Cam bearing seat structure, machining method thereof, engine and vehicle

By adjusting the raw material composition and processing methods of aluminum alloy, the problem of increasing weight and wear of aluminum-based bimetal bushings is solved, and the lightweight and wear resistance of the cam bearing seat is achieved, extending the service life and simplifying the process.

CN118912108AActive Publication Date: 2024-11-08DONGFENG COMML VEHICLE CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410998368.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

In the traditional heavy-duty diesel engine cam bearing seat assembly, the aluminum-based bimetal bushing increases the weight of the car body, and under special working conditions, there is a situation where the shaft is held, which is difficult to process and can easily lead to tool wear.

Method used

By changing the raw material composition of the cam bearing seat structure, including the ratio of Si, Mg, Mn, Ti, Sr and Zr, the weight is reduced and the process is simplified, the bushing is eliminated, the lubricating oil tank is used to reduce friction, and the solution treatment and aging treatment is improved Material wear resistance and yield strength.

Benefits of technology

The cam bearing seat structure is lightweight, wear resistance and high temperature strength, reducing the use of bushings, extending service life, and simplifying the processing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118912108A_ABST
    Figure CN118912108A_ABST
Patent Text Reader

Abstract

The invention discloses a cam bearing seat structure, a machining method thereof, an engine and a vehicle, and relates to the technical field of vehicles. Comprising a bearing base and a bearing upper cover, the bearing base and the bearing upper cover form a cam shaft hole for mounting a cam, the side wall of the cam shaft hole is provided with a lubricating oil groove, and the cam bearing seat structure comprises the following raw materials in percentage by mass: 11.5-14.5% of Si, 11.5-14.5% of Cr, 11.5-14.5% of Mo, 11.5-14.5% of Mo, and the balance of Fe. 0.35% to 0.45% of Mg; 0.35% to 0.50% of Mn; 0.06% to 0.12% of Ti; 0.015% to 0.025% of Sr; 0.01% to 0.1% of Zr; and the balance of Al and inevitable impurities. By changing the raw material composition of the cam bearing seat structure, the weight of the cam bearing seat structure can be reduced, so that the upper cover and the base of the cam bearing seat structure can be made of the same material, and meanwhile, different bearing and wear-resisting requirements of the upper cover and the base of the cam bearing seat structure are met; therefore, bushings do not need to be arranged between the upper cover and the base of the cam bearing seat structure and the cam shaft.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of vehicle technology, and in particular to a cam bearing seat structure and a processing method thereof, an engine and a vehicle. Background Art

[0002] The traditional heavy-duty diesel engine cam bearing seat assembly consists of two parts: a base and an upper cover. The base usually only bears pressure, so it is generally made of cast iron to meet the strength requirements. The upper seat needs to be assembled with the intake and exhaust rocker arm shafts, so it needs to have a higher body strength. If the engine has an exhaust brake function, the upper cover body strength requirements are higher, so the upper cover is usually made of high-grade ductile iron or forged steel.

[0003] The camshaft runs in the cam bearing hole composed of the base and the upper cover. The camshaft is usually made of chilled cast iron or carbon steel, which causes severe wear of the friction pair between the camshaft and the cam bearing seat hole even in the oil lubrication state. Therefore, the cam bearing hole of the traditional steel and iron cam bearing seat assembly needs to be equipped with an aluminum-based bimetallic bushing.

[0004] On the one hand, the aluminum-based bimetallic bushing increases the weight of the entire vehicle body and does not meet the requirements of lightweight. On the other hand, under special working conditions, there is a situation where polishing leads to shaft seizure. In addition, the lubricating oil channel on the aluminum-based bimetallic bushing is slender, which makes processing difficult and easily causes tool wear. Summary of the invention

[0005] The present application provides a cam bearing seat structure and a processing method thereof, an engine and a vehicle, so as to solve the problems that the existing aluminum-based bimetallic bushing increases the weight of the entire vehicle body and fails to meet the requirements of lightweight, and on the other hand, there is a situation where the shaft is stuck due to polishing under special working conditions, and the lubricating oil channel on the aluminum-based bimetallic bushing is slender, which makes the processing difficult and easily causes tool wear.

[0006] In a first aspect, the present application provides a cam bearing seat structure, comprising a bearing base and a bearing upper cover, wherein the bearing base and the bearing upper cover form a camshaft hole for mounting a cam, and the side wall of the camshaft hole has a lubricating oil groove, wherein:

[0007] Measured by mass fraction, the raw material composition of the cam bearing seat structure includes: Si: 11.5% to 14.5%; Mg: 0.35% to 0.45%; Mn: 0.35% to 0.50%; Ti: 0.06% to 0.12%; Sr: 0.015% to 0.025%; Zr: 0.01% to 0.1%; the remainder is Al and unavoidable impurities.

[0008] By changing the raw material composition of the cam bearing seat structure, the present application can reduce the weight of the cam bearing seat structure on the one hand, so that the upper cover and the base of the cam bearing seat structure can be processed with the same material, simplifying the process, and at the same time, it can simultaneously meet the different load-bearing and wear-resistant requirements of the upper cover and the base of the cam bearing seat structure, so that there is no need to set a bushing between the upper cover and the base of the cam bearing seat structure and the camshaft, reducing the use of bushings. Wherein the mass fraction of Si is within this range, good fluidity can be obtained, and at the same time, the cam bearing seat casting can obtain good wear resistance. The mass fraction of Mg is within this range, and the material can obtain the optimal yield strength and elongation through solution treatment + artificial aging. The mass fraction of Mn is within this range, while the material can obtain good anti-sticking properties, it can also form a "Chinese character-shaped" Fe-Mn compound with Fe added to the alloy, thereby weakening the negative impact of the lattice of needle-shaped Fe relative to the matrix structure on the yield strength and elongation of the material. The mass fraction of Ti is within this range, and the organization can be refined and reach a grain size of 7-8, thereby obtaining a good yield strength. The mass fraction of Sr is within this range, and a good modification effect can be obtained, thereby improving the yield strength of the material. When the mass fraction of Zr is within this range, the recrystallization temperature of the alloy can be increased, thereby improving the high temperature strength of the material.

[0009] It should be noted that, since the bushing structure is eliminated, in order to reduce the friction and shaft sticking between the camshaft and the cam bearing seat, a lubricating oil groove is provided on the side wall of the camshaft hole, so that the camshaft and the cam bearing seat are protected by lubricating oil and hard friction is reduced. Specifically, as an example, the oil supply pressure of the lubricating oil can be 0.68-0.72MPa, and the oil temperature of the lubricating oil can be 80-120°C.

[0010] In order to further improve the reliability of the upper cover and base of the cam bearing seat structure, in actual use, the maximum linear speed between the camshaft and the cam bearing seat is usually less than or equal to 10m / s, which can increase the service life of the upper cover and base of the cam bearing seat structure.

[0011] In some embodiments, the metallographic structure of the cam bearing seat structure includes an α-Al phase and a eutectic silicon phase. The eutectic silicon phase is relatively hard, while the α-Al phase is relatively soft. The cam bearing seat structure contains both a relatively soft phase that plays a lubricating role and a relatively hard phase that plays a wear-resistant role, thereby achieving different load-bearing and wear-resistant requirements for the upper cover and base of the cam bearing seat structure, so that there is no need to set a bushing between the upper cover and base of the cam bearing seat structure and the camshaft, reducing the use of bushings. The upper cover and base of the cam bearing seat structure can be processed with the same material to simplify the process.

[0012] In some embodiments, the mass ratio of Si to Al is (13-17): 100. Suitable α-Al phase and eutectic silicon phase can be formed, thereby improving the wear resistance and strength of the parts at the same time, and obtaining better wear resistance and sapphire fatigue performance.

[0013] In some embodiments, the load-bearing capacity of the cam bearing seat structure is 0.1 to 100 MPa. The load-bearing capacity of the cam bearing seat structure is within this range, which can further enable the upper cover and the base of the cam bearing seat structure to be processed with the same material, and the upper cover and the base of the cam bearing seat structure to maintain their respective different load requirements without the need for a bushing between the upper cover and the base of the cam bearing seat structure and the camshaft, thereby reducing the wear and failure of the upper cover and the base of the cam bearing seat structure, and improving the reliability of the upper cover and the base of the cam bearing seat structure.

[0014] In a second aspect, the present application provides a method for processing a cam bearing seat structure, comprising the following steps:

[0015] Mixing and melting the raw materials according to the raw material components to obtain an aluminum alloy melt;

[0016] The aluminum alloy melt is refined, slag-removed, degassed, modified and cooled to obtain a pretreated melt;

[0017] Casting the pretreated solution into a mold and demoulding it to obtain a prefabricated part;

[0018] The prefabricated parts are subjected to solid solution treatment, quenching and aging treatment to obtain a cam bearing seat structure.

[0019] By changing the raw material composition of the cam bearing seat structure, on the one hand, the weight of the cam bearing seat structure can be reduced, so that the upper cover and the base of the cam bearing seat structure can be processed with the same material, simplifying the process, and at the same time, it can simultaneously meet the different load-bearing and wear-resistant requirements of the upper cover and the base of the cam bearing seat structure, so that there is no need to set a bushing between the upper cover and the base of the cam bearing seat structure and the camshaft, thereby reducing the use of bushings.

[0020] In some embodiments, the pre-treated solution is molded and demolded to obtain a preform, and the mold is filled with a graphite powder layer, wherein:

[0021] The particle size of the graphite powder is 800 to 1000 nm; and / or,

[0022] The thickness of the graphite powder layer is 40 to 50 μm.

[0023] Specifically, a layer of graphite powder can be sprayed on the mold surface by electrostatic spraying, and then the mold is closed, and the treated aluminum alloy melt is pushed into the mold cavity from bottom to top along the riser pipe from the insulation furnace below the mold using high-purity nitrogen. The particle size of the graphite powder and the thickness of the graphite powder layer within this range can be more conducive to demolding and make the surface of the part smoother.

[0024] The specific casting process may be that after the aluminum alloy melt fills the mold cavity, the central extrusion column above the mold gate begins to descend and closes the gate to complete the filling process. At this time, the high-purity nitrogen in the insulation furnace is depressurized, and the excess aluminum alloy melt in the riser flows back into the insulation furnace. The central extrusion column is further descended to extrude all the aluminum alloy melt below the shoulder of the central extrusion column into the mold cavity of the mold forming casting part, and the aluminum alloy melt is demolded after it is completely solidified. The central extrusion column includes an upper end and a lower end of the extrusion column, the diameter of the upper end of the central extrusion column is greater than the diameter of the lower end, and the diameter of the upper end of the central extrusion column is 1.8 to 2.0 times the diameter of the lower end; the diameter of the lower end of the central extrusion column is adapted to the diameter of the mold gate; the slope of the transition zone between the upper end and the lower end of the central extrusion column is 45° to 60°; the extrusion pressure of the central extrusion column is 60MPa to 90MPa. The surface of the central extrusion column is sprayed with a graphite powder coating with a particle size of 800nm ​​to 1000nm and a thickness of 40μm to 50μm.

[0025] In some embodiments, the preform is subjected to solution treatment, quenching and aging treatment to obtain a cam bearing seat structure:

[0026] The solution temperature is 500-540°C; and / or,

[0027] The solution time is 2 to 4 hours; and / or,

[0028] The aging temperature is 160-180°C; and / or

[0029] The aging time is 2 to 4 hours.

[0030] Under this solution temperature, solution time, aging temperature and aging time, the cam bearing seat structure can have both a relatively soft phase that plays a lubricating role and a relatively hard phase that plays a wear-resistant role, thereby achieving different load-bearing and wear-resistant requirements for the upper cover and base of the cam bearing seat structure, so that there is no need to set a bushing between the upper cover and base of the cam bearing seat structure and the camshaft, reducing the use of bushings. The upper cover and base of the cam bearing seat structure can be processed with the same material, simplifying the process.

[0031] In some embodiments, the preform is subjected to solution treatment, quenching, and aging treatment to obtain the cam bearing seat structure, and the quenching treatment method includes water quenching, wherein:

[0032] The water quenching temperature is 70 to 90°C; and / or,

[0033] The water quenching time is 8 to 15 minutes.

[0034] The use of water quenching can make the cam bearing seat obtain higher comprehensive mechanical properties. Under this water quenching and temperature, a higher cooling rate can be obtained, reducing the precipitation of strengthening phase from the solid solution, thereby obtaining an excellent strengthening effect.

[0035] In a third aspect, the present application provides an engine, comprising the cam bearing seat structure described in the first aspect, or a cam bearing seat structure manufactured by the processing method of the cam bearing seat structure of the second aspect.

[0036] In a fourth aspect, the present application provides a vehicle comprising the parts of the third aspect. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0038] Figure 1 This is a structural diagram of a cam bearing seat according to an embodiment of the present application.

[0039] Figure 2 This is a metallographic diagram of a cam bearing seat structure according to an embodiment of the present application.

[0040] Description of Figure Numbers:

[0041] 100 cam bearing seat structure; 1 bearing base; 2 bearing upper cover; 3 camshaft hole; 31 lubricating oil groove. DETAILED DESCRIPTION

[0042] In order to make the purpose, technical solution and advantages of the present application clearer, the technical solution of the present application will be clearly and completely described below in combination with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.

[0043] The traditional heavy-duty diesel engine cam bearing seat assembly consists of two parts: a base and an upper cover. The base usually only bears pressure, so it is generally made of cast iron to meet the strength requirements. The upper seat needs to be assembled with the intake and exhaust rocker arm shafts, so it needs to have a higher body strength. If the engine has an exhaust brake function, the upper cover body strength requirements are higher, so the upper cover is usually made of high-grade ductile iron or forged steel.

[0044] The camshaft runs in the cam bearing hole composed of the base and the upper cover. The camshaft is usually made of chilled cast iron or carbon steel, which causes severe wear of the friction pair between the camshaft and the cam bearing seat hole even in the oil lubrication state. Therefore, the cam bearing hole of the traditional steel and iron cam bearing seat assembly needs to be equipped with an aluminum-based bimetallic bushing.

[0045] On the one hand, the aluminum-based bimetallic bushing increases the weight of the entire vehicle body and does not meet the requirements of lightweight. On the other hand, under special working conditions, there is a situation where polishing leads to shaft seizure. In addition, the lubricating oil channel on the aluminum-based bimetallic bushing is slender, which makes processing difficult and easily causes tool wear.

[0046] The traditional forged steel or cast iron cam bearing seat assembly needs to be equipped with an aluminum-based bimetallic bushing in the cam bearing hole. Its structure includes a wear-resistant layer and a steel backing layer, wherein the wear-resistant layer contacts the camshaft, and the steel backing layer contacts the cam bearing seat. The wear-resistant layer is AlSn20Cu alloy with a thickness of 0.2 to 0.5 mm, and the steel backing layer plays a supporting role and is 08Al with a thickness of 1 to 4 mm. In actual engineering applications, the camshaft hole lubricating oil cannot be pumped into the bushing in time during the cold start of the engine, resulting in short-term dry friction, causing the engine to work abnormally.

[0047] In view of this, the present application provides a cam bearing seat structure and a processing method thereof, an engine and a vehicle, so as to solve the problem that the existing aluminum-based bimetallic bushing, on the one hand, increases the weight of the entire vehicle body and fails to meet the requirements of lightweight; on the other hand, there is a situation where polishing causes shaft seizure under special working conditions, and the lubricating oil channel on the aluminum-based bimetallic bushing is slender, which makes processing difficult and easily causes tool wear.

[0048] like Figure 1 As shown, in the first aspect, the present application provides a cam bearing seat structure 100, comprising a bearing base 1 and a bearing upper cover 2, wherein the bearing base 1 and the bearing upper cover 2 form a camshaft hole 3 for mounting a cam, and the side wall of the camshaft hole 3 has a lubricating oil groove 31, wherein:

[0049] In terms of mass fraction, the raw material composition of the cam bearing seat structure 100 includes: Si: 11.5% to 14.5%; Mg: 0.35% to 0.45%; Mn: 0.35% to 0.50%; Ti: 0.06% to 0.12%; Sr: 0.015% to 0.025%; Zr: 0.01% to 0.1%; the remainder is Al and unavoidable impurities.

[0050] By changing the raw material composition of the cam bearing seat structure 100, the present application can reduce the weight of the cam bearing seat structure on the one hand, so that the upper cover and the base of the cam bearing seat structure 100 can be processed with the same material, simplifying the process, and at the same time, it can simultaneously meet the different load-bearing and wear-resistant requirements of the upper cover and the base of the cam bearing seat structure 100, so that there is no need to set a bushing between the upper cover and the base of the cam bearing seat structure 100 and the camshaft, reducing the use of the bushing. Wherein the mass fraction of Si is within this range, good wear resistance can be obtained, making it possible to cancel the bushing. The mass fraction of Mg is within this range, and the material can obtain the optimal yield strength and elongation through solution treatment + artificial aging. The mass fraction of Mn is within this range, which can allow the material to obtain better anti-sticking properties, and can also form a "Chinese character-shaped" Fe-Mn compound with Fe added to the alloy, thereby weakening the negative impact of the lattice of needle-shaped Fe relative to the matrix structure on the yield strength and elongation of the material. The mass fraction of Ti is within this range, and the organization can be refined and reach a grain size of 7-8, thereby obtaining a good yield strength. When the mass fraction of Sr is within this range, a better modification effect can be obtained, thereby improving the yield strength of the material. When the mass fraction of Zr is within this range, the recrystallization temperature of the alloy can be increased, thereby improving the high temperature strength of the material. The lubricating oil groove 31 is arranged on the side wall of the camshaft hole 3, which is easier to process and more conducive to the flow of lubricating oil, thereby reducing the occurrence of shaft seizure.

[0051] It should be noted that, since the structure of the bushing is eliminated, in order to reduce the friction and shaft sticking between the camshaft and the cam bearing seat, a lubricating oil groove 31 is provided on the side wall of the camshaft hole 3, so that the camshaft and the cam bearing seat are protected by lubricating oil, reducing hard friction. Specifically, as an example, the oil supply pressure of the lubricating oil can be 0.68-0.72MPa, and the oil temperature of the lubricating oil can be 80-120°C.

[0052] In order to further improve the reliability of the upper cover and the base of the cam bearing seat structure 100, in actual use, the maximum linear velocity between the camshaft and the cam bearing seat is usually less than or equal to 10 m / s, which can improve the service life of the upper cover and the base of the cam bearing seat structure 100.

[0053] like Figure 2As shown, in combination with the first aspect, in some embodiments provided in the present application, the metallographic structure of the cam bearing seat structure 100 includes an α-Al phase and a eutectic silicon phase. The eutectic silicon phase is relatively hard, while the α-Al phase is relatively soft. The cam bearing seat structure 100 has both a relatively soft phase that plays a lubricating role and a relatively hard phase that plays a wear-resistant role in its structure, thereby achieving different load-bearing and wear-resistant requirements for the upper cover and base of the cam bearing seat structure 100, so that there is no need to set a bushing between the upper cover and base of the cam bearing seat structure 100 and the camshaft, thereby reducing the use of bushings. The upper cover and base of the cam bearing seat structure 100 can be processed with the same material to simplify the process.

[0054] In combination with the first aspect, in some embodiments provided in the present application, the mass ratio of Si to Al is (13-17): 100. Suitable α-Al phase and eutectic silicon phase can be formed, thereby improving the wear resistance and strength of the parts at the same time, and obtaining better wear resistance and sapphire fatigue performance.

[0055] In combination with the first aspect, in some embodiments provided in the present application, the load-bearing capacity of the cam bearing seat structure 100 is 0.1 to 100 MPa. The load-bearing capacity of the cam bearing seat structure 100 is within this range, which can further enable the upper cover and the base of the cam bearing seat structure 100 to be processed with the same material, and the upper cover and the base of the cam bearing seat structure 100 to maintain their respective different load requirements without the need for a bushing between the upper cover and the base of the cam bearing seat structure 100 and the camshaft, thereby reducing the wear and failure of the upper cover and the base of the cam bearing seat structure 100, and improving the reliability of the upper cover and the base of the cam bearing seat structure 100.

[0056] In a second aspect, the present application provides a method for processing a cam bearing seat structure, comprising the following steps:

[0057] Mixing and melting the raw materials according to the raw material components to obtain an aluminum alloy melt;

[0058] The aluminum alloy melt is refined, slag-removed, degassed, modified and cooled to obtain a pretreated melt;

[0059] Casting the pretreated solution into a mold and demoulding it to obtain a prefabricated part;

[0060] The prefabricated parts are subjected to solid solution treatment, quenching and aging treatment to obtain a cam bearing seat structure.

[0061] By changing the raw material composition of the cam bearing seat structure, on the one hand, the weight of the cam bearing seat structure can be reduced, so that the upper cover and the base of the cam bearing seat structure can be processed with the same material, simplifying the process, and at the same time, it can simultaneously meet the different load-bearing and wear-resistant requirements of the upper cover and the base of the cam bearing seat structure, so that there is no need to set a bushing between the upper cover and the base of the cam bearing seat structure and the camshaft, thereby reducing the use of bushings.

[0062] In combination with the second aspect, in some embodiments provided in the present application, the pretreated solution is molded and demolded to obtain a preform, and the mold is filled with a graphite powder layer, wherein the particle size of the graphite powder is 800 to 1000 nm.

[0063] In combination with the second aspect, in some embodiments provided in the present application, the pretreated solution is molded and demolded to obtain a preform, and the mold is filled with a graphite powder layer, wherein the thickness of the graphite powder layer is 40 to 50 μm.

[0064] Specifically, a layer of graphite powder can be sprayed on the mold surface by electrostatic spraying, and then the mold is closed, and the treated aluminum alloy melt is pushed into the mold cavity from bottom to top along the riser pipe from the insulation furnace below the mold using high-purity nitrogen. The particle size of the graphite powder and the thickness of the graphite powder layer within this range can be more conducive to demolding and make the surface of the part smoother.

[0065] The specific casting process may be that after the aluminum alloy melt fills the mold cavity, the central extrusion column above the mold gate begins to descend and closes the gate to complete the filling process. At this time, the high-purity nitrogen in the insulation furnace is depressurized, and the excess aluminum alloy melt in the riser flows back into the insulation furnace. The central extrusion column is further descended to extrude all the aluminum alloy melt below the shoulder of the central extrusion column into the mold cavity of the mold forming casting part, and the aluminum alloy melt is demolded after it is completely solidified. The central extrusion column includes an upper end and a lower end of the extrusion column, the diameter of the upper end of the central extrusion column is greater than the diameter of the lower end, and the diameter of the upper end of the central extrusion column is 1.8 to 2.0 times the diameter of the lower end; the diameter of the lower end of the central extrusion column is adapted to the diameter of the mold gate; the slope of the transition zone between the upper end and the lower end of the central extrusion column is 45° to 60°; the extrusion pressure of the central extrusion column is 60MPa to 90MPa. The surface of the central extrusion column is sprayed with a graphite powder coating with a particle size of 800nm ​​to 1000nm and a thickness of 40μm to 50μm.

[0066] In combination with the second aspect, in some embodiments provided in the present application, the preform is subjected to solution treatment, quenching and aging treatment to obtain a cam bearing seat structure: the solution temperature is 500-540°C.

[0067] In combination with the second aspect, in some embodiments provided in the present application, the preform is subjected to solution treatment, quenching and aging treatment to obtain a cam bearing seat structure: the solution treatment time is 2 to 4 hours.

[0068] In combination with the second aspect, in some embodiments provided in the present application, the preform is subjected to solution treatment, quenching and aging treatment to obtain a cam bearing seat structure: the aging temperature is 160-180°C.

[0069] In combination with the second aspect, in some embodiments provided in the present application, the preform is subjected to solution treatment, quenching and aging treatment to obtain a cam bearing seat structure: the aging time is 2 to 4 hours.

[0070] Under this solution temperature, solution time, aging temperature and aging time, the cam bearing seat structure can have both a relatively soft phase that plays a lubricating role and a relatively hard phase that plays a wear-resistant role, thereby achieving different load-bearing and wear-resistant requirements for the upper cover and base of the cam bearing seat structure, so that there is no need to set a bushing between the upper cover and base of the cam bearing seat structure and the camshaft, reducing the use of bushings. The upper cover and base of the cam bearing seat structure can be processed with the same material, simplifying the process.

[0071] In combination with the second aspect, in some embodiments provided in the present application, the preform is subjected to solution treatment, quenching and aging treatment to obtain a cam bearing seat structure, and the quenching treatment method includes water quenching, wherein: the water quenching temperature is 70 to 90°C.

[0072] In combination with the second aspect, in some embodiments provided in the present application, the preform is subjected to solution treatment, quenching and aging treatment to obtain a cam bearing seat structure, and the quenching treatment method includes water quenching, wherein: the water quenching time is 8 to 15 minutes.

[0073] Water quenching can allow the cam bearing seat to obtain higher comprehensive mechanical properties. At this water quenching temperature and water quenching time, a higher cooling rate can be obtained at this water quenching and temperature to prevent the strengthening phase from precipitating from the solid solution, thereby obtaining a better strengthening effect. In the third aspect, the present application provides an engine, including the cam bearing seat structure described in the first aspect, or the cam bearing seat structure processed by the processing method of the cam bearing seat structure of the second aspect. The engine has all the beneficial effects of the cam bearing seat structure, and the present application will not repeat them one by one here.

[0074] In a fourth aspect, the present application provides a vehicle, comprising the parts of the third aspect. The vehicle has all the beneficial effects of the cam bearing seat structure, which will not be described in detail in this application.

[0075] The technical solution provided in this application is described in detail below in conjunction with embodiments.

[0076] Example 1

[0077] Embodiment 1 of the present application provides a method for processing a cam bearing seat structure, comprising the following steps:

[0078] The raw material composition of the cam bearing seat structure is: Si: 11.5%; Mg: 0.4%; Mn: 0.35%; Ti: 0.06%; Sr: 0.015%; Zr: 0.01%; the balance is Al and unavoidable impurities;

[0079] Adding raw materials into a melting furnace according to the respective components for melting to obtain an aluminum alloy melt;

[0080] The aluminum alloy melt is subjected to refining, slagging, degassing, modification and temperature reduction treatments;

[0081] The mold is preheated, and after reaching the set temperature of 170°C, a layer of graphite powder is sprayed on the mold surface by an electrostatic spraying process, and then the mold is closed, and the treated aluminum alloy melt is pushed from the bottom to the top along the riser pipe from the insulation furnace below the mold into the mold cavity by high-purity nitrogen. The particle size of the graphite powder is 800nm, and the spraying thickness is 40μm;

[0082] After the aluminum alloy melt fills the mold cavity, the central extrusion column above the gate in the mold begins to descend and closes the gate to complete the filling process. At this time, the high-purity nitrogen in the insulation furnace is depressurized, and the excess aluminum alloy melt in the riser flows back into the insulation furnace. The central extrusion column is further moved downward to extrude all the aluminum alloy melt below the shoulder of the central extrusion column into the mold cavity of the mold forming casting part, and the aluminum alloy melt is demolded after it is completely solidified. The central extrusion column includes an upper end and a lower end of the extrusion column. The diameter of the upper end of the central extrusion column is 1.8 times the diameter of the lower end, and the diameter of the lower end of the central extrusion column matches the diameter of the gate in the mold; the extrusion pressure of the central extrusion column is 60MPa;

[0083] The casting obtained after demoulding is heat treated to obtain a cam bearing seat assembly casting blank; the casting blank is solution treated at a solution temperature of 500°C and a solution time of 2h, the casting is water quenched at a water temperature of 70°C and a water quenching time of 8min, and then the casting is artificially aged at an aging temperature of 160°C and an aging time of 2h.

[0084] Example 2

[0085] Embodiment 2 of the present application provides a method for processing a cam bearing seat structure, comprising the following steps:

[0086] The raw material composition of the cam bearing seat structure is: Si: 14.5%; Mg: 0.45%; Mn: 0.50%; Ti: 0.12%; Sr: 0.025%; Zr: 0.1%; the balance is Al and unavoidable impurities;

[0087] Adding raw materials into a melting furnace according to the respective components for melting to obtain an aluminum alloy melt;

[0088] The aluminum alloy melt is subjected to refining, slagging, degassing, modification and temperature reduction treatments;

[0089] The mold is preheated, and after reaching the set temperature of 180°C, a layer of graphite powder is sprayed on the mold surface by an electrostatic spraying process, and then the mold is closed, and the treated aluminum alloy melt is pushed from the bottom to the top along the riser pipe from the insulation furnace below the mold into the mold cavity by high-purity nitrogen. The particle size of the graphite powder is 1000nm, and the spraying thickness is 50μm;

[0090] After the aluminum alloy melt fills the mold cavity, the central extrusion column above the gate in the mold begins to descend and closes the gate to complete the filling process. At this time, the high-purity nitrogen in the insulation furnace is depressurized, and the excess aluminum alloy melt in the riser flows back into the insulation furnace. The central extrusion column is further moved downward to extrude all the aluminum alloy melt below the shoulder of the central extrusion column into the mold cavity of the mold forming casting part, and the aluminum alloy melt is demolded after it is completely solidified. The central extrusion column includes an upper end and a lower end of the extrusion column. The diameter of the upper end of the central extrusion column is 2.0 times the diameter of the lower end, and the diameter of the lower end of the central extrusion column matches the diameter of the gate in the mold; the extrusion pressure of the central extrusion column is 90MPa;

[0091] The casting obtained after demoulding is heat treated to obtain a cam bearing seat assembly casting blank; the casting blank is solution treated at a solution temperature of 540°C and a solution time of 4 hours, the casting is water quenched at a water temperature of 90°C and a water quenching time of 15 minutes, and then the casting is artificially aged at an aging temperature of 180°C and an aging time of 4 hours.

[0092] Example 3

[0093] Embodiment 3 of the present application provides a method for processing a cam bearing seat structure, comprising the following steps:

[0094] The raw material composition of the cam bearing seat structure is: Si: 12.5%; Mg: 0.35%; Mn: 0.45%; Ti: 0.11%; Sr: 0.02%; Zr: 0.05%; the balance is Al and unavoidable impurities;

[0095] Adding raw materials into a melting furnace according to the respective components for melting to obtain an aluminum alloy melt;

[0096] The aluminum alloy melt is subjected to refining, slagging, degassing, modification and temperature reduction treatments;

[0097] The mold is preheated, and after reaching the set temperature of 190°C, a layer of graphite powder is sprayed on the mold surface by an electrostatic spraying process, and then the mold is closed, and the treated aluminum alloy melt is pushed from the bottom to the top along the riser pipe from the insulation furnace below the mold into the mold cavity by high-purity nitrogen. The particle size of the graphite powder is 900nm, and the spraying thickness is 45μm;

[0098] After the aluminum alloy melt fills the mold cavity, the central extrusion column above the gate in the mold begins to descend and closes the gate to complete the filling process. At this time, the high-purity nitrogen in the insulation furnace is depressurized, and the excess aluminum alloy melt in the riser flows back into the insulation furnace. The central extrusion column is further moved downward to extrude all the aluminum alloy melt below the shoulder of the central extrusion column into the mold cavity of the mold forming casting part, and the aluminum alloy melt is demolded after it is completely solidified. The central extrusion column includes an upper end and a lower end of the extrusion column. The diameter of the upper end of the central extrusion column is 1.8 times the diameter of the lower end, and the diameter of the lower end of the central extrusion column matches the diameter of the gate in the mold; the extrusion pressure of the central extrusion column is 85MPa;

[0099] The casting obtained after demoulding is heat treated to obtain a cam bearing seat assembly casting blank; the casting blank is solution treated at a solution temperature of 520°C and a solution time of 3 hours, the casting is water quenched at a water temperature of 80°C and a water quenching time of 9 minutes, and then the casting is artificially aged at an aging temperature of 175°C and an aging time of 3.5 hours.

[0100] Example 4

[0101] Embodiment 4 of the present application provides a method for processing a cam bearing seat structure, comprising the following steps:

[0102] The raw material composition of the cam bearing seat structure is: Si: 13.5%; Mg: 0.45%; Mn: 0.35%; Ti: 0.1%; Sr: 0.02%; Zr: 0.08%; the balance is Al and unavoidable impurities;

[0103] Adding raw materials into a melting furnace according to the respective components for melting to obtain an aluminum alloy melt;

[0104] The aluminum alloy melt is subjected to refining, slagging, degassing, modification and temperature reduction treatments;

[0105] The mold is preheated, and after reaching the set temperature of 190°C, a layer of graphite powder is sprayed on the mold surface by an electrostatic spraying process, and then the mold is closed, and the treated aluminum alloy melt is pushed from the bottom to the top along the riser pipe from the insulation furnace below the mold into the mold cavity by high-purity nitrogen. The particle size of the graphite powder is 900nm, and the spraying thickness is 45μm;

[0106] After the aluminum alloy melt fills the mold cavity, the central extrusion column above the gate in the mold begins to descend and closes the gate to complete the filling process. At this time, the high-purity nitrogen in the insulation furnace is depressurized, and the excess aluminum alloy melt in the riser flows back into the insulation furnace. The central extrusion column is further moved downward to extrude all the aluminum alloy melt below the shoulder of the central extrusion column into the mold cavity of the mold forming casting part, and the aluminum alloy melt is demolded after it is completely solidified. The central extrusion column includes an upper end and a lower end of the extrusion column. The diameter of the upper end of the central extrusion column is 1.8 times the diameter of the lower end, and the diameter of the lower end of the central extrusion column matches the diameter of the gate in the mold; the extrusion pressure of the central extrusion column is 85MPa;

[0107] The casting obtained after demoulding is heat treated to obtain a cam bearing seat assembly casting blank; the casting blank is solution treated at a solution temperature of 520°C and a solution time of 3 hours, the casting is water quenched at a water temperature of 80°C and a water quenching time of 9 minutes, and then the casting is artificially aged at an aging temperature of 175°C and an aging time of 3.5 hours.

[0108] Comparative Example 1

[0109] Comparative Example 1 of the present application provides a method for processing a cam bearing seat structure, which is similar to Example 1, except that Comparative Example 1 does not contain Si.

[0110] Comparative Example 2

[0111] Comparative Example 2 of the present application provides a method for processing a cam bearing seat structure, which is similar to Example 1, except that the mass fraction of Si in Comparative Example 2 is 10%.

[0112] Comparative Example 3

[0113] Comparative Example 3 of the present application provides a method for processing a cam bearing seat structure, which is similar to Example 1, except that the mass fraction of Si in Comparative Example 3 is 15%.

[0114] The cam bearing seat structure obtained by the processing method of the cam bearing seat structure of Examples 1 to 4 and Comparative Examples 1 to 3 was subjected to performance measurement, and its yield strength, elongation and wear resistance were tested, wherein the yield strength and elongation were measured using "GB / T 288 Metal Material Room Temperature Tensile Test Method". The wear resistance test was conducted using a pin-disc friction and wear tester, and the test method was as follows: ultrasonic cleaning was performed for 10 minutes before the test, and drying was performed after cleaning. The mass before wear was weighed using a high-precision electronic scale (accuracy 0.00001g), and the lubrication was checked regularly during the wear process. The lubricating oil was a fully synthetic lubricating oil SAE 5W 30. After wear, the sample was placed in an acetone solution for ultrasonic cleaning for 10 minutes, and weighed after drying. The wear mass of the sample was obtained using the mass difference before and after. The wear time was 1 hour; the load was 20N; the wear diameter was 10mm, and the rotation speed was 400r / min. The results are shown in Table 1.

[0115] Table 1 Performance of the cam bearing seat structure of Examples 1 to 4 and Comparative Examples 1 to 3

[0116] Yield strength / MPa Elongation / % Wear amount / mg Example 1 215 5.2 0.30 Example 2 223 4.4 0.12 Example 3 265 8.5 0.23 Example 4 244 6.3 0.18 Comparative Example 1 238 9.5 3.02 Comparative Example 2 220 5.6 1.35 Comparative Example 3 188 5.2 0.11

[0117] It can be seen from Table 1 that compared with Comparative Examples 1 to 3, the metallographic structure of the cam bearing seat structure in Examples 1 to 4 includes an α~Al phase and a eutectic silicon phase. The eutectic silicon phase is relatively hard, while the α~Al phase is relatively soft. The cam bearing seat structure contains both a relatively soft phase that plays a lubricating role and a relatively hard phase that plays a wear-resistant role, thereby achieving different load-bearing and wear-resistant requirements for the upper cover and base of the cam bearing seat structure. Since the silicon content is within a suitable range, the α~Al phase and the eutectic silicon phase can be in a suitable ratio, so that the wear resistance and strength of the cam bearing seat structure meet the requirements.

[0118] Since Comparative Example 1 does not contain silicon, its wear resistance does not meet the standard and there is a risk of shaft seizure.

[0119] In Comparative Example 2, since the mass fraction of Si is 10%, the strength is greater than 200 MPa, but the wear resistance is not up to standard and there is a risk of shaft seizure.

[0120] In Comparative Example 3, since the mass fraction of Si is 15%, the wear resistance is less than 1.00, and the wear resistance performance meets the standard, but the yield strength is less than 200 MPa, and the strength does not meet the standard.

[0121] In summary, by changing the raw material composition of the cam bearing seat structure, on the one hand, the weight of the cam bearing seat structure can be reduced, so that the upper cover and the base of the cam bearing seat structure can be processed with the same material, simplifying the process, and at the same time, it can simultaneously meet the different load-bearing and wear-resistant requirements of the upper cover and the base of the cam bearing seat structure, so that there is no need to set a bushing between the upper cover and the base of the cam bearing seat structure and the camshaft, reducing the use of bushings. Among them, the mass fraction of Si is within this range, and good wear resistance can be obtained, making it possible to cancel the bushing. When the mass fraction of Mg is within this range, the material can obtain the optimal yield strength and elongation through solution treatment + artificial aging. When the mass fraction of Mn is within this range, the material can obtain good anti-sticking properties, and it can also form a "Chinese character-shaped" Fe-Mn compound with Fe added to the alloy, thereby weakening the negative impact of the lattice of needle-shaped Fe relative to the matrix structure on the yield strength and elongation of the material. When the mass fraction of Ti is within this range, the structure can be refined and the grain size can reach 7-8 levels, thereby obtaining good yield strength. When the mass fraction of Sr is within this range, a good modification effect can be obtained, thereby improving the yield strength of the material. When the mass fraction of Zr is within this range, the recrystallization temperature of the alloy can be increased, thereby improving the high temperature strength of the material.

[0122] In the description of this specification, the description with reference to the terms "one embodiment / method", "some embodiments / methods", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment / method or example are included in at least one embodiment / method or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment / method or example. Moreover, the specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments / methods or examples. In addition, those skilled in the art may combine and combine the different embodiments / methods or examples described in this specification and the features of the different embodiments / methods or examples, unless they are contradictory.

[0123] It should be noted that, in the present application, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements defined by the sentence "comprise one..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements. In the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically stipulated.

[0124] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A cam bearing seat structure, characterized in that: The invention comprises a bearing base and a bearing upper cover, wherein the bearing base and the bearing upper cover form a camshaft hole for mounting a cam, and the side wall of the camshaft hole has a lubricating oil groove, wherein: Measured by mass fraction, the raw material composition of the cam bearing seat structure includes: Si: 11.5% to 14.5%; Mg: 0.35% to 0.45%; Mn: 0.35% to 0.50%; Ti: 0.06% to 0.12%; Sr: 0.015% to 0.025%; Zr: 0.01% to 0.1%; the remainder is Al and unavoidable impurities.

2. The cam bearing seat structure according to claim 1, characterized in that: The metallographic structure of the cam bearing seat structure includes α-Al phase and eutectic silicon phase.

3. The cam bearing seat structure according to claim 1, characterized in that: The mass ratio of Si to Al is (13-17):

100.

4. The cam bearing seat structure according to claim 1, characterized in that: The bearing load of the cam bearing seat structure is 0.1-100 MPa.

5. A method for processing a cam bearing seat structure according to any one of claims 1 to 4, characterized in that: The following steps are involved: Mixing and melting the raw materials according to the raw material components to obtain an aluminum alloy melt; The aluminum alloy melt is refined, deslagging, degassing, modifying and cooling to obtain a pretreated melt; Casting the pretreated solution into a mold and demoulding it to obtain a prefabricated part; The prefabricated parts are subjected to solid solution treatment, quenching and aging treatment to obtain a cam bearing seat structure.

6. The method for processing a cam bearing seat structure according to claim 5, characterized in that: The pre-treated melt is molded and demolded to obtain a preform, wherein the mold is filled with a graphite powder layer, wherein: The particle size of the graphite powder is 800 to 1000 nm; and / or, The thickness of the graphite powder layer is 40 to 50 μm.

7. The method for processing a cam bearing seat structure according to claim 5, characterized in that: The preform is subjected to solution treatment, quenching and aging treatment to obtain a cam bearing seat structure: The solution temperature is 500-540°C; and / or, The solution time is 2 to 4 hours; and / or, The aging temperature is 160-180°C; and / or The aging time is 2 to 4 hours.

8. The method for processing a cam bearing seat structure according to claim 5, characterized in that: The prefabricated part is subjected to solution treatment, quenching and aging treatment to obtain the cam bearing seat structure, wherein the quenching treatment method includes water quenching, wherein: The water quenching temperature is 70 to 90°C; and / or, The water quenching time is 8 to 15 minutes.

9. An engine, characterized in that: It comprises a cam bearing seat structure as described in any one of claims 1 to 4, or a cam bearing seat structure manufactured by the processing method of the cam bearing seat structure as described in any one of claims 5 to 8.

10. A vehicle, characterized in that Comprising the engine as claimed in claim 9.

Citation Information

Patent Citations

  • Anti-abrasion floating aluminum alloy bearing pedestal and preparation method thereof

    CN103291762A

  • Adjustable opening bearing seat assembly

    CN105221583A

  • Camshaft base assembly and bearing pedestal assembly

    CN111648834A

  • Double overhead camshaft bearing seat, manufacturing process, testing machine and testing method

    CN112065862A

  • Crankshaft bearing

    GB9022225D0