Method for reinforcing loess by inducing calcium carbonate deposition through combination of guar gum and soybean urease

Through the combined technology of guar gum and soy urease, nucleation sites and uniform distribution of calcium carbonate are provided, which solves the problems of uneven deposits and environmental impacts in loess reinforcement technology, significantly improves the strength and stability of loess, and achieves the Green and environmentally friendly efficient reinforcement effect.

CN118911113APending Publication Date: 2024-11-08XIJING UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410942505.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing loess reinforcement technology has problems such as uneven mixing, difficult construction, excessive curing agent consumption, high cost, environmental impact and poor long-term stability, especially when using microorganisms to induce calcium carbonate deposition and plant urease to induce calcium carbonate deposition. During technology, problems such as uneven deposition of calcium carbonate and bacterial influence.

Method used

Using the combined technology of guar gum and soy urease, guar gum and curing solution are added to the loess soil in a certain proportion, providing nucleation sites, increasing the amount of calcium carbonate production and making it evenly distributed, using guar The bonding effect of soy glue is combined with the calcium carbonate produced by soy urease to strengthen the loess.

Benefits of technology

It significantly improves the overall strength of loess, reduces water sensitivity and permeability, improves compressive strength and crack resistance, and has the characteristics of green and environmental protection, good adaptability and high curing efficiency, avoiding pollution to the soil and the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118911113A_ABST
    Figure CN118911113A_ABST
Patent Text Reader

Abstract

A method for reinforcing loess by inducing calcium carbonate deposition through combination of guar gum and soybean urease is characterized in that guar gum and a curing solution are respectively added into loess soil according to a certain proportion, and the combined reinforcing effect of the guar gum and the curing solution is achieved; the guar gum is added to provide a plurality of nucleation sites for the curing solution in the soil body, so that the generation amount of the calcium carbonate is increased, and the calcium carbonate is uniformly distributed in the soil body; the bonding effect of the guar gum and calcium carbonate generated by the soybean urease solution play a dual reinforcing effect, on one hand, soil particles are stabilized, and on the other hand, soil pores are filled with the calcium carbonate, so that the overall strength of the solidified soil body is greatly improved; the water sensitivity and permeability of the solidified soil body are greatly reduced, the compressive strength, crack resistance and water stability of loess are effectively improved, and the method has the advantages of being environmentally friendly, good in adaptability and high in solidification efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of geotechnical engineering, and in particular to a method for reinforcing loess by inducing calcium carbonate deposition using guar gum combined with soybean urease. Background Art

[0002] Loess is widely distributed in my country. It has disadvantages such as high compressibility, strong water sensitivity and severe collapsibility. At present, loess can be improved in many ways, including physical and chemical methods. Physical methods include operations such as compaction and layer replacement, which can improve the engineering properties of loess. In addition, chemical methods are also a common improvement method. Chemical substances such as cement, fly ash, and lime high-activity additives can be added to improve the performance of loess. The application of these methods can enhance the stability and bearing capacity of loess, thereby meeting the needs of engineering projects.

[0003] In recent years, some studies have pointed out that biopolymers, as a sustainable and renewable carbon-neutral material, have the property of forming hydrogels when in contact with water, so they can fill pores and cement particles, thereby significantly enhancing the density of the soil and effectively improving the mechanical strength and hydraulic properties of the soil.

[0004] Traditional loess solidification methods mainly include mechanical mixing, impregnation solidification, roller solidification and chemical reinforcement. These methods make the loess and the curing agent fully contact and react physically and chemically through mixing, injection, roller rolling or adding chemical materials, thereby improving the mechanical properties of loess and increasing its bearing capacity and stability. Although traditional loess solidification methods can improve the mechanical properties of loess and increase its bearing capacity and stability to a certain extent, there may be problems such as uneven mixing, difficult construction, excessive consumption of curing agent, high cost, environmental impact and doubts about long-term environmental stability during the operation.

[0005] Microbial induced calcium carbonate deposition (MICP) technology is an emerging soil reinforcement technology. Urea is decomposed by urease produced by specific bacteria to generate carbonate ions. These ions combine with metal cations such as calcium ions in loess to form calcium carbonate precipitation, thereby filling the pores in the loess, increasing its density and strength, and effectively improving the geological properties of loess. However, the effect of MICP on soil solidification is affected by many factors such as bacterial species, concentration, reaction time, etc. There are still certain defects and challenges in terms of technical maturity, construction conditions, reinforcement effect, long-term stability, and environmental adaptability.

[0006] The principle of strengthening loess by plant urease-induced calcium carbonate deposition (EICP) technology is to extract urease from plant sources (such as soybeans) to catalyze the decomposition of urea to produce carbonate ions, which then combine with calcium ions in the soil to form calcium carbonate precipitation. These precipitates form cementation between loess particles, enhancing the mechanical properties and stability of loess. However, the reaction speed of EICP solidification of soil is fast but varies greatly, which may lead to uneven carbonate deposition and affect the uniformity of the reinforced soil.

[0007] Jia Zhuolong et al. (Jia Zhuolong, Yan Changgen, Li Bo, et al. Experimental study on the anti-erosion characteristics and ecological slope protection of guar gum solidified fibrous loess [J]. Chinese Journal of Geotechnical Engineering, 2022, 44 (10): 1881-1889.) proposed an experimental study on the anti-erosion characteristics and ecological slope protection of guar gum solidified fibrous loess. By using guar gum to solidify the fibrous loess, it can not only promote the role of fiber reinforcement, but also fill pores and bond loess particles, thus comprehensively improving the mechanical and hydraulic properties of fibrous loess. However, the fiber plays a role in increasing permeability in the soil. Too much fiber will lead to excessive seepage in the soil, which is not conducive to the reinforcement of the soil. Secondly, the fiber may be unevenly distributed in the soil, and the tensile anchoring effect of the fiber cannot be fully exerted.

[0008] Liu Yang et al. (Liu Yang, Gao Yufeng, He Jia, et al. Experimental study on windbreak and sand fixation of soybean urease-induced calcium carbonate deposition technology [J]. Henan Science, 2019, 37(11): 1784-1789.) proposed an experimental study on windbreak and sand fixation of soybean urease-induced calcium carbonate deposition technology. The effect and mechanism of EICP were studied through indoor experiments. Urease was extracted from soybeans, mixed with equal amounts of calcium chloride and urea solution, and then sprayed on the surface of the sample to form a thin layer of hard crust on the surface of the sample; the surface hard crust formed by calcium carbonate cementation can reach MPa-level strength, and the water retention of the sample is increased by 60% compared with the untreated sample, and the wind erosion rate and infiltration rate are significantly reduced. However, a single soybean urease cannot provide nucleation sites, and the amount of calcium carbonate produced in the soil is small and unevenly distributed, and there is a lack of stabilizer addition. Summary of the invention

[0009] In order to overcome the defects of the above-mentioned prior art, the purpose of the present invention is to provide a method for reinforcing loess by inducing calcium carbonate deposition by guar gum and soybean urease, wherein guar gum and a solidifying solution are added to the loess material in a certain proportion, respectively, to achieve a combined reinforcement effect of the two; the addition of guar gum provides a plurality of nucleation sites for the solidifying solution in the soil, thereby increasing the amount of calcium carbonate generated and making the calcium carbonate evenly distributed in the soil; the bonding effect of guar gum and the calcium carbonate generated by soybean urease play a dual reinforcement role, on the one hand stabilizing the soil particles, on the other hand calcium carbonate fills the soil pores, thereby greatly improving the overall strength of the solidified soil; not only the water sensitivity and permeability of the solidified soil are greatly reduced, but also the compressive strength, crack resistance and water stability of the loess are effectively improved, and the method has the characteristics of being green and environmentally friendly, having good adaptability and high curing efficiency.

[0010] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0011] A method for reinforcing loess by inducing calcium carbonate deposition using guar gum and soybean urease, specifically comprising the following steps:

[0012] Step 1: Hammer the original air-dried loess, then sieve it through a 2-4 mm sieve, and dry the sieved loess at 95-105°C to obtain dry soil for later use;

[0013] Step 2: According to the dry density of 1.44-1.65g / cm 3 Weigh a certain mass of the dry soil obtained in step 1, and fully mix the dry soil with 1.00%-2.00% of guar gum by mass of the dry soil to obtain a mixed soil material;

[0014] Step 3: mixing soybean urease and a binder at an enzyme-to-binder volume ratio of 1:1, 1:2 or 1:3 and stirring to prepare a solidification solution;

[0015] Step 4: Add the solidification solution prepared in step 3 accounting for 7% to 14% of the dry soil mass to the mixed soil material obtained in step 2, and mix evenly to obtain a solidified soil body;

[0016] Step 5: compact the solidified soil obtained in step 4 in 4-5 layers, scrape the soil between the layers, let it stand at 20-24°C for 10-15h, and obtain reinforced soil blocks after demoulding.

[0017] In the step 2, the guar gum is:

[0018] The guar gum is white in appearance and can form a viscous colloid in cold water. The viscosity of the guar gum is 5000-5500 centipoise, the pH value is 6-8, and the particle size is 8-15 / μm.

[0019] The soybean urease extraction method in step 3 is:

[0020] The dried soybeans are ground into powder and passed through a 50-100 mesh sieve to obtain soybean powder; the soybean powder is mixed with deionized water to prepare a soybean solution with a concentration of 100-200 g / L; the soybean solution is centrifuged at a speed of 3000-5000 r·min for 15-30 minutes, and the upper light yellow clear liquid is extracted, which is the soybean urease solution.

[0021] The method for preparing the cementing liquid in step 3 is as follows:

[0022] A urea solution of a certain concentration is uniformly mixed with anhydrous calcium chloride solution in equal volumes to obtain a cementing liquid with a concentration of 0.5-2.0 mol / L.

[0023] The concentration of the urea solution is 15-65 g / L.

[0024] The concentration of the anhydrous calcium chloride solution is 20-120 g / L.

[0025] The beneficial effects of the present invention are:

[0026] (1) The present invention adopts an innovative method of combining guar gum with EICP to reinforce loess, and the synergistic effect of the two significantly improves the solidification effect of loess. Guar gum reacts with water to form a highly fluid hydrogel, which effectively fills the soil voids and reduces the permeability of the soil. The solidification solution generates calcium carbonate precipitation in the soil, which fills the soil pores and makes the soil dense, thereby improving the strength of the soil.

[0027] When guar gum is combined with EICP to solidify loess, the addition of guar gum provides more nucleation sites for the solidification solution, which not only increases the amount of calcium carbonate generated in the soil, but also makes the generated calcium carbonate particles larger in volume. The anchoring zone formed after hydration of guar gum tightly locks the calcium carbonate, while the hydrate fills the voids in the soil sample, enhances the soil density, increases the contact area and interaction force between calcium carbonate and the soil medium, and makes the solidified loess show excellent mechanical properties.

[0028] (2) Compared with the traditional loess solidification method, the present invention uses natural green materials guar gum and solidification solution, which will not cause pollution to the soil and can be self-degraded. It will not pollute the environment and affect the growth of vegetation, and it can significantly improve the strength of the soil and reduce the water sensitivity of the soil.

[0029] (3) Compared with the MICP method of solidifying soil, the present invention is simple to operate, green, pollution-free, and does not pose any danger during the sample preparation process. It does not require the cultivation of bacteria and is relatively safe to a certain extent. When solidifying the soil, no bacterial microorganisms will be generated to affect the ecological balance of the soil.

[0030] (4) Compared with the EICP method of solidifying soil, a single EICP cannot determine the nucleation site. The present invention adds guar gum to provide more nucleation sites for a single solidification solution, the amount of calcium carbonate generated gradually increases, and the soil reinforcement effect is more obvious.

[0031] In summary, the present invention uses natural, degradable, green and environmentally friendly materials, which not only effectively avoids the ecological impact on the soil, but also shows good adaptability to environmental conditions during the solidification process. The effect of guar gum combined with EICP in reinforcing loess is extremely significant, reducing the water sensitivity and permeability of the solidified soil, and improving the compressive strength, crack resistance and water stability of loess. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a flow chart of sample preparation of the present invention.

[0033] Figure 2 The figure is a relationship diagram between the guar gum content and the dry density of the sample and the compressive strength of the solidified loess without side line, wherein: Figure 2 (a) is the dry density of loess 1.44 g / cm 3 , 1.55g / cm 3 , 1.65g / cm 3 , guar gum content is 1.00%, and the solidified solution content is 14%; Figure 2 (b) Dry density is 1.44 g / cm 3 , 1.55g / cm 3 , 1.65g / cm 3 , guar gum content is 1.50%, and the solidification solution content is 14%; Figure 2 (c) Dry density 1.44 g / cm 3 , 1.55g / cm 3 , 1.65g / cm 3 g / cm 3 , the guar gum content is 2.00% and the solidified solution content is 14%.

[0034] Figure 3 is a graph showing the relationship between the guar gum content and the triaxial shear strength of solidified loess of the present invention, wherein: Figure 3 (a) is the shear strength under a confining pressure of 25 kPa when the guar gum content is 1.00, 1.50, and 2.00% and the solidified solution content is 10%; Figure 3 (b) is the shear strength under a confining pressure of 50 kPa when the guar gum content is 1.00%, 1.50%, and 2.00% and the solidified solution content is 10%; Figure 3 (c) is the shear strength under a confining pressure of 100 kPa when the guar gum content is 1.00%, 1.50%, and 2.00% and the solidified solution content is 10%.

[0035] Figure 4 The relationship between the content of guar gum and the permeability coefficient of solidified loess in the present invention is shown in FIG. Figure 4 (a) is the permeability coefficient of guar gum content of 1.00%, 1.50%, 2.00% and solidified solution content of 14% under a confining pressure of 25 kPa; Figure 4 (b) is the permeability coefficient of guar gum content of 1.00%, 1.50%, 2.00% and solidified solution content of 14% under a confining pressure of 50 kPa; Figure 4 (c) is the permeability coefficient under a confining pressure of 100 kPa when the guar gum content is 1.00%, 1.50%, and 2.00% and the solidified solution content is 14%.

[0036] Figure 5 is a graph showing the relationship between the guar gum content and the disintegration amount of solidified loess in the present invention, wherein: Figure 5 The disintegration amount in water over time when the guar gum content is 1.00%, 1.50%, 2.00% and the solidified solution content is 14%.

[0037] Figure 6 The figure is a graph showing the relationship between the guar gum content and the amount of calcium carbonate generated in the present invention, wherein: Figure 6 The calcium carbonate content generated when the guar gum content is 1.00%, 1.50%, and 2.00% respectively. DETAILED DESCRIPTION

[0038] The following will be combined with the accompanying drawings in the present invention and accompanied by text descriptions to clearly and completely explain the methods, processes and effects in the embodiments of the present invention.

[0039] Example 1

[0040] A method for reinforcing loess by inducing calcium carbonate deposition using guar gum and soybean urease, specifically comprising the following steps:

[0041] Step 1: crush the original air-dried loess with hammer, and then sieve it through a 4 mm sieve. Dry the sieved loess at 105°C to obtain dry soil for later use;

[0042] Step 2: According to the dry density of 1.65g / cm 3 Weigh a certain mass of the dry soil obtained in step 1, and fully mix the dry soil with 2.00% guar gum by mass of the dry soil to obtain a mixed soil material;

[0043] In the step 2, the guar gum is:

[0044] The guar gum is white in appearance and can form a viscous colloid in cold water, with a viscosity of 5500 centipoise, a pH value of 8, and a particle size of 15 / μm;

[0045] Step 3: Mix soybean urease and cementing liquid at an enzyme-to-binder volume ratio of 1:3 and stir to form a solidifying solution;

[0046] The soybean urease extraction method in step 3 is:

[0047] The dried soybeans were ground into powder and passed through a 100-mesh sieve to obtain soybean powder; the soybean powder was mixed with deionized water to prepare a soybean solution with a concentration of 200 g / L; the soybean solution was centrifuged at a speed of 5000 r·min for 30 min, and the upper light yellow clear liquid was extracted, which was the soybean urease solution;

[0048] The method for preparing the cementing liquid in step 3 is as follows:

[0049] The urea solution of a certain concentration and the anhydrous calcium chloride solution were uniformly mixed in equal volumes to obtain a cementing solution with a concentration of 2.0 mol / L;

[0050] The concentration of the urea solution is 60 g / L;

[0051] The concentration of the anhydrous calcium chloride solution is 110.98 g / L;

[0052] Step 4: Add the solidification solution prepared in step 3 accounting for 14% of the dry soil mass to the mixed soil material obtained in step 2, and mix evenly to obtain a solidified soil body;

[0053] Step 5: Fill the solidified soil obtained in step 4 into the sample maker coated with vaseline and prepare it in 5 layers. In order to ensure that every two contacting soil samples are better bonded together, the contact surface will be scraped after each layer is compacted, and then the next layer of soil is poured in. Repeat the operation until the fifth layer is compacted; place the solidified soil after compaction together with the sample maker in a curing room at 24°C for 15 hours; finally, open the sample maker, slowly separate the three inner walls that wrap the soil sample, and obtain the reinforced soil block after demolding.

[0054] Example 2

[0055] A method for reinforcing loess by inducing calcium carbonate deposition using guar gum and soybean urease, specifically comprising the following steps:

[0056] Step 1: Hammer the original air-dried loess, then sieve it through a 3mm sieve, dry the sieved loess at 100°C to obtain dry soil for later use;

[0057] Step 2: According to the dry density of 1.55g / cm 3 Weigh a certain mass of the dry soil obtained in step 1, and fully mix the dry soil with 1.50% of guar gum by mass of the dry soil to obtain a mixed soil material;

[0058] In the step 2, the guar gum is:

[0059] The guar gum is white in appearance and can form a viscous colloid in cold water, with a viscosity of 5300 centipoise, a pH value of 7, and a particle size of 11 / μm;

[0060] Step 3: Mix soybean urease and cementing liquid at an enzyme-to-binder volume ratio of 1:2 and stir to form a solidifying solution;

[0061] The soybean urease extraction method in step 3 is:

[0062] The dried soybeans were ground into powder and passed through a 75-mesh sieve to obtain soybean powder; the soybean powder was mixed with deionized water to prepare a soybean solution with a concentration of 200 g / L; the soybean solution was centrifuged at a speed of 4000 r·min for 20 min, and the upper light yellow clear liquid was extracted, which was the soybean urease solution;

[0063] The method for preparing the cementing liquid in step 3 is as follows:

[0064] The urea solution of a certain concentration and the anhydrous calcium chloride solution were uniformly mixed in equal volumes to obtain a cementing solution with a concentration of 1.5 mol / L;

[0065] The concentration of the urea solution is 45 g / L;

[0066] The concentration of the anhydrous calcium chloride solution is 83 g / L;

[0067] Step 4: Add the solidification solution prepared in step 3 accounting for 10% of the dry soil mass to the mixed soil material obtained in step 2, and mix evenly to obtain a solidified soil body;

[0068] Step 5: Fill the solidified soil obtained in step 4 into the sample maker coated with vaseline and prepare it in 5 layers. In order to ensure that every two contacting soil samples are better bonded together, the contact surface will be scraped after each layer is compacted, and then the next layer of soil is poured in. Repeat the operation until the fifth layer is compacted; place the solidified soil after compaction together with the sample maker in a curing room at 22°C for 12 hours; finally, open the sample maker, slowly separate the three inner walls that wrap the soil sample, and obtain the reinforced soil block after demolding.

[0069] Example 3

[0070] A method for reinforcing loess by inducing calcium carbonate deposition using guar gum and soybean urease, specifically comprising the following steps:

[0071] Step 1: Hammer the original air-dried loess, then sieve it through a 2mm sieve, dry the sieved loess at 95°C to obtain dry soil for later use;

[0072] Step 2: According to the dry density of 1.44g / cm 3Weigh a certain mass of the dry soil obtained in step 1, and fully mix the dry soil with 1.00% guar gum by mass of the dry soil to obtain a mixed soil material;

[0073] In the step 2, the guar gum is:

[0074] The guar gum is white in appearance and can form a viscous colloid in cold water, with a viscosity of 5000 centipoise, a pH value of 6, and a particle size of 8 / μm;

[0075] Step 3: Mix soybean urease and cementing liquid at an enzyme-to-binder volume ratio of 1:1 and stir to form a solidifying solution;

[0076] The soybean urease extraction method in step 3 is:

[0077] The dried soybeans were ground into powder and passed through a 50-mesh sieve to obtain soybean powder; the soybean powder was mixed with deionized water to prepare a soybean solution with a concentration of 100 g / L; the soybean solution was centrifuged at a speed of 3000 r·min for 15 min, and the upper light yellow clear liquid was extracted, which was the soybean urease solution;

[0078] The method for preparing the cementing liquid in step 3 is as follows:

[0079] The urea solution of a certain concentration and the anhydrous calcium chloride solution were uniformly mixed in equal volumes to obtain a cementing solution with a concentration of 1.0 mol / L;

[0080] The concentration of the urea solution is 35 g / L;

[0081] The concentration of the anhydrous calcium chloride solution is 55.4 g / L;

[0082] Step 4: Add the solidification solution prepared in step 3 accounting for 7% of the dry soil mass to the mixed soil obtained in step 2, and mix evenly to obtain a solidified soil body;

[0083] Step 5: Fill the solidified soil obtained in step 4 into the sample maker coated with vaseline and prepare it in 4 layers. In order to ensure that every two contacting soil samples are better bonded together, the contact surface will be scraped after each layer is compacted, and then the next layer of soil is poured in. Repeat the operation until the fifth layer is compacted; place the solidified soil after compaction together with the sample maker in a curing room at 20°C for 10 hours; finally, open the sample maker, slowly separate the three inner walls that wrap the soil sample, and obtain the reinforced soil block after demolding.

[0084] Example 4

[0085] A method for reinforcing loess by inducing calcium carbonate deposition using guar gum and soybean urease, specifically comprising the following steps:

[0086] Step 1: Hammer the original air-dried loess, then sieve it through a 2 mm sieve, dry the sieved loess at 100°C to obtain dry soil for later use;

[0087] Step 2: According to the dry density of 1.65g / cm 3 Weigh a certain mass of the dry soil obtained in step 1, and fully mix the dry soil with 1.50% of guar gum by mass of the dry soil to obtain a mixed soil material;

[0088] In the step 2, the guar gum is:

[0089] The guar gum is white in appearance and can form a viscous colloid in cold water, with a viscosity of 5500 centipoise, a pH value of 7, and a particle size of 13 / μm;

[0090] Step 3: Mix soybean urease and cementing liquid at an enzyme-to-binder volume ratio of 1:2 and stir to form a solidifying solution;

[0091] The soybean urease extraction method in step 3 is:

[0092] The dried soybeans were ground into powder and passed through a 50-mesh sieve to obtain soybean powder; the soybean powder was mixed with deionized water to prepare a soybean solution with a concentration of 200 g / L; the soybean solution was centrifuged at a speed of 5000 r·min for 30 min, and the upper light yellow clear liquid was extracted, which was the soybean urease solution;

[0093] The method for preparing the cementing liquid in step 3 is as follows:

[0094] The urea solution of a certain concentration and the anhydrous calcium chloride solution were uniformly mixed in equal volumes to obtain a cementing solution with a concentration of 1.5 mol / L;

[0095] The concentration of the urea solution is 45 g / L;

[0096] The concentration of the anhydrous calcium chloride solution is 83 g / L;

[0097] Step 4: Add the solidification solution prepared in step 3 accounting for 14% of the dry soil mass to the mixed soil material obtained in step 2, and mix evenly to obtain a solidified soil body;

[0098] Step 5: Fill the solidified soil obtained in step 4 into the sample maker coated with vaseline and prepare it in 5 layers. In order to ensure that every two contacting soil samples are better bonded together, the contact surface will be scraped after each layer is compacted, and then the next layer of soil is poured in. Repeat the operation until the fifth layer is compacted; place the solidified soil after compaction together with the sample maker in a curing room at 24°C for 15 hours; finally, open the sample maker, slowly separate the three inner walls that wrap the soil sample, and obtain the reinforced soil block after demolding.

[0099] Test verification

[0100] In order to verify the feasibility of the scheme of the present invention, the following experiments were conducted to compare and analyze the effects of different guar gum contents, different soil dry densities or solidification solution contents on the permeability, disintegration and mechanical properties of loess.

[0101] The specific schemes for preparing different guar gum contents, dry densities, and solidification solution contents are shown in Table 1:

[0102] Table 1

[0103]

[0104] Test method: According to the standard of geotechnical test methods (GBT 50123-2019), permeability test, disintegration test and triaxial shear strength test were carried out on the solidified loess samples. The permeability coefficient was determined by the variable head method in the permeability test. The disintegration test was determined by a disintegration instrument, and the triaxial shear strength test was carried out by a triaxial test using a KTL-LDF 50 soil static triaxial testing machine to carry out an unconsolidated and undrained test;

[0105] The test results and conclusions are as follows:

[0106] The permeability, disintegration and triaxial shear strength characteristics of guar gum-solidified loess were studied experimentally.

[0107] The non-lateral compressive strength, triaxial shear strength, permeability and disintegration characteristics of loess solidified by guar gum combined with EICP were studied experimentally.

[0108] The effects of guar gum content and sample dry density on the compressive strength of solidified loess without lateral line were analyzed. Figure 2 is the relationship between guar gum content and sample dry density on the non-lateral compressive strength of solidified loess. Figure 2 It can be seen that the no-sideline compressive strength of the sample increases with the increase of dry density and guar gum content. The no-sideline compressive strength of loess solidified by guar gum combined with solidification solution is greater than that of loess solidified by a single solidification solution. This shows that the addition of guar gum provides more nucleation sites for the solidification solution in the soil and generates more calcium carbonate content, so the no-sideline compressive strength will increase. Due to the increase in dry density, the pores in the soil become smaller, and the calcium carbonate generated by the solidification solution fills the pores more tightly. Secondly, the solution generated by guar gum after meeting water penetrates into the fine pores of the soil, better wraps the soil, bonds calcium carbonate and soil particles, and stabilizes soil deformation. Therefore, with the increase of dry density, the no-sideline compressive strength of the soil will increase.

[0109] The effect of guar gum content on the triaxial shear strength of solidified loess was analyzed. Figure 3 is the relationship between guar gum content and triaxial shear strength of solidified loess. Figure 3 As shown in (a): Under a confining pressure of 25 kPa, the triaxial shear strength of EICP-solidified loess is significantly greater than that of untreated loess. With the addition of guar gum, the shear strength of the solidified loess increases with the increase of guar gum content. Figure 3 (b) Figure 3 As shown in (c), under high confining pressure, guar gum combined with EICP solidified loess exhibits higher shear strength, and single EICP solidified loess does not have higher shear strength than guar gum combined with EICP solidified loess. Under a confining pressure of 25 kPa, the shear strength of solidified loess with a guar gum content of 1.50% is not much different from that of solidified loess with a guar gum content of 2.00%. Under a confining pressure of 100 kPa, the shear strength of solidified loess with a guar gum content of 1.50% is not much different from that of solidified loess with a guar gum content of 2.00%. This is because the calcium carbonate content generated by urease solution with a guar gum content of 1.50% and a guar gum content of 2.00% is not much different, and it cannot play a better advantage. Therefore, the shear strength of solidified loess with a guar gum content of 1.50% is similar to that of solidified loess with a guar gum content of 2.00%.

[0110] The effect of guar gum content on the permeability coefficient of solidified loess was analyzed. Figure 4 is the relationship between guar gum content and permeability coefficient of solidified loess. Figure 4 (a) The permeability coefficient of EICP-solidified loess under a confining pressure of 25 kPa is 0.984610 -5 cm·s -1 , the permeability coefficient decreased by 33% compared with the untreated loess, indicating that the calcium carbonate generated by the solidification solution in the soil filled part of the pores, so the permeability of the loess decreased. When the guar gum content was 1.00%, the permeability coefficient of the co-solidified loess was 0.834210 -5 cm·s -1 Compared with EICP-solidified loess, the permeability coefficient is reduced by 15.5%, indicating that the gel generated by guar gum after contact with water fills part of the soil pores not filled by calcium carbonate. As the confining pressure increases further, the soil becomes compact and the pores become smaller. The permeability of guar gum combined with EICP-solidified loess decreases more significantly. When the guar gum content is 2.00%, the permeability coefficient of the combined solidified loess is 0.22510 -5 cm·s -1 , the permeability coefficient decreased by 62.3% compared with the untreated loess.

[0111] The effect of guar gum content on disintegration was analyzed. Figure 5 The figure is the relationship between guar gum content and disintegration amount. Figure 5It can be seen that the untreated loess completely disintegrated in water within 500s, while the guar gum combined with EICP solidified loess still did not completely disintegrate after 1800s. And the disintegration amount of the solidified soil gradually decreased with the increase of guar gum content. The main reason is that with the increase of guar gum content, the degree of adhesion of the gum to the soil particles is enhanced, which not only bonds the calcium carbonate in the soil but also stabilizes the movement of the soil particles, thus improving the disintegration resistance of the solidified loess.

[0112] The effect of guar gum content on calcium carbonate production was analyzed. Figure 6 The figure is the relationship between guar gum content and calcium carbonate production. Figure 6 It can be seen that with the increase of guar gum content, the amount of calcium carbonate generated also gradually increases, but the calcium carbonate content generated by guar gum content of 1.50% and guar gum content of 2.00% is not much different. The calcium carbonate content generated by guar gum content of 1.50% and guar gum content of 1.00% is significantly different. This may be because the content of the solidified solution limits the reaction of higher content guar gum. Therefore, under the experimental conditions, when the guar gum content is 1.50%, it is the optimal content considering economic benefits.

[0113] It can be seen from the above embodiments that compared with the prior art:

[0114] The present invention adopts an innovative method of combining guar gum with EICP to reinforce loess, and the synergistic effect of the two significantly improves the solidification effect of loess. Guar gum reacts with water to form a highly fluid hydrogel, which effectively fills soil voids and reduces soil permeability. The solidification solution generates calcium carbonate precipitation in the soil, which fills the soil pores and makes the soil dense, thereby improving the strength of the soil.

[0115] When guar gum is combined with EICP to solidify loess, the addition of guar gum provides more nucleation sites for the solidification solution, which not only increases the amount of calcium carbonate generated in the soil, but also makes the generated calcium carbonate particles larger in volume. The anchoring zone formed after hydration of guar gum tightly locks the calcium carbonate, while the hydrate fills the voids in the soil sample, enhances the soil density, increases the contact area and interaction force between calcium carbonate and the soil medium, and makes the solidified loess show excellent mechanical properties.

[0116] Compared with the traditional loess solidification method, the present invention adopts the natural green material guar gum and solidification solution, which will not pollute the soil and can be self-degraded. It will not pollute the environment and affect the growth of vegetation, and it can significantly improve the strength of the soil and reduce the water sensitivity of the soil.

[0117] Compared with the MICP method of solidifying soil, the present invention is simple to operate, green, pollution-free, and does not cause danger during the sample preparation process. It does not require the cultivation of bacteria, is safer to a certain extent, and does not produce bacterial microorganisms that affect the ecological balance of the soil when solidifying the soil.

[0118] Compared with the EICP method of solidifying soil, a single EICP cannot determine the nucleation site. The present invention adds guar gum to provide more nucleation sites for a single solidification solution, the amount of calcium carbonate generated gradually increases, and the soil reinforcement effect is more obvious.

[0119] In summary, the present invention uses natural, degradable, green and environmentally friendly materials, which not only effectively avoids the ecological impact on the soil, but also shows good adaptability to environmental conditions during the solidification process. The effect of guar gum combined with EICP in reinforcing loess is extremely significant, reducing the water sensitivity and permeability of the solidified soil, and improving the compressive strength, crack resistance and water stability of loess.

[0120] The present invention and its embodiments are described above, which is not restrictive. The drawings are only one of the embodiments of the present invention. In short, if ordinary technicians in the field are inspired by it and design structural methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A method for strengthening loess by inducing calcium carbonate deposition by combining guar gum with soybean urease, characterized in that: The specific steps include: Step 1: Hammer the original air-dried loess, then sieve it through a 2-4 mm sieve, and dry the sieved loess at 95-105°C to obtain dry soil for later use; Step 2: According to the dry density of 1.44-1.65g / cm 3 Weigh a certain mass of the dry soil obtained in step 1, and fully mix the dry soil with 1.00%-2.00% of guar gum by mass of the dry soil to obtain a mixed soil material; Step 3: mixing soybean urease and a binder at an enzyme-to-binder volume ratio of 1:1, 1:2 or 1:3 and stirring to prepare a solidification solution; Step 4: Add the solidification solution prepared in step 3 accounting for 7% to 14% of the dry soil mass to the mixed soil material obtained in step 2, and mix evenly to obtain a solidified soil body; Step 5: compact the solidified soil obtained in step 4 in 4-5 layers, scrape the soil between the layers, let it stand at 20-24°C for 10-15h, and obtain reinforced soil blocks after demoulding.

2. The method for strengthening loess by inducing calcium carbonate deposition by combining guar gum and soybean urease according to claim 1, characterized in that: In the step 2, the guar gum is: The guar gum is white in appearance and can form a viscous colloid in cold water. The viscosity of the guar gum is 5000-5500 centipoise, the pH value is 6-8, and the particle size is 8-15 / μm.

3. The method for reinforcing loess by inducing calcium carbonate deposition by combining guar gum with soybean urease according to claim 1, characterized in that: The soybean urease extraction method in step 3 is: The dried soybeans are ground into powder and passed through a 50-100 mesh sieve to obtain soybean powder; the soybean powder is mixed with deionized water to prepare a soybean solution with a concentration of 100-200 g / L; the soybean solution is centrifuged at a speed of 3000-5000 r·min for 15-30 minutes, and the upper light yellow clear liquid is extracted, which is the soybean urease solution.

4. The method for reinforcing loess by inducing calcium carbonate deposition by combining guar gum and soybean urease according to claim 1, characterized in that: The method for preparing the cementing liquid in step 3 is as follows: A urea solution of a certain concentration is uniformly mixed with anhydrous calcium chloride solution in equal volumes to obtain a cementing liquid with a concentration of 0.5-2.0 mol / L.

5. The method for reinforcing loess by inducing calcium carbonate deposition by combining guar gum with soybean urease according to claim 4, characterized in that: The concentration of the urea solution is 15-65 g / L.

6. The method for consolidating loess by inducing calcium carbonate deposition by combining guar gum and soybean urease according to claim 4, characterized in that: The concentration of the anhydrous calcium chloride solution is 20-120 g / L.

7. A method for strengthening loess by inducing calcium carbonate deposition using guar gum and soybean urease, characterized in that: The specific steps include: Step 1: Hammer the original air-dried loess, then sieve it through a 4 mm sieve, place the sieved loess at 105°C for drying, and prepare dry soil for later use; Step 2: According to the dry density of 1.65g / cm 3 Weigh a certain mass of the dry soil obtained in step 1, and fully mix the dry soil with 2.00% guar gum by mass of the dry soil to obtain a mixed soil material; In the step 2, the guar gum is: The guar gum is white in appearance and can form a viscous colloid in cold water, with a viscosity of 5500 centipoise, a pH value of 8, and a particle size of 15 / μm; Step 3: Mix soybean urease and cementing liquid at an enzyme-to-binder volume ratio of 1:3 and stir to form a solidifying solution; The soybean urease extraction method in step 3 is: The dried soybeans were ground into powder and passed through a 100-mesh sieve to obtain soybean powder; the soybean powder was mixed with deionized water to prepare a soybean solution with a concentration of 200 g / L; the soybean solution was centrifuged at a speed of 5000 r·min for 30 min, and the upper light yellow clear liquid was extracted, which was the soybean urease solution; The method for preparing the cementing liquid in step 3 is as follows: The urea solution of a certain concentration and the anhydrous calcium chloride solution were uniformly mixed in equal volumes to obtain a cementing solution with a concentration of 2.0 mol / L; The concentration of the urea solution is 60 g / L; The concentration of the anhydrous calcium chloride solution is 110.98 g / L; Step 4: Add the solidification solution prepared in step 3 accounting for 14% of the dry soil mass to the mixed soil material obtained in step 2, and mix evenly to obtain a solidified soil body; Step 5: compact the solidified soil obtained in step 4 in 5 layers, scrape the soil between the layers, let it stand at 24°C for 15 hours, and obtain reinforced soil blocks after demoulding.

8. A method for strengthening loess by inducing calcium carbonate deposition using guar gum and soybean urease, characterized in that: The specific steps include: Step 1: Hammer the original air-dried loess, then sieve it through a 3mm sieve, dry the sieved loess at 100°C to obtain dry soil for later use; Step 2: According to the dry density of 1.55g / cm 3 Weigh a certain mass of the dry soil obtained in step 1, and fully mix the dry soil with 1.50% of guar gum by mass of the dry soil to obtain a mixed soil material; In the step 2, the guar gum is: The guar gum is white in appearance and can form a viscous colloid in cold water, with a viscosity of 5300 centipoise, a pH value of 7, and a particle size of 11 / μm; Step 3: Mix soybean urease and cementing liquid at an enzyme-to-binder volume ratio of 1:2 and stir to form a solidifying solution; The soybean urease extraction method in step 3 is: The dried soybeans were ground into powder and passed through a 75-mesh sieve to obtain soybean powder; the soybean powder was mixed with deionized water to prepare a soybean solution with a concentration of 200 g / L; the soybean solution was centrifuged at a speed of 4000 r·min for 20 min, and the upper light yellow clear liquid was extracted, which was the soybean urease solution; The method for preparing the cementing liquid in step 3 is as follows: The urea solution of a certain concentration and the anhydrous calcium chloride solution were uniformly mixed in equal volumes to obtain a cementing solution with a concentration of 1.5 mol / L; The concentration of the urea solution is 45 g / L; The concentration of the anhydrous calcium chloride solution is 83 g / L; Step 4: Add the solidification solution prepared in step 3 accounting for 10% of the dry soil mass to the mixed soil material obtained in step 2, and mix evenly to obtain a solidified soil body; Step 5: compact the solidified soil obtained in step 4 in 5 layers, scrape the soil between the layers, let it stand at 22°C for 12 hours, and obtain reinforced soil blocks after demoulding.

9. A method for strengthening loess by inducing calcium carbonate deposition by combining guar gum with soybean urease, characterized in that: The specific steps include: Step 1: Hammer the original air-dried loess, then sieve it through a 2mm sieve, dry the sieved loess at 95°C to obtain dry soil for later use; Step 2: According to the dry density of 1.44g / cm 3 Weigh a certain mass of the dry soil obtained in step 1, and fully mix the dry soil with 1.00% guar gum by mass of the dry soil to obtain a mixed soil material; In the step 2, the guar gum is: The guar gum is white in appearance and can form a viscous colloid in cold water, with a viscosity of 5000 centipoise, a pH value of 6, and a particle size of 8 / μm; Step 3: Mix soybean urease and cementing liquid at an enzyme-to-binder volume ratio of 1:1 and stir to form a solidifying solution; The soybean urease extraction method in step 3 is: The dried soybeans were ground into powder and passed through a 50-mesh sieve to obtain soybean powder; the soybean powder was mixed with deionized water to prepare a soybean solution with a concentration of 100 g / L; the soybean solution was centrifuged at a speed of 3000 r·min for 15 min, and the upper light yellow clear liquid was extracted, which was the soybean urease solution; The method for preparing the cementing liquid in step 3 is as follows: The urea solution of a certain concentration and the anhydrous calcium chloride solution were uniformly mixed in equal volumes to obtain a cementing solution with a concentration of 1.0 mol / L; The concentration of the urea solution is 35 g / L; The concentration of the anhydrous calcium chloride solution is 55.4 g / L; Step 4: Add the solidification solution prepared in step 3 accounting for 7% of the dry soil mass to the mixed soil obtained in step 2, and mix evenly to obtain a solidified soil body; Step 5: compact the solidified soil obtained in step 4 in 4 layers, scrape the layers, let it stand at 20°C for 10 hours, and obtain reinforced soil blocks after demoulding.

10. A method for strengthening loess by inducing calcium carbonate deposition by combining guar gum with soybean urease, characterized in that: The specific steps include: Step 1: Hammer the original air-dried loess, then sieve it through a 2 mm sieve, dry the sieved loess at 100°C to obtain dry soil for later use; Step 2: According to the dry density of 1.65g / cm 3 Weigh a certain mass of the dry soil obtained in step 1, and fully mix the dry soil with 1.50% of guar gum by mass of the dry soil to obtain a mixed soil material; In the step 2, the guar gum is: The guar gum is white in appearance and can form a viscous colloid in cold water, with a viscosity of 5500 centipoise, a pH value of 7, and a particle size of 13 / μm; Step 3: Mix soybean urease and cementing liquid at an enzyme-to-binder volume ratio of 1:2 and stir to form a solidifying solution; The soybean urease extraction method in step 3 is: The dried soybeans were ground into powder and passed through a 50-mesh sieve to obtain soybean powder; the soybean powder was mixed with deionized water to prepare a soybean solution with a concentration of 200 g / L; the soybean solution was centrifuged at a speed of 5000 r·min for 30 min, and the upper light yellow clear liquid was extracted, which was the soybean urease solution; The method for preparing the cementing liquid in step 3 is as follows: The urea solution of a certain concentration and the anhydrous calcium chloride solution were uniformly mixed in equal volumes to obtain a cementing solution with a concentration of 1.5 mol / L; The concentration of the urea solution is 45 g / L; The concentration of the anhydrous calcium chloride solution is 83 g / L; Step 4: Add the solidification solution prepared in step 3 accounting for 14% of the dry soil mass to the mixed soil material obtained in step 2, and mix evenly to obtain a solidified soil body; Step 5: compact the solidified soil obtained in step 4 in 5 layers, scrape the soil between the layers, let it stand at 24°C for 15 hours, and obtain reinforced soil blocks after demoulding.

Citation Information

Cited By

  • Enzyme-induced calcium carbonate precipitation and vegetation synergistic slope covering layer and construction method thereof

    CN122304380A

  • Design method for soil solidification by inducing calcium carbonate precipitation through urease

    CN122548851A