Interdigital electrode biosensor based on paper-based cellulose and preparation method thereof
Poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy) of interdigital electrode structure in paper-based cellulose sensor- As electrode materials, disulfonic acid and nanocellulose dispersions solve the problems of uneven conductivity and poor reusability of existing biosensor electrode materials, achieving high reaction rate and stability, and improving biosensor compatibility and reusability.
Patent Information
- Application Number
- CN202410892267.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-04
AI Technical Summary
The selection of electrode materials for existing biosensors is limited, the conductivity is uneven, the reusability is poor, and the preparation cost is high, which affects environmental protection.
Using a paper-based cellulose-based interdigital electrode biosensor through poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)- The dispersion of butyl-1-sulfonic acid and nanocellulose is used as the electrode material. The interdigital electrode structure is coated on the filter paper and soaked in the succinic acid crosslinker solution to activate the electrode material and improve compatibility and conductivity.
It improves the reaction rate and stability of the biosensor, enhances compatibility with biomaterials, improves the reusability of the biosensor, and maintains conductive properties and flexibility.
Smart Images

Figure CN118910920A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of paper-based cellulose biosensors, in particular to an interdigital electrode biosensor based on paper-based cellulose and a preparation method thereof. Background Art
[0002] A biosensor is a device that uses biologically active units as sensitive elements and combines chemical and physical conversion elements to be highly selective for the analyte. It has the advantages of high sensitivity, fast detection speed, easy operation, and continuous dynamic monitoring. It has broad application prospects in the field of health examination and monitoring.
[0003] In the prior art, biosensors usually use metal or semiconductor materials as sensor carriers, which makes the preparation and processing costs of biosensors high and is not conducive to environmental protection. Therefore, paper-based materials are now mostly used as carriers, including electrochemical sensors and optical sensors. Among them, electrochemical sensors print or coat conductive materials on paper-based materials to form electrodes for detecting electrochemical signals generated when the target substance is detected; optical sensors use changes in optical properties to detect through a paper-based platform. However, the electrode material selection of the two sensors is limited, the conductivity is uneven, and the reusability is poor. Summary of the invention
[0004] The present invention provides an interdigital electrode biosensor based on paper-based cellulose and a preparation method thereof. The prepared biosensor has high reaction rate and good stability, which not only improves the compatibility with biological materials, but also improves the reusability of the biosensor.
[0005] In order to achieve the above object, the specific scheme adopted by the present invention is: a method for preparing an interdigital electrode biosensor based on paper-based cellulose, comprising the following steps:
[0006] S1, Preparation of poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxo-2-ylmethoxy)-butane-1-sulfonic acid:
[0007] Poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxo-2-ylmethoxy)-butane-1-sulfonic acid) was prepared using EDOT-S (thienylethylene glycol thiophene), ferrous chloride and sodium persulfate as raw materials. The specific steps are as follows:
[0008] S101, adding ferrous chloride to the EDOT-S aqueous solution and letting it stand for 20-40 minutes to obtain solution A;
[0009] S102, adding sodium persulfate aqueous solution to solution A, stirring until the solution becomes viscous, standing for 2-4 hours, adding acetone and centrifuging to obtain a polymer precipitate;
[0010] S103, dissolving the polymer precipitate obtained in S102 in water, and adding a resin to obtain poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid);
[0011] S2, coating the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid prepared in S1 on filter paper in the form of an interdigitated electrode structure, and drying at room temperature to obtain a poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material;
[0012] S3, dripping the glucose oxidase solution onto the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxo-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material and drying at room temperature.
[0013] As an optimization scheme of the above-mentioned method for preparing the interdigital electrode biosensor based on paper-based cellulose: in the S101, the concentration of the EDOT-S aqueous solution is 0.05-0.07 g / mL.
[0014] As another optimization scheme of the above-mentioned method for preparing the interdigital electrode biosensor based on paper-based cellulose: in the above 102, the concentration of the sodium persulfate aqueous solution is 0.14-0.15 g / mL.
[0015] As another optimization scheme of the above-mentioned method for preparing an interdigital electrode biosensor based on paper-based cellulose: in S2, a nanocellulose dispersion is first added to poly (4-(2,3-dihydrothieno [3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid, and then the poly (4-(2,3-dihydrothieno [3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid added with the nanocellulose dispersion is coated on the filter paper.
[0016] As another optimization scheme of the above-mentioned method for preparing an interdigitated electrode biosensor based on paper-based cellulose: the mass ratio of the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid to the nanocellulose dispersion is 1:14-16.
[0017] As another optimization scheme of the above-mentioned method for preparing the interdigital electrode biosensor based on paper-based cellulose: S3 comprises:
[0018] S301, adding succinic acid, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide into a solvent to obtain a succinic acid crosslinker solution;
[0019] S302, the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxo-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material obtained in S2 is immersed in a succinic acid crosslinker solution for 25-35 minutes and then dried at room temperature;
[0020] S303, preparing a glucose oxidase solution, and dropping the solution onto the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material obtained in S302.
[0021] As another optimization scheme of the above-mentioned method for preparing an interdigital electrode biosensor based on paper-based cellulose: in the S301, the molar ratio of succinic acid, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide in the succinic acid crosslinker solution is 1:2:2.
[0022] As another optimization scheme of the above-mentioned method for preparing the interdigital electrode biosensor based on paper-based cellulose: in the S301, the solvent is a phosphate buffered saline solution.
[0023] As another optimization scheme of the above-mentioned method for preparing the interdigital electrode biosensor based on paper-based cellulose: the concentration of the glucose oxidase solution is 10 mg / mol.
[0024] The biosensor was prepared according to the above method.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] 1. The present invention provides a paper-based cellulose-based interdigitated electrode biosensor and a preparation method thereof, wherein filter paper is used as the paper-based material, and poly (4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid (PEDOT:SH) is used as the electrode material and is coated on the filter paper in an interdigitated structure. The biosensor has the advantages of fast reaction rate and good stability, and can improve the compatibility of the biosensor with biological materials, and at the same time, improves the reusability of the biosensor.
[0027] 2. In the present invention, a nanocellulose dispersion is added to poly (4-(2,3-dihydrothieno [3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid. The addition of the nanocellulose dispersion can provide more surface adhesion points for poly (4-(2,3-dihydrothieno [3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid, thereby enhancing the adhesion between poly (4-(2,3-dihydrothieno [3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid and the filter paper substrate, so that poly (4-(2,3-dihydrothieno [3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid adheres more firmly to the filter paper.
[0028] 3. In the present invention, the electrode material is coated on the filter paper in the form of an interdigitated electrode structure, which has a highly branched shape, does not affect the flexibility of the filter paper, and also maintains the good electrical conductivity of the electrode material, while improving the reaction rate and sensitivity of the electrode.
[0029] 4. In the present invention, before fixing glucose oxidase, the poly (4- (2,3-dihydrothieno [3,4-b] [1,4] dioxy-2-ylmethoxy) -butane-1-sulfonic acid / filter paper composite material is first immersed in a succinic acid crosslinker solution, which can fully activate the carboxyl functional groups on the surface of poly (4- (2,3-dihydrothieno [3,4-b] [1,4] dioxy-2-ylmethoxy) -butane-1-sulfonic acid, and the electrode material has good contact with the electrolyte, fast electron transmission and higher conductivity; at the same time, it is beneficial to the fixation of glucose oxidase, so that it is more firmly combined with the base to form a stable complex. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The invention relates to a preparation process of poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid;
[0031] Figure 2 It is the coating of the interdigitated electrode structure;
[0032] Figure 3 It is the fixation process of glucose oxidase. DETAILED DESCRIPTION
[0033] The technical solution of the present invention is further elaborated in detail below in conjunction with specific embodiments. The parts of the present invention that are not described and disclosed in detail in the following embodiments should be understood as the prior art known or should be known to those skilled in the art.
[0034] A method for preparing a paper-based cellulose interdigital electrode biosensor comprises the following steps:
[0035] S1, Preparation of poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxo-2-ylmethoxy)-butane-1-sulfonic acid (Preparation of PEDOT:SH):
[0036] Poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxo-2-ylmethoxy)-butane-1-sulfonic acid) was prepared using EDOT-S, ferrous chloride and sodium persulfate as raw materials. The specific steps are as follows:
[0037] S101, adding ferrous chloride to an EDOT-S aqueous solution, wherein the concentration of the EDOT-S aqueous solution is 0.05-0.07 g / mL, and the mass ratio of EDOT-S to ferrous chloride in the EDOT-S aqueous solution is 1:0.3; after the ferrous chloride is added to the EDOT-S aqueous solution, stirring is performed evenly with a stirring rod to ensure that the two are fully reacted, and the mixture is allowed to stand for 20-40 minutes to obtain a solution A;
[0038] S102, adding sodium persulfate aqueous solution dropwise to solution A, wherein the concentration of the sodium persulfate aqueous solution is 0.14-0.15 g / mL, and the mass ratio of solution A to the sodium persulfate solution is 3:2, and stirring is continuously performed during the process of adding the sodium persulfate aqueous solution until the solution becomes viscous. After standing for 2-4 hours, a polymer solution is obtained, 30-50 mL of acetone solution is added to the polymer solution and stirred evenly, and the evenly mixed solution is centrifuged to fully precipitate the polymer in acetone to obtain a polymer precipitate.
[0039] S103, dissolving the polymer precipitate obtained in S102 in water, adding the resin AMBERLITE HPR1100 sodium form, and stirring continuously to allow the resin AMBERLITE HPR1100 sodium form to fully contact with the polymer to obtain poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid;
[0040] S2, the poly (4-(2,3-dihydrothieno [3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid prepared in S1 is coated on the filter paper in the form of an interdigitated electrode structure. Specifically, the nanocellulose dispersion is first added to the poly (4-(2,3-dihydrothieno [3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid, and then the poly (4-(2,3-dihydrothieno [3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid added with the nanocellulose dispersion is coated on the filter paper, and dried at room temperature to obtain the poly (4-(2,3-dihydrothieno [3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material.
[0041] In this embodiment, No. 4 filter paper is used, which can more effectively adsorb poly (3, 4-ethylenedioxythiophene): sulfonic acid.
[0042] The mass ratio of the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid to the nanocellulose dispersion is 1:14-16; the nanocellulose dispersion is added to the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid, and the addition of the nanocellulose dispersion can provide more surface active agents for the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid. The surface adhesion points are increased, and the adhesion between poly (4-(2,3-dihydrothieno [3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid and the filter paper substrate is enhanced, so that poly (4-(2,3-dihydrothieno [3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid adheres more firmly to the filter paper. At the same time, the conductive performance of poly (4-(2,3-dihydrothieno [3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid is better and more stable, and the surface is more uniform and smooth.
[0043] The electrode material is coated on the filter paper in the form of an interdigitated electrode structure. Specifically, the interdigitated electrode structure is composed of a plurality of parallel interdigitated electrodes, the width of the interdigitated fingers is 1 mm, and the distance between the interdigitated fingers is 0.5 mm, so that the electrode material is highly branched on the filter paper. The bending angle of the interdigitated electrode structure can be 30°, 45°, 60° and 75°. The resistance value of the electrode material increases only slightly with the increase of the bending angle, and no circuit breaking occurs, which fully demonstrates that the interdigitated electrode structure will not affect the flexibility of the filter paper, and also maintains the good conductivity of the electrode material, while improving the reaction rate and sensitivity of the electrode.
[0044] Refrigeration and room temperature can promote the crystallization of poly (4- (2,3-dihydrothieno [3,4-b] [1,4] dioxy-2-ylmethoxy) -butane-1-sulfonic acid, improve its orderliness and charge transport performance, and enhance the conductivity of poly (4- (2,3-dihydrothieno [3,4-b] [1,4] dioxy-2-ylmethoxy) -butane-1-sulfonic acid. Lower temperature will lead to insufficient crystallinity, and higher temperature will lead to thermal decomposition or destruction of the lattice structure. Therefore, in this embodiment, poly (4- (2,3-dihydrothieno [3,4-b] [1,4] dioxy-2-ylmethoxy) -butane-1-sulfonic acid is coated on filter paper and then dried at room temperature.
[0045] S3, dripping the glucose oxidase solution onto the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material and drying at room temperature. Specifically:
[0046] S301, adding succinic acid, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide to a solvent, wherein the solvent is a phosphate buffered saline solution, to obtain a succinic acid crosslinker solution; the molar ratio of succinic acid, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide in the succinic acid crosslinker solution is 1:2:2.
[0047] S302, the poly (4- (2,3-dihydrothieno [3,4-b] [1,4] dioxy-2-ylmethoxy) -butane-1-sulfonic acid / filter paper composite material obtained in S2 is immersed in a succinic acid crosslinker solution, immersed for 25-35 minutes and then dried at room temperature; before fixing glucose oxidase, the poly (4- (2,3-dihydrothieno [3,4-b] [1,4] dioxy-2-ylmethoxy) -butane-1-sulfonic acid / filter paper composite material is first immersed in a succinic acid crosslinker solution, which can fully activate the carboxyl functional groups on the surface of poly (4- (2,3-dihydrothieno [3,4-b] [1,4] dioxy-2-ylmethoxy) -butane-1-sulfonic acid, and the electrode material has good contact with the electrolyte, fast electron transfer and higher conductivity; at the same time, it is beneficial to the fixation of glucose oxidase, so that it is more firmly combined with the base to form a stable complex.
[0048] S303, prepare a glucose oxidase solution, the concentration of which is 10 mg / mol, and add it dropwise onto the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material obtained in S302.
[0049] The measurement principle of the biobed dryer prepared based on the above preparation method is: when glucose is present, glucose oxidase catalyzes the reaction of glucose and oxygen to produce hydrogen peroxide, and the concentration of glucose is determined by measuring the current or potential change of hydrogen peroxide. That is, the glucose content in human sweat can be obtained by non-invasive detection, which shows the broad application prospects of this biosensor in the field of health examination and monitoring in the future.
[0050] Example 1
[0051] A method for preparing a paper-based cellulose interdigital electrode biosensor comprises the following steps:
[0052] S1, Preparation of poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxo-2-ylmethoxy)-butane-1-sulfonic acid:
[0053] Poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxo-2-ylmethoxy)-butane-1-sulfonic acid) was prepared using EDOT-S, ferrous chloride and sodium persulfate as raw materials. The specific steps are as follows:
[0054] S101, weigh 0.2 g of EDOT-S and mix it with 4 mL of water, stir continuously to completely dissolve it to obtain an EDOT-S aqueous solution, weigh 0.06 g of ferrous chloride and add it to the prepared EDOT-S aqueous solution, continue to stir evenly to ensure sufficient reaction, and let it stand for 20 minutes.
[0055] S102, weighing 0.28 g of sodium persulfate and mixing it with 2 mL of water to obtain a sodium persulfate aqueous solution; dropping the filtered sodium persulfate aqueous solution into solution A, stirring continuously during the dropping process, stirring until the solution becomes viscous and then standing for 3 hours, adding 40 mL of acetone solution to the solution after standing, and stirring sufficiently, and then centrifuging at a speed of 3500 rpm for 5 minutes to obtain a polymer precipitate;
[0056] S103, the obtained polymer precipitate was mixed with 7 mL of water and allowed to stand for 5 minutes, and then 0.3 g of resin AMBERLITE HPR1100 sodium form was added and stirred, and then allowed to stand for 10 minutes after stirring to obtain poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid;
[0057] S2, adding nanocellulose dispersion into poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid, the mass ratio of poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid to nanocellulose dispersion is 1:14;
[0058] S3, dripping the glucose oxidase solution onto the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material and drying at room temperature. Specifically:
[0059] S301, adding succinic acid, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide to a solvent, wherein the solvent is a phosphate buffered saline solution, to obtain a succinic acid crosslinker solution; the molar ratio of succinic acid, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide in the succinic acid crosslinker solution is 1:2:2.
[0060] S302, the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxo-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material obtained in S2 is immersed in a succinic acid crosslinker solution, immersed for 25 minutes and then dried at room temperature;
[0061] S303, preparing a glucose oxidase solution with a concentration of 10 mg / mol, and dropping the glucose oxidase solution onto the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material obtained in S302.
[0062] Example 2
[0063] A method for preparing a paper-based cellulose interdigital electrode biosensor comprises the following steps:
[0064] S1, Preparation of poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxo-2-ylmethoxy)-butane-1-sulfonic acid:
[0065] Poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxo-2-ylmethoxy)-butane-1-sulfonic acid) was prepared using EDOT-S, ferrous chloride and sodium persulfate as raw materials. The specific steps are as follows:
[0066] S101, weigh 0.28 g of EDOT-S and mix it with 4 mL of water, stir continuously to completely dissolve it to obtain an EDOT-S aqueous solution, weigh 0.042 g of ferrous chloride and add it to the prepared EDOT-S aqueous solution, continue to stir evenly to ensure sufficient reaction, and let it stand for 20 minutes.
[0067] S102, weighing 0.3 g of sodium persulfate and mixing it with 2 mL of water to obtain a sodium persulfate aqueous solution; dropping the filtered sodium persulfate aqueous solution into solution A, stirring continuously during the dropping process, stirring until the solution becomes viscous and then standing for 3 hours, adding 30 mL of acetone solution to the solution after standing, and stirring sufficiently, and then centrifuging at a speed of 3500 rpm for 5 minutes to obtain a polymer precipitate;
[0068] S103, the obtained polymer precipitate was mixed with 7 mL of water and allowed to stand for 5 minutes, and then 0.3 g of resin AMBERLITE HPR1100 sodium form was added and stirred, and then allowed to stand for 10 minutes after stirring to obtain poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid;
[0069] S2, adding nanocellulose dispersion into poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid, the mass ratio of poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid to nanocellulose dispersion is 1:16;
[0070] S3, dripping the glucose oxidase solution onto the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material and drying at room temperature. Specifically:
[0071] S301, adding succinic acid, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide to a solvent, wherein the solvent is a phosphate buffered saline solution, to obtain a succinic acid crosslinker solution; the molar ratio of succinic acid, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide in the succinic acid crosslinker solution is 1:2:2.
[0072] S302, the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxo-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material obtained in S2 is immersed in a succinic acid crosslinker solution, immersed for 35 minutes and then dried at room temperature;
[0073] S303, preparing a glucose oxidase solution with a concentration of 10 mg / mol, and dropping the glucose oxidase solution onto the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material obtained in S302.
[0074] Example 3
[0075] A method for preparing a paper-based cellulose interdigital electrode biosensor comprises the following steps:
[0076] S1, Preparation of poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxo-2-ylmethoxy)-butane-1-sulfonic acid:
[0077] Poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxo-2-ylmethoxy)-butane-1-sulfonic acid) was prepared using EDOT-S, ferrous chloride and sodium persulfate as raw materials. The specific steps are as follows:
[0078] S101, weigh 0.24 g of EDOT-S and mix it with 4 mL of water, stir continuously to completely dissolve it to obtain an EDOT-S aqueous solution, weigh 0.072 g of ferrous chloride and add it to the prepared EDOT-S aqueous solution, continue to stir evenly to ensure sufficient reaction, and let it stand for 20 minutes.
[0079] S102, weighing 0.29 g of sodium persulfate and mixing it with 2 mL of water to obtain a sodium persulfate aqueous solution; dropping the filtered sodium persulfate aqueous solution into solution A, stirring continuously during the dropping process, stirring until the solution becomes viscous and then standing for 3 hours, adding 30 mL of acetone solution to the solution after standing, and stirring sufficiently, and then centrifuging at a speed of 3500 rpm for 5 minutes to obtain a polymer precipitate;
[0080] S103, the obtained polymer precipitate was mixed with 7 mL of water and allowed to stand for 5 minutes, and then 0.3 g of resin AMBERLITE HPR1100 sodium form was added and stirred, and then allowed to stand for 10 minutes after stirring to obtain poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid;
[0081] S2, adding the nanocellulose dispersion into poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid, the mass ratio of poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid to the nanocellulose dispersion is 1:15;
[0082] S3, dripping the glucose oxidase solution onto the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material and drying at room temperature. Specifically:
[0083] S301, adding succinic acid, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide to a solvent, wherein the solvent is a phosphate buffered saline solution, to obtain a succinic acid crosslinker solution; the molar ratio of succinic acid, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide in the succinic acid crosslinker solution is 1:2:2.
[0084] S302, the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxol-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material obtained in S2 is immersed in a succinic acid crosslinker solution, immersed for 30 minutes and then dried at room temperature;
[0085] S303, preparing a glucose oxidase solution with a concentration of 10 mg / mol, and dropping the glucose oxidase solution onto the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material obtained in S302.
[0086] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a paper-based cellulose interdigital electrode biosensor, characterized in that: The following steps are involved: S1, Preparation of poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxo-2-ylmethoxy)-butane-1-sulfonic acid: Poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxo-2-ylmethoxy)-butane-1-sulfonic acid) was prepared using EDOT-S, ferrous chloride and sodium persulfate as raw materials. The specific steps are as follows: S101, adding ferrous chloride to the EDOT-S aqueous solution and letting it stand for 20-40 minutes to obtain solution A; S102, adding a sodium persulfate aqueous solution to solution A, stirring until the solution becomes viscous, standing for 2-4 hours, adding acetone and centrifuging to obtain a polymer precipitate; S103, dissolving the polymer precipitate obtained in S102 in water, and adding a resin to obtain poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid); S2, coating the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid prepared in S1 on filter paper in the form of an interdigitated electrode structure, and drying at room temperature to obtain a poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material; S3, dripping the glucose oxidase solution onto the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material and drying at room temperature.
2. The method for preparing a paper-based cellulose interdigital electrode biosensor according to claim 1, characterized in that: In the S101, the concentration of the EDOT-S aqueous solution is 0.05-0.07 g / mL.
3. The method for preparing a paper-based cellulose interdigital electrode biosensor according to claim 1, characterized in that: In the step 102, the concentration of the sodium persulfate aqueous solution is 0.14-0.15 g / mL.
4. The method for preparing a paper-based cellulose interdigital electrode biosensor according to claim 1, characterized in that: In S2, a nanocellulose dispersion is first added to poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid, and then the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid to which the nanocellulose dispersion is added is coated on filter paper.
5. The method for preparing a paper-based cellulose interdigital electrode biosensor according to claim 4, characterized in that: The mass ratio of the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid to the nanocellulose dispersion is 1:14-16.
6. The method for preparing a paper-based cellulose interdigital electrode biosensor according to claim 1, characterized in that: The S3 includes: S301, adding succinic acid, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide into a solvent to obtain a succinic acid crosslinker solution; S302, the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxo-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material obtained in S2 is immersed in a succinic acid crosslinker solution for 25-35 minutes and then dried at room temperature; S303, preparing a glucose oxidase solution, and dropping the solution onto the poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxy-2-ylmethoxy)-butane-1-sulfonic acid / filter paper composite material obtained in S302.
7. The method for preparing a paper-based cellulose interdigital electrode biosensor according to claim 6, characterized in that: In the S301, the molar ratio of succinic acid, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide in the succinic acid cross-linking agent solution is 1:2:
2.
8. The method for preparing a paper-based cellulose interdigital electrode biosensor according to claim 6, characterized in that: In the S301, the solvent is a phosphate buffered saline solution.
9. The method for preparing a paper-based cellulose interdigital electrode biosensor according to claim 1, characterized in that: The concentration of the glucose oxidase solution is 10 mg / mol.
10. The biosensor prepared according to the method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Thiophene copolymer, aqueous solution thereof, thiophene monomer composition and method for producing the same
JP2015168793A
Electroconductive material and electrical element provided with same, and sensor
WO2019240241A1
High purity sulfonated thiophene monomers
WO2024037738A1