the discharge specific capacity after 100 cycles is 144.5 mAh / g, with a capacity retention rate of 88.7%.
[0046] Example 3
[0047] 1. Add cellulose to water and stir to form a uniform dispersion.
[0048] 2. Pour the above solution into a sand core funnel and filter it to form a film. Control the amount of solution added so that the film thickness is 100 μm.
[0049] 3. Place the above cellulose film in an oven and heat it at 60 °C for 30 min to remove some moisture.
[0050] 4. Remove the partially dried membrane completely and immerse it in DMF. Replace the DMF every 24 hours and repeat this process three times to completely remove moisture.
[0051] 5. The solvent-exchanged cellulose membrane was immersed in a mixed solution of lithium salt and interface optimizer. After 48 hours, the surface liquid was removed and wiped dry. At this time, the liquid content in the cellulose membrane was 10%. The lithium salt and interface optimizer were LiTFSI and FEC, respectively. The weight ratio of LiTFSI and FEC was 1.0:2.5, and the lithium salt concentration was 1.5 mol / L.
[0052] 6. Mix the lithium iron phosphate positive electrode material, conductive additive and binder in a mass ratio of 8.5:1.3:1.3, then add N-methylpyrrolidone (NMP) and stir evenly to obtain a positive electrode slurry with a certain fluidity. Apply the above positive electrode slurry on aluminum foil, and then transfer it to a 100 ℃ oven to dry NMP. Cut the dried electrode into a disc with a diameter of 12 mm to obtain a lithium iron phosphate positive electrode.
[0053] 7. Lithium-ion batteries were assembled in a glove box filled with argon gas, and the battery shell used was a 2032-type button cell assembly.
[0054] The first discharge specific capacity is 163.0 mAh / g, and the discharge specific capacity after 100 cycles is 143.3 mAh / g, with a capacity retention rate of 87.9%.
[0055] Example 4
[0056] 1. Add cellulose to water and stir to form a uniform dispersion.
[0057] 2. Pour the above solution into a sand core funnel and filter it to form a film. Control the amount of solution added so that the film thickness is 100 μm.
[0058] 3. Place the above cellulose film in an oven and heat it at 60 °C for 30 min to remove some moisture.
[0059] 4. Remove the partially dried membrane completely and immerse it in DMF. Replace the DMF every 24 hours and repeat this process three times to completely remove moisture.
[0060] 5. The solvent-exchanged cellulose membrane was immersed in a mixed solution of lithium salt and interface optimizer. After 48 hours, the surface liquid was removed and wiped dry. At this time, the liquid content in the cellulose membrane was 10%. The lithium salt and interface optimizer were LiTFSI and FEC, respectively. The weight ratio of LiTFSI and FEC was 1.0:2.1, and the lithium salt concentration was 1.5 mol / L.
[0061] 6. Mix the lithium iron phosphate positive electrode material, conductive additive and binder in a mass ratio of 8.0:0.7:1.0, then add N-methylpyrrolidone (NMP) and stir evenly to obtain a positive electrode slurry with a certain fluidity. Apply the above positive electrode slurry on aluminum foil, and then transfer it to a 100 ℃ oven to dry NMP. Cut the dried electrode into a disc with a diameter of 12 mm to obtain a lithium iron phosphate positive electrode.
[0062] 7. Lithium-ion batteries were assembled in a glove box filled with argon gas, and the battery shell used was a 2032-type button cell assembly.
[0063] The first discharge specific capacity is 162.8 mAh / g, and the discharge specific capacity after 100 cycles is 142.1 mAh / g, with a capacity retention rate of 87.3%.
[0064] Example 5
[0065] 1. Add cellulose to water and stir to form a uniform dispersion.
[0066] 2. Pour the above solution into a sand core funnel and filter it to form a film. Control the amount of solution added so that the film thickness is 100 μm.
[0067] 3. Place the above cellulose film in an oven and heat it at 60 °C for 30 min to remove some moisture.
[0068] 4. Remove the partially dried membrane completely and immerse it in DMF. Replace the DMF every 24 hours and repeat this process three times to completely remove moisture.
[0069] 5. The solvent-exchanged cellulose membrane was immersed in a mixed solution of lithium salt and interface optimizer. After 48 hours, the surface liquid was removed and wiped dry. At this time, the liquid content in the cellulose membrane was 10%. The lithium salt and interface optimizer were LiTFSI and FEC, respectively. The weight ratio of LiTFSI and FEC was 1.0:2.3, and the lithium salt concentration was 1.5 mol / L.
[0070] 6. Mix the lithium iron phosphate positive electrode material, conductive additive and binder in a mass ratio of 8.0:1.3:0.7, then add N-methylpyrrolidone (NMP) and stir evenly to obtain a positive electrode slurry with a certain fluidity. Apply the above positive electrode slurry on aluminum foil, and then transfer it to a 100 ℃ oven to dry NMP. Cut the dried electrode into a disc with a diameter of 12 mm to obtain a lithium iron phosphate positive electrode.
[0071] 7. Lithium-ion batteries were assembled in a glove box filled with argon gas, and the battery shell used was a 2032-type button cell assembly.
[0072] The first discharge specific capacity is 161.9 mAh / g, and the discharge specific capacity after 100 cycles is 141.0 mAh / g, with a capacity retention rate of 87.1%.
[0073] Example 6
[0074] 1. Add cellulose to water and stir to form a uniform dispersion.
[0075] 2. Pour the above solution into a sand core funnel and filter it to form a film. Control the amount of solution added so that the film thickness is 100 μm.
[0076] 3. Place the above cellulose film in an oven and heat it at 60 °C for 30 min to remove some moisture.
[0077] 4. Remove the partially dried membrane completely and immerse it in DMF. Replace the DMF every 24 hours and repeat this process three times to completely remove moisture.
[0078] 5. The solvent-exchanged cellulose membrane was immersed in a mixed solution of lithium salt and interface optimizer. After 48 hours, the surface liquid was removed and wiped dry. At this time, the liquid content in the cellulose membrane was 10%. The lithium salt and interface optimizer were LiTFSI and FEC, respectively. The weight ratio of LiTFSI and FEC was 1.0:2.7, and the lithium salt concentration was 1.5 mol / L.
[0079] 6. Mix the lithium iron phosphate positive electrode material, conductive additive and binder in a mass ratio of 8.5:1.0:1.3, then add N-methylpyrrolidone (NMP) and stir evenly to obtain a positive electrode slurry with a certain fluidity. Apply the above positive electrode slurry on aluminum foil, and then transfer it to a 100 ℃ oven to dry NMP. Cut the dried electrode into a disc with a diameter of 12 mm to obtain a lithium iron phosphate positive electrode.
[0080] 7. Lithium-ion batteries were assembled in a glove box filled with argon gas, and the battery shell used was a 2032-type button cell assembly.
[0081] The first discharge specific capacity is 161.5 mAh / g, and the discharge specific capacity after 100 cycles is 140.2 mAh / g, with a capacity retention rate of 86.8%.
[0082] Comparative Example 1
[0083] 1. Under stirring conditions, add LiTFSI to a DME / DOL mixed solution with a volume ratio of 1:1 to prepare a lithium-ion battery electrolyte with a lithium salt concentration of 1.2 mol / L~1.9 mol / L.
[0084] 2. Mix the lithium iron phosphate positive electrode material, conductive additive and binder in a mass ratio of 8:1:1, then add N-methylpyrrolidone (NMP) and stir evenly to obtain a positive electrode slurry with a certain fluidity. Apply the above positive electrode slurry on aluminum foil, and then transfer it to a 100 ℃ oven to dry NMP. Cut the dried electrode into discs with a diameter of 12 mm to obtain the lithium iron phosphate positive electrode.
[0085] 3. Lithium-ion batteries were assembled in a glove box in the order of positive battery shell, lithium iron phosphate positive electrode sheet, electrolyte, lithium sheet, negative battery shell, and the lithium-ion batteries were obtained after packaging. The first discharge capacity was 137.4 mAh / g, and the discharge capacity after 100 cycles was 125.1 mAh / g, with a capacity retention rate of 91.0%.
[0086] The lithium ion batteries assembled in Example 1 and Comparative Example 1 were tested after standing at 28°C for 2 h. During the test, they were first activated at a current density of 0.1 C for one cycle, and then charged and discharged at 0.5 C. The charge and discharge cut-off voltage was 2.5-3.8 V.
[0087] See attached Figure 1 : Figure 1 The lithium ion battery cycle performance diagram of Example 1 and Comparative Example 1. Figure 1 It can be seen that the first discharge specific capacity of the lithium-ion battery using cellulose solid electrolyte is 163.5 mAh / g, the discharge specific capacity after 100 cycles is 149.7 mAh / g, and the capacity retention rate is 91.6%.
[0088] See attached Figure 1 : Figure 1 The curve marked with hollow circles represents the coulombic efficiency of Example 1, and the curve marked with hollow triangles represents the coulombic efficiency of Comparative Example 1. The two curves show the change of coulombic efficiency in 300 cycles. Figure 1 It can be seen that the coulombic efficiency of Example 1 is almost maintained at 100%, indicating that the charge and discharge efficiency of the battery in Example 1 is very high, and there is almost no energy loss, proving that the battery has good cycle stability and energy retention capacity. However, the coulombic efficiency of Comparative Example 1 fluctuates greatly, and the cycle stability becomes poor.
[0089] It can be seen that compared with Comparative Example 1, the lithium ion battery prepared in Example 1 has higher initial discharge specific capacity, capacity retention rate and coulombic efficiency.
[0090] See attached Figure 3 : The battery cycle test results show that the cellulose solid electrolyte of the present invention can provide a continuous, fast and unobstructed ion conduction path, improve the lithium ion transfer kinetics, and thus enhance the cycle performance of lithium ion batteries.
[0091] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A cellulose solid electrolyte for lithium-ion batteries, characterized in that: The cellulose solid electrolyte comprises a cellulose matrix, a lithium salt and an interface optimizer, and the mass ratio thereof is 5.0-9.0:0.5-2.0:0.5-3.
0.
2. The cellulose solid electrolyte for lithium ion batteries according to claim 1, characterized in that: The cellulose matrix is a macromolecular polysaccharide with a molecular weight of 100 Da to 20,000 Da.
3. The cellulose solid electrolyte for lithium ion batteries according to claim 1, characterized in that: The lithium salt is any one of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide and lithium tetrafluoroborate.
4. The cellulose solid electrolyte for lithium ion batteries according to claim 1, characterized in that: The interface optimizer is a mixed solvent consisting of lithium salt and any one or more of fluoroethylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, ethylene glycol dimethyl ether, and dioxolane.
5. The cellulose solid electrolyte for lithium ion batteries according to claim 1, characterized in that: The mass ratio of the cellulose matrix, the lithium salt and the interface optimizer is 7.5-8.5:0.7-1.3:0.7-1.
3.
6. The method for preparing a cellulose solid electrolyte for lithium ion batteries according to any one of claims 1 to 5, characterized in that: The cellulose is evenly dispersed in deionized water, and after being made into a membrane, solvent exchange is performed to remove water to form a cellulose matrix. Finally, the lithium salt is directionally introduced into the cellulose matrix by soaking a lithium salt-interface optimizer mixed solution.
7. The method for preparing a cellulose solid electrolyte for lithium ion batteries according to claim 6, characterized in that: The following steps are involved: a) adding cellulose into water and stirring to form a uniform dispersion; b) pouring the above dispersion into a sand core funnel, filtering it to form a film to obtain a cellulose membrane, and controlling the amount of solution added to make the membrane thickness between 20 μm and 100 μm; c) placing the cellulose film in an oven and heating it for 30-40 minutes to remove some of the moisture; d) immersing the cellulose membrane from which some water has been removed in N,N-dimethylformamide for solvent exchange, replacing the N,N-dimethylformamide every 24 hours, and repeating the replacement three times to completely remove the water; e) The cellulose membrane after solvent exchange is used as a matrix and immersed in a mixed solution of lithium salt and interface optimizer to introduce lithium salt in a directional manner, and then post-treated to obtain the result.
8. The method for preparing a cellulose solid electrolyte for lithium ion batteries according to claim 7, characterized in that: The concentration of lithium salt in the mixed solution in step e) is 1.2 mol / L to 1.9 mol / L.
9. The use of the cellulose solid electrolyte for lithium ion batteries according to any one of claims 1 to 5, characterized in that: For lithium-ion batteries.
Citation Information
Patent Citations
Drying method of bacterial cellulose material for preparing lithium ion battery separation membrane
CN106549127A
Molecular brush polymer film based on cellulose network structure, and preparation method and application thereof
CN112072173A
Preparation method of natural cellulose-based polymer electrolyte
CN114106378A
Composite solid electrolyte membrane and preparation method and application thereof
CN117013056A
Preparation method of functionalized nano cellulose diaphragm
CN117175138A
Cited By
Solid electrolyte material and preparation method and application thereof
CN120824419A
Solid-state electrolyte material, preparation method therefor, and use thereof
CN120824419B
Sulfur-containing lithium salt solid-state electrolyte, solid-state battery and preparation method therefor, battery device and electric device
WO2026200220A1