Preparation method and application of hydrophilic polyphenylene sulfide superfine fiber pulp
By mixing sodium 1-naphthalene sulfonate with polyphenylene sulfide powder resin and melting it in a twin-screw extruder, and melt-blown spinning through a meltblown machine, the processing difficulty and poor hydrophilicity of polyphenylene sulfide material are solved. The problem is that polyphenylene sulfide microfiber pulp with high fluidity and good hydrophilicity is prepared, which improves its performance in composite materials.
Patent Information
- Application Number
- CN202410955457.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
Due to its poor hydrophilicity and high melting point, polyphenylene sulfide materials are difficult to process and have low fluidity, which affects their application in composite materials.
By mixing sodium 1-naphthalene sulfonate with polyphenylene sulfide powder resin and melting it in a twin screw extruder to form a modified masterbatch, and melt-blown spinning is carried out through a meltblown machine to generate hydrophilic polyphenylene sulfide Microfiber non-woven fabrics were then beaten to prepare polyphenylene sulfide microfiber pulp with high fluidity and good hydrophilicity.
The high flowability and good hydrophilicity of polyphenylene sulfide material are achieved, and its mechanical properties, thermal insulation properties and filtration efficiency in composite paper and composite membrane are improved. It is suitable for the preparation of high-performance composite materials.
Smart Images

Figure BDA0004948620390000141
Abstract
Description
Technical Field
[0001] The invention belongs to the field of composite materials, and more specifically, relates to a preparation method and application of hydrophilic polyphenylene sulfide ultrafine fiber pulp. Background Art
[0002] Polyphenylene sulfide is a thermoplastic polymer composed of benzene rings and sulfur atoms arranged alternately. Therefore, it has good flame retardancy, a limiting oxygen index of 34, will not drip when encountering an open flame, and will quickly extinguish after leaving the fire source. Polyphenylene sulfide has excellent chemical and solvent resistance and is almost insoluble in organic solvents at 200°C. In addition, polyphenylene sulfide has good thermal stability, processing performance, excellent mechanical properties, etc., so it is often used in aerospace, chemical industry, electronic appliances and other fields. However, it is precisely because of the alternating structure of benzene rings and sulfur atoms in polyphenylene sulfide that the sulfur atoms and benzene rings inside the polyphenylene sulfide molecule are not hydrophilic. The rigid structure of the benzene ring and the properties of the sulfur atom jointly determine that the solubility and interaction of polyphenylene sulfide in water molecules are weak, thus showing poor hydrophilicity. At the same time, due to the high melting point of polyphenylene sulfide, it is easy to undergo thermal oxidation cross-linking reaction with oxygen in the air during the melting process, resulting in reduced fluidity and increased processing difficulty.
[0003] In order to solve the above problems, in recent years, researchers have improved the hydrophilicity of polyphenylene sulfide by introducing hydrophilic groups or changing the surface properties of polyphenylene sulfide through surface activation treatment, hydrophilic modification, and compounding with other materials (such as graphene oxide). At the same time, the processing properties of polyphenylene sulfide are improved by controlling the processing conditions.
[0004] However, although surface modification technology can improve the hydrophilicity of polyphenylene sulfide, the common surface modification technology usually affects other properties of polyphenylene sulfide, such as mechanical strength and thermal stability. At the same time, the modification process may increase certain costs, and the modified polyphenylene sulfide material may not be suitable for all application scenarios that require high hydrophilicity. In addition, although lowering the processing temperature, adjusting parameters such as melt temperature and injection speed can improve the processing performance of polyphenylene sulfide, this method not only has very limited effect, but also may sacrifice other properties such as crystallinity and thermal stability. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a method for preparing hydrophilic polyphenylene sulfide ultrafine fiber pulp to solve the problems of poor hydrophilicity and great processing difficulty of polyphenylene sulfide.
[0006] To achieve the above object, in a first aspect, the present invention provides a method for preparing hydrophilic polyphenylene sulfide ultrafine fiber pulp, the preparation method comprising the following steps:
[0007] Sodium 1-naphthalenesulfonate and polyphenylene sulfide powder resin are mixed and fed into a twin-screw extruder as raw materials, and the raw materials are melted and extruded into continuous strips through the die head of the twin-screw extruder;
[0008] The strips are cut into fixed lengths to prepare polyphenylene sulfide modified masterbatches, and the polyphenylene sulfide modified masterbatches are mixed with polyphenylene sulfide resin slices to obtain a polyphenylene sulfide mixture;
[0009] After the polyphenylene sulfide mixture is dried, it is melt-blown by a melt-blown machine to obtain a hydrophilic polyphenylene sulfide ultrafine fiber non-woven fabric; wherein the temperature used by the melt-blown machine is higher than the melting point of sodium 1-naphthalenesulfonate, so that the dried polyphenylene sulfide mixture has a melting point mutation at the melt-blowing temperature, thereby achieving high fluidity;
[0010] The hydrophilic polyphenylene sulfide ultrafine fiber nonwoven fabric is subjected to pulping treatment to obtain hydrophilic polyphenylene sulfide ultrafine fiber pulp.
[0011] Furthermore, the melt index of the polyphenylene sulfide powder resin and the polyphenylene sulfide resin slices are both 80-120.
[0012] Furthermore, the sodium 1-naphthalenesulfonate and the polyphenylene sulfide powder resin are mixed in a mass ratio of 1 to 1.5:5; the polyphenylene sulfide modified masterbatch and the polyphenylene sulfide resin chips are mixed in a mass ratio of 1 to 3:100.
[0013] Furthermore, the melt index of the polyphenylene sulfide mixture used for melt-blowing at the melt-blowing temperature is 320-410; the melt-blowing temperature is 310-330°C.
[0014] Furthermore, the polyphenylene sulfide mixture is dried at 140-160° C. for 4-6 hours.
[0015] Furthermore, during the pulping process, the circulation grinding time is 10 to 120 minutes, and the slit-type sieve hole of the pressure screen used for screening is 0.2 to 0.3 mm.
[0016] Furthermore, the prepared hydrophilic polyphenylene sulfide ultrafine fiber pulp has a length of 1 to 3 mm.
[0017] In a second aspect, the present invention provides a hydrophilic polyphenylene sulfide ultrafine fiber pulp, wherein the hydrophilic polyphenylene sulfide ultrafine fiber pulp is prepared by the method for preparing the hydrophilic polyphenylene sulfide ultrafine fiber pulp according to the first aspect.
[0018] In the third aspect, the present invention provides a composite material, which is prepared from any one of polytetrafluoroethylene, carbon fiber, polyimide, PBO, para-aramid, meta-aramid and heterocyclic aramid chopped fibers and the hydrophilic polyphenylene sulfide ultrafine fiber pulp as described in the second aspect by fiber decomposition and dispersion, wet web making, drying and hot pressing processes.
[0019] In general, the above technical solutions conceived by the present invention can achieve the following beneficial effects:
[0020] 1. The present invention uses sodium 1-naphthalenesulfonate with a melting point of 300°C to be in a molten state at a melt-blowing temperature higher than the melting point, the intermolecular interaction force is weakened, the fluidity is enhanced, and the mixed slurry produces a melt index mutation at the melt-blowing temperature to achieve high fluidity, so that the melt-blown polyphenylene sulfide ultrafine fibers are finer, and successfully solves the problems of low fluidity in the melt-blowing process of polyphenylene sulfide and difficulty in processing polyphenylene sulfide pulp. The prepared hydrophilic polyphenylene sulfide ultrafine fiber pulp has the advantages of small diameter, large specific surface area, high temperature resistance and flame retardancy, and is widely used in materials such as high-performance composite paper and composite films, and can well enhance the mechanical properties, thermal insulation properties, filtration efficiency and particle capture capacity of materials such as high-performance composite paper and composite films.
[0021] 2. Sodium 1-naphthalenesulfonate is a high temperature resistant, high carbonization rate, and highly flame retardant substance. It can give polyphenylene sulfide microfiber pulp higher flame retardancy and burning resistance, and can be used in some fireproof materials.
[0022] 3. Sodium 1-naphthalenesulfonate has good hydrophilicity. Due to the addition of sodium 1-naphthalenesulfonate, the prepared polyphenylene sulfide ultrafine fiber pulp also has good hydrophilicity, which effectively solves the problem of poor dispersibility of polyphenylene sulfide ultrafine fiber pulp and avoids the problems of excessive foam and uneven dispersion in the preparation of pulp due to the hydrophobicity of polyphenylene sulfide.
[0023] 4. Sodium 1-naphthalenesulfonate is an anionic surfactant that can enhance the electrostatic interaction between polyphenylene sulfide fibers, successfully solving the problem caused by static electricity that may be generated during the processing of polyphenylene sulfide pulp, avoiding the problem of fiber aggregation caused by static electricity of polyphenylene sulfide fibers, and further improving the product quality and processing efficiency of hydrophilic polyphenylene sulfide ultrafine fiber pulp. DETAILED DESCRIPTION
[0024] In order to make the technical scheme, purpose and advantages of the present invention more clearly understood, the following is a specific description of a method for preparing a hydrophilic polyphenylene sulfide ultrafine fiber pulp provided by the present invention in combination with specific embodiments, and the application of the pulp in the preparation of aramid composite paper and polytetrafluoroethylene composite paper is described. It should be understood that the following embodiments are only used to explain the present invention and are not intended to limit the scope of the present invention.
[0025] Embodiment 1:
[0026] A method for preparing hydrophilic polyphenylene sulfide ultrafine fiber pulp, the specific implementation steps are as follows:
[0027] Step 1, mixing sodium 1-naphthalenesulfonate with a melting point of 300°C and a polyphenylene sulfide powder resin with a melt index of 80 (300°C test) at a mass ratio of (1:5), feeding the mixed raw materials into a twin-screw extruder, the raw materials melt at a high temperature of 300°C and are extruded into continuous strips through the die head of the extruder. Subsequently, a granulator is used to cut the strips into a fixed length to prepare a polyphenylene sulfide modified masterbatch. The polyphenylene sulfide modified masterbatch is mixed with a polyphenylene sulfide resin slice with a melt index of 80 at a mass ratio of (1:100) to obtain a polyphenylene sulfide mixture.
[0028] Step 2, drying the polyphenylene sulfide mixture obtained in step 1 at 140° C. for 4 hours, conveying it to the screw extruder of the meltblown nonwoven machine, and entering the melt pipeline after compaction and plasticization, screw melting, and filtering by the filter, wherein the filter mesh number of the filter is 200 meshes. Subsequently, the mixture is extruded through a spinneret and connected to a condensation curtain to form a net, thereby obtaining a hydrophilic polyphenylene sulfide ultrafine fiber nonwoven fabric. Among them, the melt index of the polyphenylene sulfide mixture used for melt blowing is 320 at the melt blowing temperature, and the melt blowing temperature is 310°C. The dried polyphenylene sulfide mixture has a melt index mutation at the melt blowing temperature to achieve high fluidity; the speed of the metering pump during the feeding process is 10rpm, the feeding zone temperature of the screw barrel during the melt extrusion process is 320°C, the compression zone temperature is 320°C, the melting zone temperature is 320°C, the top nozzle temperature is 320°C, the hot air temperature is 330°C, the side blowing rate during the cooling process is 0.4m / s, the melt blowing receiving distance is 60cm, and the laying rate is 0.lmin.
[0029] Step 3, add 30L of water to the cleaned Wali beater, turn on the Wali beater for cyclic grinding, and the cyclic grinding time is 10 minutes. The polyphenylene sulfide slurry obtained by grinding is sieved using a slit-type pressure screen with a pore size of 0.2 mm to obtain hydrophilic polyphenylene sulfide ultrafine fiber pulp with a length of 1 to 3 mm.
[0030] The pulp is further used to prepare para-aramid composite paper, and the specific implementation steps are as follows:
[0031] Step 4, weigh 2.4g polyethylene oxide and 0.4g anionic polyacrylamide into a beaker containing 1.6L water, and place the beaker in a magnetic stirrer and stir at 600rpm / min for 6 hours to obtain a dispersant for standby use. Weigh 3.456g hydrophilic polyphenylene sulfide superfine fiber pulp and 8.064g para-aramid short fibers, first decompose the weighed hydrophilic polyphenylene sulfide superfine fiber pulp in a fiber decompressor for 20min, the fiber decompressor impeller speed is 5010rpm / min, the decompressed hydrophilic polyphenylene sulfide superfine fiber pulp and the weighed para-aramid short fibers are mixed in water, poured into the fiber decompressor for decompression three times, each decompression for 20min, the fiber decompressor impeller speed is 5010rpm / min, and the hydrophilic polyphenylene sulfide superfine fiber / para-aramid short fiber composite slurry can be obtained. The composite slurry was mixed evenly with the prepared dispersant in advance and poured into a paper sheet former to form a sheet. After dehydration, a wet hydrophilic polyphenylene sulfide ultrafine fiber / para-aramid short fiber composite paper with a size of 0.096 m2 and a gram weight of 120 g / m2 was obtained. The paper was then placed in a 60°C forced air drying oven and dried for 8 hours to obtain a hydrophilic polyphenylene sulfide ultrafine fiber / para-aramid short fiber composite paper base paper.
[0032] Step 5, placing the hydrophilic polyphenylene sulfide superfine fiber / para-aramid short fiber composite paper base paper into a precision roller press for the first hot pressing treatment, the parameters are: pressure 0.1MPa, temperature 120°C, and extrusion roller speed 0.5m / min, so that the hydrophilic polyphenylene sulfide superfine fiber is slightly melted and tightly attached to the surface of the para-aramid short fiber; after completion, the temperature of the precision roller press is increased to 180°C, the pressure and the extrusion roller speed remain unchanged, and the composite paper after the first hot rolling treatment is hot pressed again to further melt and expand the hydrophilic polyphenylene sulfide superfine fiber, better wrap the para-aramid short fiber, and increase the contact area between the two; after completion, the temperature of the precision roller press is increased to 300°C, the pressure and the extrusion roller speed remain unchanged, and the third hot pressing treatment is performed to completely melt the hydrophilic polyphenylene sulfide superfine fiber and restore the room temperature after hot pressing to quickly plasticize and set. After completion, the hydrophilic polyphenylene sulfide superfine fiber / para-aramid short fiber composite paper is obtained.
[0033] Embodiment 2:
[0034] A method for preparing hydrophilic polyphenylene sulfide ultrafine fiber pulp, the specific implementation steps are as follows:
[0035] Step 1, mixing sodium 1-naphthalenesulfonate with a melting point of 300°C and a polyphenylene sulfide powder resin with a melt index of 100 (300°C test) at a mass ratio of (1.2:5), feeding the mixed raw materials into a twin-screw extruder, the raw materials melt at a high temperature of 300°C and are extruded into continuous strips through the die head of the extruder. Subsequently, a granulator is used to cut the strips into a fixed length to prepare a polyphenylene sulfide modified masterbatch. The polyphenylene sulfide modified masterbatch is mixed with a polyphenylene sulfide resin slice with a melt index of 100 at a mass ratio of (2:100) to obtain a polyphenylene sulfide mixture.
[0036] Step 2, drying the polyphenylene sulfide mixture obtained in step 1 at 150° C. for 5 hours, conveying it to the screw extruder of the meltblown nonwoven machine, and entering the melt pipeline after compaction and plasticization, screw melting, and filtering by the filter, wherein the filter mesh number of the filter is 200 meshes. Subsequently, the mixture is extruded through a spinneret and connected to a condensation curtain to form a net, thereby obtaining a hydrophilic polyphenylene sulfide ultrafine fiber nonwoven fabric. Among them, the melt index of the polyphenylene sulfide mixture used for melt blowing is 360 at the melt blowing temperature, and the melt blowing temperature is 320°C. The dried polyphenylene sulfide mixture has a melt index mutation at the melt blowing temperature to achieve high fluidity; the speed of the metering pump during the feeding process is 10rpm, the feeding zone temperature of the screw barrel during the melt extrusion process is 320°C, the compression zone temperature is 320°C, the melting zone temperature is 320°C, the top nozzle temperature is 320°C, the hot air temperature is 330°C, the side blowing rate during the cooling process is 0.4m / s, the melt blowing receiving distance is 60cm, and the laying rate is 0.lmin.
[0037] Step 3, add 30L of water to the cleaned Wali beater, turn on the Wali beater for cyclic grinding, and the cyclic grinding time is 60min. The polyphenylene sulfide slurry obtained by grinding is sieved with a slit-type pressure screen with a pore size of 0.25mm to obtain hydrophilic polyphenylene sulfide ultrafine fiber pulp with a length of 1 to 3mm.
[0038] The pulp is further used to prepare para-aramid composite paper, and the specific implementation steps are as follows:
[0039] Step 4, weigh 2.4g polyethylene oxide and 0.4g anionic polyacrylamide into a beaker containing 1.6L water, and place the beaker in a magnetic stirrer and stir at 600rpm / min for 6 hours to obtain a dispersant for standby use. Weigh 3.456g hydrophilic polyphenylene sulfide superfine fiber pulp and 8.064g para-aramid short fibers, first decompose the weighed hydrophilic polyphenylene sulfide superfine fiber pulp in a fiber decompressor for 20min, the fiber decompressor impeller speed is 5010rpm / min, the decompressed hydrophilic polyphenylene sulfide superfine fiber pulp and the weighed para-aramid short fibers are mixed in water, poured into the fiber decompressor for decompression three times, each decompression for 20min, the fiber decompressor impeller speed is 5010rpm / min, and the hydrophilic polyphenylene sulfide superfine fiber / para-aramid short fiber composite slurry can be obtained. The composite slurry was mixed evenly with the prepared dispersant in advance and poured into a paper sheet former to form a sheet. After dehydration, a wet hydrophilic polyphenylene sulfide ultrafine fiber / para-aramid short fiber composite paper with a size of 0.096 m2 and a gram weight of 120 g / m2 was obtained. The paper was then placed in a 60°C forced air drying oven and dried for 8 hours to obtain a hydrophilic polyphenylene sulfide ultrafine fiber / para-aramid short fiber composite paper base paper.
[0040] Step 5, placing the hydrophilic polyphenylene sulfide superfine fiber / para-aramid short fiber composite paper base paper into a precision roller press for the first hot pressing treatment, the parameters are: pressure 0.1MPa, temperature 120°C, and extrusion roller speed 0.5m / min, so that the hydrophilic polyphenylene sulfide superfine fiber is slightly melted and tightly attached to the surface of the para-aramid short fiber; after completion, the temperature of the precision roller press is increased to 180°C, the pressure and the extrusion roller speed remain unchanged, and the composite paper after the first hot rolling treatment is hot pressed again to further melt and expand the hydrophilic polyphenylene sulfide superfine fiber, better wrap the para-aramid short fiber, and increase the contact area between the two; after completion, the temperature of the precision roller press is increased to 300°C, the pressure and the extrusion roller speed remain unchanged, and the third hot pressing treatment is performed to completely melt the hydrophilic polyphenylene sulfide superfine fiber and restore the room temperature after hot pressing to quickly plasticize and set. After completion, the hydrophilic polyphenylene sulfide superfine fiber / para-aramid short fiber composite paper is obtained.
[0041] Embodiment 3:
[0042] A method for preparing hydrophilic polyphenylene sulfide ultrafine fiber pulp, the specific implementation steps are as follows:
[0043] Step 1, 1-naphthalene sodium sulfonate with a melting point of 300°C and a polyphenylene sulfide powder resin with a melt index of 120 (300°C test) are mixed in a mass ratio of (1.5:5), and the mixed raw materials are fed into a twin-screw extruder, and the raw materials are melted at a high temperature of 300°C and extruded into continuous strips through the die head of the extruder. Subsequently, a granulator is used to cut the strips into a fixed length to prepare a polyphenylene sulfide modified masterbatch. The polyphenylene sulfide modified masterbatch is mixed with a polyphenylene sulfide resin slice with a melt index of 120 in a mass ratio of (3:100) to obtain a polyphenylene sulfide mixture.
[0044] Step 2, drying the polyphenylene sulfide mixture obtained in step 1 at 160° C. for 6 hours, conveying it to the screw extruder of the meltblown nonwoven machine, and entering the melt pipeline after compaction and plasticization, screw melting, and filtering by the filter, wherein the filter mesh number of the filter is 200 meshes. Subsequently, the mixture is extruded through a spinneret and connected to a condensation curtain to form a net, thereby obtaining a hydrophilic polyphenylene sulfide ultrafine fiber nonwoven fabric. Among them, the melt index of the polyphenylene sulfide mixture used for melt blowing is 410 at the melt blowing temperature, and the melt blowing temperature is 330°C. The dried polyphenylene sulfide mixture has a melt index mutation at the melt blowing temperature to achieve high fluidity; the speed of the metering pump during the feeding process is 10rpm, the feeding zone temperature of the screw barrel during the melt extrusion process is 320°C, the compression zone temperature is 320°C, the melting zone temperature is 320°C, the top nozzle temperature is 320°C, the hot air temperature is 330°C, the side blowing rate during the cooling process is 0.4m / s, the melt blowing receiving distance is 60cm, and the laying rate is 0.lmin.
[0045] Step 3, add 30L of water to the cleaned Wali beater, turn on the Wali beater for cyclic grinding, and the cyclic grinding time is 120min. The polyphenylene sulfide slurry obtained by grinding is sieved with a slit-type pressure screen with a pore size of 0.3mm to obtain hydrophilic polyphenylene sulfide ultrafine fiber pulp with a length of 1 to 3mm.
[0046] The pulp is further used to prepare para-aramid composite paper, and the specific implementation steps are as follows:
[0047] Step 4, weigh 2.4g polyethylene oxide and 0.4g anionic polyacrylamide into a beaker containing 1.6L water, and place the beaker in a magnetic stirrer and stir at 600rpm / min for 6 hours to obtain a dispersant for standby use. Weigh 3.456g hydrophilic polyphenylene sulfide superfine fiber pulp and 8.064g para-aramid short fibers, first decompose the weighed hydrophilic polyphenylene sulfide superfine fiber pulp in a fiber decompressor for 20min, the fiber decompressor impeller speed is 5010rpm / min, the decompressed hydrophilic polyphenylene sulfide superfine fiber pulp and the weighed para-aramid short fibers are mixed in water, poured into the fiber decompressor for decompression three times, each decompression for 20min, the fiber decompressor impeller speed is 5010rpm / min, and the hydrophilic polyphenylene sulfide superfine fiber / para-aramid short fiber composite slurry can be obtained. The composite slurry was mixed evenly with the prepared dispersant in advance and poured into a paper sheet former to form a sheet. After dehydration, a wet hydrophilic polyphenylene sulfide ultrafine fiber / para-aramid short fiber composite paper with a size of 0.096 m2 and a gram weight of 120 g / m2 was obtained. The paper was then placed in a 60°C forced air drying oven and dried for 8 hours to obtain a hydrophilic polyphenylene sulfide ultrafine fiber / para-aramid short fiber composite paper base paper.
[0048] Step 5, placing the hydrophilic polyphenylene sulfide superfine fiber / para-aramid short fiber composite paper base paper into a precision roller press for the first hot pressing treatment, the parameters are: pressure 0.1MPa, temperature 120°C, and extrusion roller speed 0.5m / min, so that the hydrophilic polyphenylene sulfide superfine fiber is slightly melted and tightly attached to the surface of the para-aramid short fiber; after completion, the temperature of the precision roller press is increased to 180°C, the pressure and the extrusion roller speed remain unchanged, and the composite paper after the first hot rolling treatment is hot pressed again to further melt and expand the hydrophilic polyphenylene sulfide superfine fiber, better wrap the para-aramid short fiber, and increase the contact area between the two; after completion, the temperature of the precision roller press is increased to 300°C, the pressure and the extrusion roller speed remain unchanged, and the third hot pressing treatment is performed to completely melt the hydrophilic polyphenylene sulfide superfine fiber and restore the room temperature after hot pressing to quickly plasticize and set. After completion, the hydrophilic polyphenylene sulfide superfine fiber / para-aramid short fiber composite paper is obtained.
[0049] Embodiment 4:
[0050] A method for preparing hydrophilic polyphenylene sulfide ultrafine fiber pulp, the specific implementation steps are as follows:
[0051] Step 1, mixing sodium 1-naphthalenesulfonate with a melting point of 300°C and a polyphenylene sulfide powder resin with a melt index of 80 (300°C test) at a mass ratio of (1:5), feeding the mixed raw materials into a twin-screw extruder, the raw materials melt at a high temperature of 300°C and are extruded into continuous strips through the die head of the extruder. Subsequently, a granulator is used to cut the strips into a fixed length to prepare a polyphenylene sulfide modified masterbatch. The polyphenylene sulfide modified masterbatch is mixed with a polyphenylene sulfide resin slice with a melt index of 80 at a mass ratio of (1:100) to obtain a polyphenylene sulfide mixture.
[0052] Step 2, drying the polyphenylene sulfide mixture obtained in step 1 at 140° C. for 4 hours, conveying it to the screw extruder of the meltblown nonwoven machine, and entering the melt pipeline after compaction and plasticization, screw melting, and filtering by the filter, wherein the filter mesh number of the filter is 200 meshes. Subsequently, the mixture is extruded through a spinneret and connected to a condensation curtain to form a net, thereby obtaining a hydrophilic polyphenylene sulfide ultrafine fiber nonwoven fabric. Among them, the melt index of the polyphenylene sulfide mixture used for melt blowing is 320 at the melt blowing temperature, and the melt blowing temperature is 310°C. The dried polyphenylene sulfide mixture has a melt index mutation at the melt blowing temperature to achieve high fluidity; the speed of the metering pump during the feeding process is 10rpm, the feeding zone temperature of the screw barrel during the melt extrusion process is 320°C, the compression zone temperature is 320°C, the melting zone temperature is 320°C, the top nozzle temperature is 320°C, the hot air temperature is 330°C, the side blowing rate during the cooling process is 0.4m / s, the melt blowing receiving distance is 60cm, and the laying rate is 0.lmin.
[0053] Step 3, add 30L of water to the cleaned Wali beater, turn on the Wali beater for cyclic grinding, and the cyclic grinding time is 10 minutes. The polyphenylene sulfide slurry obtained by grinding is sieved using a slit-type pressure screen with a pore size of 0.2 mm to obtain hydrophilic polyphenylene sulfide ultrafine fiber pulp with a length of 1 to 3 mm.
[0054] The pulp is further used to prepare polytetrafluoroethylene composite paper, and the specific implementation steps are as follows:
[0055] Step 4, weigh 2.4g polyethylene oxide and 0.4g anionic polyacrylamide and put them into a beaker filled with 1.6L water, and place the beaker in a magnetic stirrer and stir at 600rpm / min for 6 hours to obtain a dispersant for standby use. Weigh 3.456g hydrophilic polyphenylene sulfide superfine fiber pulp and 8.064g PTFE fiber, first decompose the weighed hydrophilic polyphenylene sulfide superfine fiber pulp in a fiber decompressor for 20min, the fiber decompressor stirring impeller speed is 5010rpm / min, the decompressed hydrophilic polyphenylene sulfide superfine fiber pulp and the weighed PTFE fiber are mixed in water, poured into the fiber decompressor for decompression three times, each decompression for 20min, the fiber decompressor stirring impeller speed is 5010rpm / min, and the hydrophilic polyphenylene sulfide superfine fiber / PTFE composite slurry can be obtained. The composite slurry was mixed evenly with the prepared dispersant in advance and poured into a paper sheet former to form a sheet. After dehydration, a wet hydrophilic polyphenylene sulfide superfine fiber / PTFE composite paper with a size of 0.096 m2 and a gram weight of 120 g / m2 was obtained. The paper was then placed in a 60°C forced air drying oven and dried for 8 hours to obtain a hydrophilic polyphenylene sulfide superfine fiber / PTFE composite paper base paper.
[0056] Step 5, placing the hydrophilic polyphenylene sulfide superfine fiber / PTFE composite paper base paper into a precision roller press for the first hot pressing treatment, the parameters are: pressure 0.1MPa, temperature 120°C, and extrusion roller speed 0.5m / min, so that the hydrophilic polyphenylene sulfide superfine fiber is slightly melted and tightly attached to the surface of the PTFE fiber; after completion, the temperature of the precision roller press is increased to 180°C, the pressure and the extrusion roller speed remain unchanged, and the composite paper after the first hot rolling treatment is hot pressed again to further melt and expand the hydrophilic polyphenylene sulfide superfine fiber, better wrap the PTFE fiber, and increase the contact area between the two; after completion, the temperature of the precision roller press is increased to 300°C, the pressure and the extrusion roller speed remain unchanged, and the third hot pressing treatment is performed to completely melt the hydrophilic polyphenylene sulfide superfine fiber and restore it to room temperature after hot pressing to quickly plasticize and set. After completion, the hydrophilic polyphenylene sulfide superfine fiber / PTFE composite paper is obtained.
[0057] Embodiment 5:
[0058] A method for preparing hydrophilic polyphenylene sulfide ultrafine fiber pulp, the specific implementation steps are as follows:
[0059] Step 1, mixing sodium 1-naphthalenesulfonate with a melting point of 300°C and a polyphenylene sulfide powder resin with a melt index of 100 (300°C test) at a mass ratio of (1.2:5), feeding the mixed raw materials into a twin-screw extruder, the raw materials melt at a high temperature of 300°C and are extruded into continuous strips through the die head of the extruder. Subsequently, a granulator is used to cut the strips into a fixed length to prepare a polyphenylene sulfide modified masterbatch. The polyphenylene sulfide modified masterbatch is mixed with a polyphenylene sulfide resin slice with a melt index of 100 at a mass ratio of (2:100) to obtain a polyphenylene sulfide mixture.
[0060] Step 2, drying the polyphenylene sulfide mixture obtained in step 1 at 150° C. for 5 hours, conveying it to the screw extruder of the meltblown nonwoven machine, and entering the melt pipeline after compaction and plasticization, screw melting, and filtering by the filter, wherein the filter mesh number of the filter is 200 meshes. Subsequently, the mixture is extruded through a spinneret and connected to a condensation curtain to form a net, thereby obtaining a hydrophilic polyphenylene sulfide ultrafine fiber nonwoven fabric. Among them, the melt index of the polyphenylene sulfide mixture used for melt blowing is 360 at the melt blowing temperature, and the melt blowing temperature is 320°C. The dried polyphenylene sulfide mixture has a melt index mutation at the melt blowing temperature to achieve high fluidity; the speed of the metering pump during the feeding process is 10rpm, the feeding zone temperature of the screw barrel during the melt extrusion process is 320°C, the compression zone temperature is 320°C, the melting zone temperature is 320°C, the top nozzle temperature is 320°C, the hot air temperature is 330°C, the side blowing rate during the cooling process is 0.4m / s, the melt blowing receiving distance is 60cm, and the laying rate is 0.lmin.
[0061] Step 3, add 30L of water to the cleaned Wali beater, turn on the Wali beater for cyclic grinding, and the cyclic grinding time is 60min. The polyphenylene sulfide slurry obtained by grinding is sieved with a slit-type pressure screen with a pore size of 0.25mm to obtain hydrophilic polyphenylene sulfide ultrafine fiber pulp with a length of 1 to 3mm.
[0062] The pulp is further used to prepare polytetrafluoroethylene composite paper, and the specific implementation steps are as follows:
[0063] Step 4, weigh 2.4g polyethylene oxide and 0.4g anionic polyacrylamide and put them into a beaker filled with 1.6L water, and place the beaker in a magnetic stirrer and stir at 600rpm / min for 6 hours to obtain a dispersant for standby use. Weigh 3.456g hydrophilic polyphenylene sulfide superfine fiber pulp and 8.064g PTFE fiber, first decompose the weighed hydrophilic polyphenylene sulfide superfine fiber pulp in a fiber decompressor for 20min, the fiber decompressor stirring impeller speed is 5010rpm / min, the decompressed hydrophilic polyphenylene sulfide superfine fiber pulp and the weighed PTFE fiber are mixed in water, poured into the fiber decompressor for decompression three times, each decompression for 20min, the fiber decompressor stirring impeller speed is 5010rpm / min, and the hydrophilic polyphenylene sulfide superfine fiber / PTFE composite slurry can be obtained. The composite slurry was mixed evenly with the prepared dispersant in advance and poured into a paper sheet former to form a sheet. After dehydration, a wet hydrophilic polyphenylene sulfide superfine fiber / PTFE composite paper with a size of 0.096 m2 and a gram weight of 120 g / m2 was obtained. The paper was then placed in a 60°C forced air drying oven and dried for 8 hours to obtain a hydrophilic polyphenylene sulfide superfine fiber / PTFE composite paper base paper.
[0064] Step 5, placing the hydrophilic polyphenylene sulfide superfine fiber / PTFE composite paper base paper into a precision roller press for the first hot pressing treatment, the parameters are: pressure 0.1MPa, temperature 120°C, and extrusion roller speed 0.5m / min, so that the hydrophilic polyphenylene sulfide superfine fiber is slightly melted and tightly attached to the surface of the PTFE fiber; after completion, the temperature of the precision roller press is increased to 180°C, the pressure and the extrusion roller speed remain unchanged, and the composite paper after the first hot rolling treatment is hot pressed again to further melt and expand the hydrophilic polyphenylene sulfide superfine fiber, better wrap the PTFE fiber, and increase the contact area between the two; after completion, the temperature of the precision roller press is increased to 300°C, the pressure and the extrusion roller speed remain unchanged, and the third hot pressing treatment is performed to completely melt the hydrophilic polyphenylene sulfide superfine fiber and restore it to room temperature after hot pressing to quickly plasticize and set. After completion, the hydrophilic polyphenylene sulfide superfine fiber / PTFE composite paper is obtained.
[0065] Embodiment 6:
[0066] A method for preparing hydrophilic polyphenylene sulfide ultrafine fiber pulp, the specific implementation steps are as follows:
[0067] Step 1, 1-naphthalene sodium sulfonate with a melting point of 300°C and a polyphenylene sulfide powder resin with a melt index of 120 (300°C test) are mixed in a mass ratio of (1.5:5), and the mixed raw materials are fed into a twin-screw extruder, and the raw materials are melted at a high temperature of 300°C and extruded into continuous strips through the die head of the extruder. Subsequently, a granulator is used to cut the strips into a fixed length to prepare a polyphenylene sulfide modified masterbatch. The polyphenylene sulfide modified masterbatch is mixed with a polyphenylene sulfide resin slice with a melt index of 120 in a mass ratio of (3:100) to obtain a polyphenylene sulfide mixture.
[0068] Step 2, drying the polyphenylene sulfide mixture obtained in step 1 at 160° C. for 6 hours, conveying it to the screw extruder of the meltblown nonwoven machine, and entering the melt pipeline after compaction and plasticization, screw melting, and filtering by the filter, wherein the filter mesh number of the filter is 200 meshes. Subsequently, the mixture is extruded through a spinneret and connected to a condensation curtain to form a net, thereby obtaining a hydrophilic polyphenylene sulfide ultrafine fiber nonwoven fabric. Among them, the melt index of the polyphenylene sulfide mixture used for melt blowing is 410 at the melt blowing temperature, and the melt blowing temperature is 330°C. The dried polyphenylene sulfide mixture has a melt index mutation at the melt blowing temperature to achieve high fluidity; the speed of the metering pump during the feeding process is 10rpm, the feeding zone temperature of the screw barrel during the melt extrusion process is 320°C, the compression zone temperature is 320°C, the melting zone temperature is 320°C, the top nozzle temperature is 320°C, the hot air temperature is 330°C, the side blowing rate during the cooling process is 0.4m / s, the melt blowing receiving distance is 60cm, and the laying rate is 0.lmin.
[0069] Step 3, add 30L of water to the cleaned Wali beater, turn on the Wali beater for cyclic grinding, and the cyclic grinding time is 120min. The polyphenylene sulfide slurry obtained by grinding is sieved with a slit-type pressure screen with a pore size of 0.3mm to obtain hydrophilic polyphenylene sulfide ultrafine fiber pulp with a length of 1 to 3mm.
[0070] The pulp is further used to prepare polytetrafluoroethylene composite paper, and the specific implementation steps are as follows:
[0071] Step 4, weigh 2.4g polyethylene oxide and 0.4g anionic polyacrylamide and put them into a beaker filled with 1.6L water, and place the beaker in a magnetic stirrer and stir at 600rpm / min for 6 hours to obtain a dispersant for standby use. Weigh 3.456g hydrophilic polyphenylene sulfide superfine fiber pulp and 8.064g PTFE fiber, first decompose the weighed hydrophilic polyphenylene sulfide superfine fiber pulp in a fiber decompressor for 20min, the fiber decompressor stirring impeller speed is 5010rpm / min, the decompressed hydrophilic polyphenylene sulfide superfine fiber pulp and the weighed PTFE fiber are mixed in water, poured into the fiber decompressor for decompression three times, each decompression for 20min, the fiber decompressor stirring impeller speed is 5010rpm / min, and the hydrophilic polyphenylene sulfide superfine fiber / PTFE composite slurry can be obtained. The composite slurry was mixed evenly with the prepared dispersant in advance and poured into a paper sheet former to form a sheet. After dehydration, a wet hydrophilic polyphenylene sulfide superfine fiber / PTFE composite paper with a size of 0.096 m2 and a gram weight of 120 g / m2 was obtained. The paper was then placed in a 60°C forced air drying oven and dried for 8 hours to obtain a hydrophilic polyphenylene sulfide superfine fiber / PTFE composite paper base paper.
[0072] Step 5, placing the hydrophilic polyphenylene sulfide superfine fiber / PTFE composite paper base paper into a precision roller press for the first hot pressing treatment, the parameters are: pressure 0.1MPa, temperature 120°C, and extrusion roller speed 0.5m / min, so that the hydrophilic polyphenylene sulfide superfine fiber is slightly melted and tightly attached to the surface of the PTFE fiber; after completion, the temperature of the precision roller press is increased to 180°C, the pressure and the extrusion roller speed remain unchanged, and the composite paper after the first hot rolling treatment is hot pressed again to further melt and expand the hydrophilic polyphenylene sulfide superfine fiber, better wrap the PTFE fiber, and increase the contact area between the two; after completion, the temperature of the precision roller press is increased to 300°C, the pressure and the extrusion roller speed remain unchanged, and the third hot pressing treatment is performed to completely melt the hydrophilic polyphenylene sulfide superfine fiber and restore it to room temperature after hot pressing to quickly plasticize and set. After completion, the hydrophilic polyphenylene sulfide superfine fiber / PTFE composite paper is obtained.
[0073] Embodiment 7-8:
[0074] Examples 7-8 are the same as Example 1, except that in Example 1, sodium 1-naphthalenesulfonate with a melting point of 300°C and polyphenylene sulfide powder resin with a melting index of 80 (300°C test) are mixed at a mass ratio of (1:5), while in Examples 7 and 8, the mass ratios are (1.2:5) and (1.5:5), respectively. The performance test data of the prepared composite paper are shown in Table 1.
[0075] Embodiment 9-10:
[0076] Examples 9-10 are the same as Example 4, except that in Example 4, sodium 1-naphthalenesulfonate with a melting point of 300°C and polyphenylene sulfide powder resin with a melting index of 80 (300°C test) are mixed at a mass ratio of (1:5), while in Examples 9 and 10, the mass ratios are (1.2:5) and (1.5:5), respectively. The performance test data of the prepared composite paper are shown in Table 1.
[0077] Table 1 Performance test data of composite paper prepared in Examples 1, 7-8, 4, 9-10
[0078]
[0079] Comparative Examples 1, 7-8, or Comparative Examples 4, 9-10, it can be seen that with the increase of the content of sodium 1-naphthalenesulfonate, the tensile strength, tear degree and water absorption rate of the prepared composite paper all show an upward trend, and the thermal conductivity shows a downward trend, indicating that the hydrophilic polyphenylene sulfide ultrafine fiber pulp prepared by this method can effectively improve the mechanical properties and hydrophilicity of the finished composite paper, and can also improve the thermal insulation performance of the composite paper.
[0080] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing hydrophilic polyphenylene sulfide ultrafine fiber pulp, characterized in that: The preparation method comprises the following steps: Sodium 1-naphthalenesulfonate and polyphenylene sulfide powder resin are mixed and fed into a twin-screw extruder as raw materials, and the raw materials are melted and extruded into continuous strips through the die head of the twin-screw extruder; The strips are cut into fixed lengths to prepare polyphenylene sulfide modified masterbatches, and the polyphenylene sulfide modified masterbatches are mixed with polyphenylene sulfide resin slices to obtain a polyphenylene sulfide mixture; After the polyphenylene sulfide mixture is dried, it is melt-blown by a melt-blown machine to obtain a hydrophilic polyphenylene sulfide ultrafine fiber non-woven fabric; wherein the temperature used by the melt-blown machine is higher than the melting point of sodium 1-naphthalenesulfonate, so that the dried polyphenylene sulfide mixture has a melting point mutation at the melt-blowing temperature, thereby achieving high fluidity; The hydrophilic polyphenylene sulfide ultrafine fiber nonwoven fabric is subjected to pulping treatment to obtain hydrophilic polyphenylene sulfide ultrafine fiber pulp.
2. The method for preparing hydrophilic polyphenylene sulfide ultrafine fiber pulp according to claim 1, characterized in that: The melt index of the polyphenylene sulfide powder resin and the polyphenylene sulfide resin slices are both 80-120.
3. The method for preparing hydrophilic polyphenylene sulfide ultrafine fiber pulp according to claim 1, characterized in that: The sodium 1-naphthalenesulfonate and the polyphenylene sulfide powder resin are mixed in a mass ratio of 1 to 1.5:5; the polyphenylene sulfide modified masterbatch and the polyphenylene sulfide resin slices are mixed in a mass ratio of 1 to 3:
100.
4. The method for preparing hydrophilic polyphenylene sulfide ultrafine fiber pulp according to claim 1, characterized in that: The melt index of the polyphenylene sulfide mixture used for melt-blowing at the melt-blowing temperature is 320-410; the melt-blowing temperature is 310-330°C.
5. The method for preparing hydrophilic polyphenylene sulfide ultrafine fiber pulp according to claim 1, characterized in that: The polyphenylene sulfide mixture is dried at 140-160° C. for 4-6 hours.
6. The method for preparing hydrophilic polyphenylene sulfide ultrafine fiber pulp according to claim 1, characterized in that: During the beating treatment, the circulation grinding time is 10 to 120 minutes, and the slit-type sieve aperture of the pressure screen used for screening is 0.2 to 0.3 mm.
7. The method for preparing hydrophilic polyphenylene sulfide ultrafine fiber pulp according to claim 1, characterized in that: The prepared hydrophilic polyphenylene sulfide ultrafine fiber pulp has a length of 1 to 3 mm.
8. A hydrophilic polyphenylene sulfide ultrafine fiber pulp, characterized in that: The hydrophilic polyphenylene sulfide ultrafine fiber pulp is prepared by the method for preparing hydrophilic polyphenylene sulfide ultrafine fiber pulp according to any one of claims 1 to 7.
9. A composite material, characterized in that: The composite material is prepared by using any one of polytetrafluoroethylene, carbon fiber, polyimide, PBO, para-aramid, meta-aramid and heterocyclic aramid short-cut fibers and the hydrophilic polyphenylene sulfide ultrafine fiber pulp as claimed in claim 8 as raw materials through fiber decomposition and dispersion, wet web making, drying and hot pressing processes.