Method for preparing fabric-based flexible strain sensor based on LIG and product

By depositing and laser-induced graphene on the fabric, the problems of difficulty and shedding of LIG and fabrics in the prior art are solved, and the stable combination and high sensitivity of fabric-based flexible strain sensors are achieved, which simplifies the packaging process.

CN118913080APending Publication Date: 2024-11-08WUHAN TEXTILE UNIV +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411020234.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Prior Art When preparing fabric-based flexible strain sensors, laser-induced graphene (LIG) is difficult to compound with the fabric, easily fall off, damages the performance of the fabric, and is complicated to package.

Method used

Polyamic acid analogs are prepared by adding 4,4'-diaminodiphenyl ether and bisphenol A-type diether dianhydride to m-cresol, and imidized to form a white filamentous solid, followed by Deposition on the fabric and LIG is generated by laser induced, and conductive copper paste and polydimethicone encapsulation is performed.

Benefits of technology

The stable combination of LIG and fabric is achieved, avoiding shedding, simplifying packaging steps, retaining LIG's 3D structure, improving the conductivity and sensitivity of the sensor, and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118913080A_ABST
    Figure CN118913080A_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing a fabric-based flexible strain sensor based on LIG. The preparation method comprises the following steps: preparing a pale yellow and viscous polyamide acid analogue from 4, 4 '-diaminodiphenyl ether and bisphenol A type diether dianhydride, adding an accelerator into the polyamide acid analogue under the protection of nitrogen, heating, preserving heat, cooling to room temperature, washing with ethanol and deionized water to obtain a white and filamentous polyimide analogue, adding the polyimide analogue into N, N'-diaminodiphenyl ether and bisphenol A type diether dianhydride at normal temperature, and reacting at room temperature to obtain the polyimide analogue. The preparation method comprises the following steps: dissolving graphene in N, N-dimethylacetamide to obtain a mixed solution, contacting the mixed solution with one side of a fabric, standing at normal temperature until a membranoid substance is deposited on the bottom surface of the fabric, performing laser induction on the membranoid substance by using laser to generate laser-induced graphene, and packaging to obtain a product. According to the design, films can be smoothly formed inside and outside the fabric at normal temperature so as to enhance the binding force, the damage to the fabric caused by laser induction can be avoided, and the performance of the fabric is favorably exerted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a fabric-based flexible strain sensor, belonging to the field of smart wearables, and in particular to a method and product for preparing a fabric-based flexible strain sensor based on LIG. Background Art

[0002] With the continuous advancement of science and technology, the development of smart wearable devices is very rapid. Smart wearable devices refer to the general term for smart devices that can be worn on the body or worn on the body. Sensing technology and wireless communication technology are embedded in wearable devices to realize data collection, storage and computing functions, and enhance human-computer interaction. As the largest type of human wearables, fabrics are undoubtedly the most important in smart wearables, which also puts forward better application requirements for fabrics, such as building flexible strain sensors on fabrics to monitor various movements of the human body, especially micro-movements. At this time, fabric-based strain sensors come into being.

[0003] At present, there are two main methods for preparing fabric-based strain sensors by laser induction:

[0004] (1) Sodium carboxymethyl cellulose is impregnated on the fabric in the hope of reducing the resistance of laser-induced graphene (LIG) and preventing the fabric from burning. However, the LIG prepared by this method is directly induced on the fabric, which will damage the basic properties of the fabric, and there are many subsequent packaging operations;

[0005] (2) First, laser induction is used on a commercial polyimide (PI) film to generate LIG, and then the LIG is transferred to the fabric by heat pressing to prepare a fabric-based flexible strain sensor. However, the LIG produced by this method is difficult to be composited with the fabric and is easy to fall off, which cannot bring out the performance advantages of the fabric.

[0006] The information disclosed in this background technology section is only intended to increase the understanding of the overall background of the application, and should not be regarded as acknowledging or suggesting in any form that the information constitutes the prior art already known to ordinary technicians in this field. Summary of the invention

[0007] The purpose of the present invention is to overcome the defects and problems existing in the prior art that impair the performance of fabrics, and to provide a method and product for preparing a fabric-based flexible strain sensor based on LIG that is beneficial to the performance of fabrics.

[0008] To achieve the above objectives, the technical solution of the present invention is: a method for preparing a fabric-based flexible strain sensor based on LIG, the method comprising the following steps:

[0009] The first step: first add 4,4'-diaminodiphenyl ether to m-cresol, and then stir until the 4,4'-diaminodiphenyl ether is completely dissolved, then add bisphenol A type diether dianhydride in batches, and continue to stir until a light yellow, viscous mixture is obtained, which is a polyamic acid analogue;

[0010] Step 2: first, under nitrogen protection, add a catalyst to the above polyamic acid analog, the catalyst being any one of triethanolamine, triethylamine, 3-methylpyridine, pyridine or isoquinoline, then gradually raise the temperature to 180-250°C, then keep the temperature until the imidization degree reaches the highest, then end the heat preservation, then cool to room temperature, and then wash with ethanol and deionized water to obtain a white filamentous solid, which is a polyimide analog;

[0011] Step 3: First, at room temperature, add the above polyimide analog to N, N-dimethylacetamide to dissolve it to obtain a mixed solution, then pour the mixed solution into an open container, with the liquid level line aligned with or close to the opening of the container, then cover the opening of the container with a layer of fabric, the bottom surface of the fabric is in contact with the mixed solution, and then wait at room temperature until a film is deposited on the bottom surface of the fabric, and then take away the fabric with the film;

[0012] Step 4: first lay the fabric with the film flat with the film side facing upwards, and then use a laser to induce the membrane on the fabric with the film to generate laser induced graphene. The area where the laser induced graphene is located is the sensing area. Then stop the laser induction and package the sensing area to obtain the product, which is the fabric-based flexible strain sensor.

[0013] In the fourth step, packaging the sensing area means: firstly applying conductive copper paste on both ends of the sensing area, then gluing a conductive part on the conductive copper paste, and then coating polydimethylsiloxane above the sensing area and above the conductive copper paste and the conductive part to which it is bonded for packaging.

[0014] In the first step, the amount ratio of m-cresol, 4,4'-diaminodiphenyl ether, and bisphenol A type diether dianhydride is: 10-50 ml: 1-5 mmol: 1-5 mmol;

[0015] In the second step, the accelerator is 0.01%-0.05% of the volume of m-cresol.

[0016] In the second step, the chemical structural formula of the polyimide analog is as follows:

[0017]

[0018] In the second step, the insulation time is 12 hours.

[0019] In the second step, washing with ethanol and deionized water refers to:

[0020] First, add ethanol to the mixture cooled to room temperature, and stir until white filaments appear, then pour out the supernatant, then add ethanol to the remaining mixture, and stir, and pour out the supernatant, then add ethanol to the remaining mixture, and stir, and then pour out the supernatant, then add deionized water to the remaining mixture, and stir, and pour out the supernatant, then add deionized water to the remaining mixture, and stir, and then pour out the supernatant, then add deionized water to the remaining mixture, and stir, and then pour out the supernatant, then add deionized water to the remaining mixture, and stir, and then pour out the supernatant.

[0021] In the third step, the mass percentage concentration of the polyimide analog in the mixed solution is 5%-7.5%.

[0022] In the third step, the standing time is 45 min-60 min.

[0023] In the fourth step, the power of the laser is 20%*30W-60%*30W, and the scanning speed of the laser is 200-2000mm / s.

[0024] A fabric-based flexible strain sensor is a product of the above-mentioned method for preparing a fabric-based flexible strain sensor based on LIG.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1. In a method and product for preparing a fabric-based flexible strain sensor based on LIG of the present invention, a light yellow, viscous mixture, i.e., a polyamic acid analogue, is first prepared, and a catalyzer is added to the polyamic acid analogue for mixing, and then the temperature is increased and kept warm until the imidization degree reaches the highest, and then the heat preservation is terminated, and then the mixture is cooled to room temperature, and then washed with ethanol and deionized water to obtain a white filamentous solid, i.e., a polyimide analogue, and then the polyimide analogue is added to N, N-dimethylacetamide at room temperature for dissolution to obtain a mixed solution, and then the mixed solution is poured into an open container, and the liquid level line is aligned with or close to the opening of the container, and then a layer of fabric is covered on the opening of the container, and the bottom surface of the fabric is in contact with the mixed solution, and then it is left to stand at room temperature until a film is deposited on the bottom surface of the fabric, and then the fabric with the film is taken away, and then the fabric with the film is laid flat, with the film side facing up, and then the film on the fabric with the film is laser-induced by laser to generate laser-induced graphene. The advantages of this design include:

[0027] First point: when the fabric comes into contact with the mixed liquid (polyimide analogue, N, N-dimethylacetamide), under the action of capillary phenomenon, the mixed liquid directly penetrates into the interior of the fabric and comes into contact with each fabric fiber. Subsequently, when the mixed liquid forms a film, the outside of each fiber is wrapped with the film until it extends to the outside of the fabric and becomes a membrane-like object. At this time, the fabric is wrapped in the inside of the film from the inside to the outside, which not only has a strong bonding force, but also will not fall off after laser induction of graphene. Moreover, when the film is laser-induced, the membrane-like object and the film wrapped on the fabric fiber will protect the fabric, preventing the laser from acting directly on the fiber and preventing the high temperature generated by the laser from carbonizing the fiber, thereby damaging the basic performance of the fabric. In addition, the thermal conductivity of the film is also poor, and the high temperature of the laser will not be transmitted to the fiber.

[0028] Second point: Under the action of capillary absorption, the fabric will absorb a large amount of mixed liquid, thereby constructing a thicker membrane with a thickness greater than or equal to 200 microns, while the action depth of laser-induced graphene is 50-100 microns (starting from the surface of the membrane, the induction depth is 50-100 microns downward), and it is difficult to directly contact the fiber, further avoiding the risk of carbonization of the fiber. In addition, absorbing a large amount of mixed liquid can also increase the overall weight of the fabric, so that it tends to the inside of the vessel under the action of gravity to ensure that it is always in contact with the mixed liquid and ensure the smooth formation of the membrane;

[0029] Third point: The present invention specifically prepares a polyimide analogue that can be dissolved in N,N-dimethylacetamide at room temperature, which not only reduces the difficulty of subsequent film formation, but also saves the cost of obtaining a mixed solution and reduces the implementation conditions;

[0030] Fourth point: The present invention first specially prepares a polyamic acid analogue, and then uses it in cooperation with a catalyst to achieve the highest degree of imidization at a relatively low temperature. At the same time, the imidization degree increase and subsequent film formation can be separated into two separate steps to avoid damaging the properties of the fabric.

[0031] Therefore, the present invention can not only independently prepare polyamic acid analogs and polyimide analogs, but also can smoothly form films on the inside and outside of fabrics at room temperature, while enhancing the bonding strength, it can also avoid laser-induced damage to the fabric, which is beneficial to the performance of the fabric.

[0032] 2. In the method and product of preparing a fabric-based flexible strain sensor based on LIG of the present invention, currently, the more common polyimide products on the market are insoluble in common solvents, such as water, alcohol, dimethyl sulfoxide, etc. Even when dissolved in solutions such as DMF and DMAc, they need to be heated and stirred for more than 5 hours under high temperature conditions. Moreover, even if dissolved, they cannot be deposited on the fabric at room temperature during subsequent film formation, which limits the use of polyimide products to a certain extent. For this reason, the present invention specially prepares a white, filamentous polyimide analogue, which is It is soluble, and after obtaining the mixed solution, it can be deposited on the fabric to form a film at room temperature, which can not only reduce the difficulty of compounding with the fabric, but also avoid the damage to the fabric caused by forced compounding in the prior art, and it can also have strong flexibility after film formation, and is very suitable for making flexible strain sensors. In addition, in terms of the production process, the present invention not only has fewer steps and is easy to operate, but also has lower production conditions, and the temperature only needs to be around 200°C; therefore, the present invention can not only innovatively produce a polyimide analogue that can be deposited on the fabric to form a film at room temperature, but is also easy to operate, and the film has good flexibility after film formation.

[0033] 3. In the method and product for preparing a fabric-based flexible strain sensor based on LIG of the present invention, in order to prepare a polyimide analog that meets the requirements, the present invention not only limits the cooperation of the polyamic acid analog and the promoter to achieve the highest degree of imidization under relatively low temperature conditions (the promoter can promote the imidization process of the polyamic acid analog under low temperature conditions) and eliminates the obstacles to subsequent combination with the fabric, but also limits the use of m-cresol, 4,4'-diaminodiphenyl ether, and bisphenol A type diether dianhydride as raw materials to meet the cooperation requirements (polyamic acid analog is a soluble prepolymer required for preparing polyimide analog), and limits the order of addition and mixing to produce a polyamic acid analog that meets the cooperation requirements; therefore, the present invention can not only produce a polyimide analog that is soluble at room temperature and can be deposited on the fabric to form a film at room temperature, but also has low operation difficulty and low realization requirements.

[0034] 4. In a method and product for preparing a fabric-based flexible strain sensor based on LIG of the present invention, during laser induction, the laser power is preferably 20%*30W-60%*30W, which can ensure the performance of laser-induced graphene (LIG) without damaging the fabric and damaging the basic properties of the fabric. In addition, the present invention also preferably sets the laser scanning speed to 200-2000mm / s, which can ensure the normal progress of laser-induced graphene and avoid too long scanning time and too low laser duty cycle, thereby ablating the fabric. Therefore, the present invention can not only smoothly realize laser-induced graphene on the fabric, but also avoid damage to the basic properties of the fabric.

[0035] 5. In a method and product for preparing a fabric-based flexible strain sensor based on LIG of the present invention, when encapsulating the sensing area, it is preferred to first apply a conductive copper paste to both ends of the sensing area, then adhere a conductive part to the conductive copper paste, and then apply polydimethylsiloxane above the sensing area and above the portion of the conductive copper paste and the conductive part to which it is adhered for encapsulation. This design avoids the hot pressing packaging commonly used in the prior art, which not only saves costs, but also retains the 3D structure of LIG to the greatest extent, improves the conductivity and sensitivity of the sensor, and preferably has a surface resistance of 30-40Ω / sq. In addition, the encapsulation step is greatly simplified, and it can be prepared in only one step without the need for complex operations such as transfer printing; therefore, the present invention is not only easy to encapsulate, but also has a high sensitivity of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 It is a production flow chart of the present invention.

[0037] Figure 2 It is a packaging flow chart of the present invention.

[0038] Figure 3 It is a schematic diagram of the changes in the deposition of the film on the fabric according to the present invention.

[0039] Figure 4 It is a structural diagram of the equipment for testing the performance of the fabric-based flexible strain sensor in the present invention.

[0040] Figure 5 yes Figure 4 Schematic diagram of the test results (positive bending).

[0041] Figure 6 yes Figure 4 Schematic diagram of the test results (reverse bending). DETAILED DESCRIPTION

[0042] The present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0043] See also Figure 1 — Figure 6 , a method for preparing a fabric-based flexible strain sensor based on LIG, the method comprising the following steps:

[0044] The first step: first add 4,4'-diaminodiphenyl ether to m-cresol, and then stir until the 4,4'-diaminodiphenyl ether is completely dissolved, then add bisphenol A type diether dianhydride in batches, and continue to stir until a light yellow, viscous mixture is obtained, which is a polyamic acid analogue;

[0045] Step 2: first, under nitrogen protection, add a catalyst to the above polyamic acid analog, the catalyst being any one of triethanolamine, triethylamine, 3-methylpyridine, pyridine or isoquinoline, then gradually raise the temperature to 180-250°C, then keep the temperature until the imidization degree reaches the highest, then end the heat preservation, then cool to room temperature, and then wash with ethanol and deionized water to obtain a white filamentous solid, which is a polyimide analog;

[0046] Step 3: First, at room temperature, add the above polyimide analog to N, N-dimethylacetamide to dissolve it to obtain a mixed solution, then pour the mixed solution into an open container, with the liquid level line aligned with or close to the opening of the container, then cover the opening of the container with a layer of fabric, the bottom surface of the fabric is in contact with the mixed solution, and then wait at room temperature until a film is deposited on the bottom surface of the fabric, and then take away the fabric with the film;

[0047] Step 4: first lay the fabric with the film flat with the film side facing upwards, and then use a laser to induce the membrane on the fabric with the film to generate laser induced graphene. The area where the laser induced graphene is located is the sensing area. Then stop the laser induction and package the sensing area to obtain the product, which is the fabric-based flexible strain sensor.

[0048] In the fourth step, packaging the sensing area means: firstly applying conductive copper paste on both ends of the sensing area, then gluing a conductive part on the conductive copper paste, and then coating polydimethylsiloxane above the sensing area and above the conductive copper paste and the conductive part to which it is bonded for packaging.

[0049] In the first step, the amount ratio of m-cresol, 4,4'-diaminodiphenyl ether, and bisphenol A type diether dianhydride is: 10-50 ml: 1-5 mmol: 1-5 mmol;

[0050] In the second step, the accelerator is 0.01%-0.05% of the volume of m-cresol.

[0051] In the second step, the chemical structural formula of the polyimide analog is as follows:

[0052]

[0053] In the second step, the insulation time is 12 hours.

[0054] In the second step, washing with ethanol and deionized water refers to:

[0055] First, add ethanol to the mixture cooled to room temperature, and stir until white filaments appear, then pour out the supernatant, then add ethanol to the remaining mixture, and stir, and pour out the supernatant, then add ethanol to the remaining mixture, and stir, and then pour out the supernatant, then add deionized water to the remaining mixture, and stir, and pour out the supernatant, then add deionized water to the remaining mixture, and stir, and then pour out the supernatant, then add deionized water to the remaining mixture, and stir, and then pour out the supernatant, then add deionized water to the remaining mixture, and stir, and then pour out the supernatant.

[0056] In the third step, the mass percentage concentration of the polyimide analog in the mixed solution is 5%-7.5%.

[0057] In the third step, the standing time is 45 min-60 min.

[0058] In the fourth step, the power of the laser is 20%*30W-60%*30W, and the scanning speed of the laser is 200-2000mm / s.

[0059] A fabric-based flexible strain sensor is a product of the above-mentioned method for preparing a fabric-based flexible strain sensor based on LIG.

[0060] The supplementary technical features of the present invention are as follows:

[0061] The molecular formula of 4,4'-diaminodiphenyl ether in the present invention is C12H12N2O.

[0062] The molecular formula of the bisphenol A diether dianhydride in the present invention is C31H20O8.

[0063] The type of fiber in the fabric of the present invention is preferably cotton fiber or hemp fiber.

[0064] The reason why the insulation time is limited to 12 hours in the present invention is that the time is determined according to the degree of imidization of the generated polyimide analog. In practice, after every two hours of insulation, part of the solution needs to be taken to characterize its performance, and its degree of imidization is explored by Raman, XPS, etc. It is finally found that the degree of imidization is the highest under 12 hours of insulation.

[0065] The reason why the present invention adds a accelerator to the polyamic acid analog to react under nitrogen protection is that the purpose of nitrogen protection is to prevent the polyamic acid analog from hydrolyzing during the heating process, to eliminate interfering gases during the heating process, and to maintain the purity of the experimental environment to ensure the accuracy of the experimental results.

[0066] The reason why the mass percentage concentration of the polyimide analog in the mixed solution is limited to 5%-7.5% in the present invention is that if it is greater than 7.5%, not only the stirring time is too long, but also it is difficult to completely dissolve; if it is less than 5%, the solid content in the solution is too low and the film formation is discontinuous.

[0067] The reason why the laser power is limited to 20%*30W-60%*30W in the present invention is that laser induction requires a certain laser energy. When the power is lower than 20%, the energy is insufficient and graphene cannot be formed on the film surface, and only wrinkles are formed on the film. When the power is greater than 60%, the energy is too high and the laser will penetrate the film, which is likely to burn the fabric. In addition, the formed graphene will be over-oxidized to generate impurities such as graphene oxide or CO2, which will affect the conductivity of the final product.

[0068] The conductive member in the present invention is preferably a copper foil tape.

[0069] In the present invention, under nitrogen protection, during the heating and heat preservation process after adding the accelerator, stirring is preferably performed simultaneously until the imidization degree reaches the highest. If stirring is not performed, the imidization degree of the polyamic acid analogue will be lowered, polyimide may not be generated, and there will be obvious hydrolysis during the washing process.

[0070] Embodiment 1:

[0071] See also Figure 1 — Figure 2 , a method for preparing a fabric-based flexible strain sensor based on LIG, the method comprising the following steps:

[0072] The first step: first add 4,4'-diaminodiphenyl ether to m-cresol, and then stir until the 4,4'-diaminodiphenyl ether is completely dissolved, then add bisphenol A type diether dianhydride in batches, and continue to stir until a light yellow, viscous mixture is obtained, which is a polyamic acid analogue;

[0073] Step 2: first, under nitrogen protection, add a catalyst to the above polyamic acid analog, the catalyst being any one of triethanolamine, triethylamine, 3-methylpyridine, pyridine or isoquinoline, then gradually raise the temperature to 180-250°C, then keep the temperature until the imidization degree reaches the highest, then end the heat preservation, then cool to room temperature, and then wash with ethanol and deionized water to obtain a white filamentous solid, which is a polyimide analog;

[0074] Step 3: First, at room temperature, add the above polyimide analog to N, N-dimethylacetamide to dissolve it to obtain a mixed solution, then pour the mixed solution into an open container, with the liquid level line aligned with or close to the opening of the container, then cover the opening of the container with a layer of fabric, the bottom surface of the fabric is in contact with the mixed solution, and then wait at room temperature until a film is deposited on the bottom surface of the fabric, and then take away the fabric with the film;

[0075] Step 4: first lay the fabric with the film flat with the film side facing upwards, and then use a laser to induce the membrane on the fabric with the film to generate laser induced graphene. The area where the laser induced graphene is located is the sensing area. Then stop the laser induction and package the sensing area to obtain the product, which is the fabric-based flexible strain sensor.

[0076] A fabric-based flexible strain sensor is a product of the above-mentioned method for preparing a fabric-based flexible strain sensor based on LIG.

[0077] like Figure 4 As shown, the two ends of the above-mentioned product are clamped in the testing instrument. At the same time, the two ends of the product are connected to the circuit through the conductive parts. As the instrument rises or falls, the flexible strain sensor will bend forward or reverse accordingly (the sensing area convex outward is a positive bend, and the sensing area concave inward is a reverse bend).

[0078] Depend on Figure 5 As shown in the figure, when the sensor is bent in the positive direction, the resistance first decreases slightly and then remains stable. From the enlarged view of the strain curve, it can be seen that the sensor has good repeatability.

[0079] Depend on Figure 6 As shown in the figure, the stability of reverse bending is worse than that of forward bending, and there is no obvious pattern to follow, but it gradually stabilizes after 300s.

[0080] Embodiment 2:

[0081] The basic content is the same as that of Example 1, except that:

[0082] See also Figure 3 In the fourth step, the packaging of the sensing area refers to: first applying conductive copper paste on both ends of the sensing area, then gluing a conductive part on the conductive copper paste, and then coating polydimethylsiloxane above the sensing area and above the conductive copper paste and the conductive part to which it is bonded for packaging.

[0083] Embodiment 3:

[0084] The basic content is the same as that of Example 1, except that:

[0085] In the first step, the amount ratio of m-cresol, 4,4'-diaminodiphenyl ether, and bisphenol A type diether dianhydride is: 10-50 ml: 1-5 mmol: 1-5 mmol;

[0086] In the second step, the accelerator is 0.01%-0.05% of the volume of m-cresol.

[0087] Embodiment 4:

[0088] The basic content is the same as that of Example 3, except that:

[0089] In the first step, m-cresol is 20 mL, 4,4'-diaminodiphenyl ether is 3.19 mmol, and bisphenol A diether dianhydride is added in batches within 2 hours, with a total amount of 3.19 mmol;

[0090] In the second step, the accelerator is isoquinoline, the dosage is 0.798 mL, the insulation temperature is 200°C, and the insulation time is 12 hours;

[0091] In the fourth step, the power of the laser is 30%*30W, the scanning speed is 1000mm / s, and the surface resistance of the laser-induced graphene finally obtained is 30-40Ω / sq.

[0092] The above description is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiment. Any equivalent modifications or changes made by ordinary technicians in this field based on the contents disclosed by the present invention should be included in the protection scope recorded in the claims.

Claims

1. A method for preparing a fabric-based flexible strain sensor based on LIG, characterized in that: The method comprises the following steps: The first step: first add 4,4'-diaminodiphenyl ether to m-cresol, and then stir until the 4,4'-diaminodiphenyl ether is completely dissolved, then add bisphenol A type diether dianhydride in batches, and continue to stir until a light yellow, viscous mixture is obtained, which is a polyamic acid analogue; Step 2: first, under nitrogen protection, add a catalyst to the above polyamic acid analog, the catalyst being any one of triethanolamine, triethylamine, 3-methylpyridine, pyridine or isoquinoline, then gradually raise the temperature to 180-250°C, then keep the temperature until the imidization degree reaches the highest, then end the heat preservation, then cool to room temperature, and then wash with ethanol and deionized water to obtain a white filamentous solid, which is a polyimide analog; Step 3: First, at room temperature, add the above polyimide analog to N, N-dimethylacetamide to dissolve it to obtain a mixed solution, then pour the mixed solution into an open container, with the liquid level line aligned with or close to the opening of the container, then cover the opening of the container with a layer of fabric, the bottom surface of the fabric is in contact with the mixed solution, and then wait at room temperature until a film is deposited on the bottom surface of the fabric, and then take away the fabric with the film; Step 4: first lay the fabric with the film flat with the film side facing upwards, and then use a laser to induce the membrane on the fabric with the film to generate laser induced graphene. The area where the laser induced graphene is located is the sensing area. Then stop the laser induction and package the sensing area to obtain the product, which is the fabric-based flexible strain sensor.

2. The method for preparing a fabric-based flexible strain sensor based on LIG according to claim 1, characterized in that: In the fourth step, packaging the sensing area means: firstly applying conductive copper paste on both ends of the sensing area, then gluing a conductive part on the conductive copper paste, and then coating polydimethylsiloxane above the sensing area and above the conductive copper paste and the conductive part to which it is bonded for packaging.

3. The method for preparing a fabric-based flexible strain sensor based on LIG according to claim 1 or 2, characterized in that: In the first step, the amount ratio of m-cresol, 4,4'-diaminodiphenyl ether, and bisphenol A type diether dianhydride is: 10-50 ml: 1-5 mmol: 1-5 mmol; In the second step, the accelerator is 0.01%-0.05% of the volume of m-cresol.

4. The method for preparing a fabric-based flexible strain sensor based on LIG according to claim 1 or 2, characterized in that: In the second step, the chemical structural formula of the polyimide analog is as follows:

5. The method for preparing a fabric-based flexible strain sensor based on LIG according to claim 1 or 2, characterized in that: In the second step, the insulation time is 12 hours.

6. The method for preparing a fabric-based flexible strain sensor based on LIG according to claim 1 or 2, characterized in that: In the second step, washing with ethanol and deionized water refers to: First, add ethanol to the mixture cooled to room temperature, and stir until white filaments appear, then pour out the supernatant, then add ethanol to the remaining mixture, and stir, and pour out the supernatant, then add ethanol to the remaining mixture, and stir, and then pour out the supernatant, then add deionized water to the remaining mixture, and stir, and pour out the supernatant, then add deionized water to the remaining mixture, and stir, and then pour out the supernatant, then add deionized water to the remaining mixture, and stir, and then pour out the supernatant, then add deionized water to the remaining mixture, and stir, and then pour out the supernatant.

7. The method for preparing a fabric-based flexible strain sensor based on LIG according to claim 1 or 2, characterized in that: In the third step, the mass percentage concentration of the polyimide analog in the mixed solution is 5%-7.5%.

8. The method for preparing a fabric-based flexible strain sensor based on LIG according to claim 1 or 2, characterized in that: In the third step, the standing time is 45 min-60 min.

9. The method for preparing a fabric-based flexible strain sensor based on LIG according to claim 1 or 2, characterized in that: In the fourth step, the power of the laser is 20%*30W-60%*30W, and the scanning speed of the laser is 200-2000mm / s.

10. A fabric-based flexible strain sensor, characterized in that: The fabric-based flexible strain sensor is a product of the method for preparing a fabric-based flexible strain sensor based on LIG as described in claim 1 or 2.

Citation Information

Cited By

  • Preparation method of conformal bonding interface enhanced laser-induced patterned graphene functional layer

    CN121922434A

  • Method for preparing a laser-induced patterned graphene functional layer with conformal adhesion interface