Negative temperature coefficient thermistor temperature sensor and manufacturing method and application thereof
By performing 1/3 thickness pre-cut and multiple magnetron sputtering processes on a single crystal silicon substrate, Mn-Co-Ni-Cu-O thermal film was prepared, combined with silver glue to bond the platinum wire electrode, the existing solution was solved In the technology, the complex preparation of thermal films and large resistance problems have been achieved, and the efficient and simple production of thermistor temperature sensors has been achieved, meeting the application needs of integrated circuits and other fields.
Patent Information
- Application Number
- CN202410969622.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-18
AI Technical Summary
The application of existing negative temperature coefficient thermal-sensitive films in integrated circuits and other fields is limited by problems such as complex preparation process, large resistance, large in-plane residual stress, easy oxidation and easy breakage of electrodes, and cannot meet smaller sizes and higher measurements. Requirements for accuracy and less measurement uncertainty.
Using Mn-Co-Ni-Cu-O thermosensitive film, a thermal film with a thickness of more than 7.7μm was prepared by pre-cutting 1/3 of the thickness and multiple magnetron sputtering processes on a single crystal silicon substrate, and combined with silver glue. Bond the platinum wire electrodes to simplify the process and reduce resistance.
It realizes efficient preparation of thermal films, with resistance less than 500Ω, good surface, good binding force, avoid cracking and falling off, improves production efficiency and yield, and meets application needs in fields such as integrated circuits.
Smart Images

Figure CN118913470A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the detection field, and in particular to a negative temperature coefficient thermistor temperature sensor and a manufacturing method and application thereof. Background Art
[0002] Negative temperature coefficient (NTC) thermistor temperature sensors have the advantages of high temperature measurement accuracy, high sensitivity, good stability, low price, and long service life. They are widely and importantly used in aerospace, marine environment, and household appliances. However, as integrated circuit process becomes smaller and smaller, and the wafer multi-parameter and multi-module integration level becomes higher and higher, NTC thermistors are required to have smaller size, higher measurement accuracy, and smaller uncertainty.
[0003] Currently, there are many types of block, thin film, and spherical thermistor temperature sensors on the market, but they have problems such as large size, complex manufacturing process, large performance differences between product batches, and measurement precision and accuracy that need to be further improved. They cannot meet the requirements of integrated circuits, advanced manufacturing, micro-nano processing and other fields for smaller size, higher measurement accuracy and smaller measurement uncertainty of temperature sensors.
[0004] Compared with bulk, thin film and spherical thermistor temperature sensors, negative temperature coefficient thermistor films are most likely to meet the application requirements of integrated circuits, advanced manufacturing, and micro-nano devices. At present, some research teams have successfully prepared negative temperature coefficient thermistor films by magnetron sputtering, molecular beam epitaxy, pump laser deposition or chemical solution deposition. Among them, magnetron sputtering to prepare thermistor films is the main existing method. Its technical route is: first, magnetron sputtering growth is used on a single crystal silicon wafer with a silicon dioxide layer to prepare thermistor films. The thickness of the prepared thermistor films is usually tens to hundreds of nanometers, because the brittle thermosensitive films are grown on (4-8) inch single crystal silicon wafers, and the film thickness generally cannot exceed 1μm. If the thickness of the brittle thermosensitive film exceeds 1μm, its in-plane residual stress is very large, which will cause the film to crack or fall off from the substrate.
[0005] However, if the thickness of the thermistor film is too small (tens to hundreds of nanometers), its resistance is very large, usually (100-1000) kΩ. If the resistance is too large, the temperature measurement accuracy and resolution of the thermistor film will be very poor. Therefore, in order to reduce the resistance of the thermistor film, the prepared thermistor film must be subjected to multiple annealing heat treatments. The annealing heat treatment can reduce the resistance of the thermistor film and release the residual stress in the surface of the thermistor film. After the annealing heat treatment, electrodes are prepared on the surface of the thermistor film using evaporation coating or other techniques. After preparing the electrodes, a laser cutting machine is used to cut the wafer through its full thickness to obtain separate individual thermistors. Because there are many thermistors on a large wafer, they must be cut and separated before they can be actually used.
[0006] The existing magnetron sputtering technology route for preparing thermosensitive films has the following problems: 1) The prepared thermosensitive film needs to be subjected to multiple annealing heat treatments to reduce resistance and in-plane residual stress, which makes the technology route lengthy and complicated to operate; 2) The thermosensitive film is easily oxidized during multiple annealing heat treatments, resulting in changes in the chemical composition of the thermosensitive film; 3) The use of evaporation coating or other technologies to prepare electrodes increases the complexity and operability of the technology route, and the electrodes prepared by these technologies are prone to disconnection and failure; 4) Finally, the thermosensitive devices on the wafer are cut and separated, which is easy to contaminate and damage the thermosensitive devices, reducing the yield rate. These problems hinder the development and application of negative temperature coefficient thermistor temperature sensors in fields such as integrated circuits. Summary of the invention
[0007] Purpose of the Invention
[0008] In order to overcome the above-mentioned shortcomings, the object of the present invention is to provide a simple and efficient negative temperature coefficient thermistor temperature sensor with very high production efficiency and yield rate, and a manufacturing method and application thereof.
[0009] Solution
[0010] To achieve the purpose of the present invention, the technical solution adopted by the present invention is as follows:
[0011] In a first aspect, the present invention provides a negative temperature coefficient thermistor temperature sensor, comprising a single crystal silicon substrate block and a negative temperature coefficient thermistor film grown on a silicon dioxide layer of the single crystal silicon substrate block, wherein the negative temperature coefficient thermistor film is a Mn-Co-Ni-Cu-O thermistor film having a spinel structure; in the negative temperature coefficient thermistor film, the mass ratio of Mn, Co, Ni, Cu, and O is (28-32): (28-32): (14-16): (0.1-2.5): (20-28).
[0012] Furthermore, platinum wires are bonded to both sides of the negative temperature coefficient thermistor film, and optionally, silver glue is used for bonding.
[0013] Furthermore, the thickness of the negative temperature coefficient thermistor film is ≥7 μm, optionally ≥7.5 μm, optionally ≥7.7 μm.
[0014] Furthermore, the resistance of the negative temperature coefficient thermistor film is less than 700Ω, and optionally less than 500Ω.
[0015] Furthermore, the size of the negative temperature coefficient thermistor film is (2-10) mm×(2-10) mm, and optionally 5 mm×5 mm.
[0016] Furthermore, the negative temperature coefficient thermistor film is formed by multiple depositions using a Mn-Co-Ni-Cu-O alloy target by a physical deposition coating method; optionally, the physical deposition coating method includes magnetron sputtering, laser molecular beam epitaxy or electron beam evaporation; optionally, the deposition times are at least twice.
[0017] Furthermore, in the negative temperature coefficient thermistor film, the mass ratio of Mn, Co, Ni, Cu and O is (28-30): (28-30): (15-15.5): (0.5-2): (23-28), and optionally 30: 30: (15-15.5): (0.5-2): (23-24).
[0018] Furthermore, the structure of the spinel unit cell is AB2O4, wherein the A ions occupy the oxygen tetrahedral voids formed by four oxygen atoms, and the B ions occupy the oxygen octahedral voids formed by six oxygen atoms.
[0019] In the second aspect, a single crystal silicon substrate is provided for preparing the negative temperature coefficient thermistor temperature sensor described in the first aspect, wherein the single crystal silicon substrate is cut with longitudinal and transverse interlaced grooves to form a plurality of small units, which are used to be divided into a plurality of single crystal silicon substrate blocks along the grooves.
[0020] Further, the groove depth on the single crystal silicon substrate is 160 μm to 320 μm; optionally, the groove depth is 1 / 4 to 1 / 2 of the thickness of the single crystal silicon substrate, and optionally 1 / 3;
[0021] Furthermore, the plurality of small units are a plurality of square units, and optionally the size of the square units is (2-10) mm×(2-10) mm, and optionally 5 mm×5 mm.
[0022] In a third aspect, a method for manufacturing a negative temperature coefficient thermistor film is provided, comprising the following steps:
[0023] 1) Pre-treat the Mn-Co-Ni-Cu-O alloy target to remove the surface oxide layer and pollutants;
[0024] 2) pre-treating the single crystal silicon substrate described in the second aspect to remove surface impurities and contaminants;
[0025] 3) Physical deposition coating is performed on the single crystal silicon substrate pretreated in step 2) by using the Mn-Co-Ni-Cu-O alloy target pretreated in step 1), at least twice, to obtain a negative temperature coefficient thermistor film.
[0026] Further, in step 3), the method of physical deposition coating includes: when starting coating, performing a first sputtering coating in an inert atmosphere, then cooling, performing a second sputtering coating, and cooling; and so on, obtaining a negative temperature coefficient thermistor film by at least two sputtering coatings.
[0027] Furthermore, the time of the first sputtering coating is (150-250) minutes, and optionally 200 minutes.
[0028] Furthermore, the second sputtering coating time is (250-350) min, optionally 300 min.
[0029] Furthermore, the power of the sputtering coating is (200-260)W, optionally 240W.
[0030] Furthermore, the inert atmosphere is argon or helium.
[0031] Furthermore, the flow rate of the inert atmosphere is (48-52) sccm, optionally 50 sccm.
[0032] Furthermore, the sputtering vacuum degree is (10 -7 ~10 -8 )Torr, optionally 10 -7 Torr.
[0033] Furthermore, in step 3), before starting the coating, the Mn-Co-Ni-Cu-O alloy target is pre-sputtered to remove pollutants and impurities on the surface of the target.
[0034] Furthermore, the method further comprises a segmentation step: segmenting the negative temperature coefficient thermosensitive film obtained in step 3), optionally segmenting along the corresponding part of the groove of the single crystal silicon substrate.
[0035] In a fourth aspect, a method for manufacturing the negative temperature coefficient thermistor temperature sensor described in the first aspect is provided, wherein liquid silver glue is added to both sides of a negative temperature coefficient thermistor film of appropriate size prepared by the manufacturing method described in the third aspect, and a platinum wire electrode is inserted into the liquid silver glue, stabilized, cured, and dried to obtain a negative temperature coefficient thermistor temperature sensor.
[0036] In the fifth aspect, there is provided an application of the negative temperature coefficient thermistor temperature sensor described in the first aspect, the single crystal silicon substrate described in the second aspect, the negative temperature coefficient thermistor film prepared by the manufacturing method described in the third aspect, and the negative temperature coefficient thermistor temperature sensor prepared by the manufacturing method described in the fourth aspect in integrated circuits, advanced manufacturing, and micro-nano processing.
[0037] Beneficial Effects
[0038] The present invention optimizes the brittleness and plasticity of the thermosensitive film, reduces the in-plane residual stress of the thermosensitive film, and prepares a Mn-Co-Ni-Cu-O thermosensitive film with a thickness of more than 7.7 μm by introducing the Cu element, performing 1 / 3 thickness pre-cutting on a single crystal silicon substrate, and adopting two magnetron sputtering processes. The surface of the thermosensitive film is intact and well bonded to the silicon dioxide layer, and no cracking or falling off occurs; the resistance of the prepared thermosensitive film is less than 500Ω, and no annealing heat treatment is required; compared with the existing technical route, the technical route of the present application is simple and efficient, and the production efficiency and yield rate are very high. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] One or more embodiments are exemplarily described by the pictures in the accompanying drawings, and these exemplary descriptions do not constitute limitations on the embodiments. The special word "exemplary" here means "used as an example, embodiment or illustrative". Any embodiment described as "exemplary" here is not necessarily interpreted as being superior or better than other embodiments.
[0040] Figure 1 A diagram of an embodiment of a negative temperature coefficient thermistor temperature sensor prepared according to the present invention.
[0041] Figure 2 The photos and structural diagrams of the single crystal silicon substrate pre-cut to 1 / 3 thickness according to the present invention; A is a real photo; B is a top view structural diagram of the single crystal silicon substrate, and C is a partial structure of the cross-sectional diagram.
[0042] Figure 3 This is a practical photo of the negative temperature coefficient thermistor temperature sensor prepared according to the present invention.
[0043] Figure 4 This is a SEM image of the Mn-Co-Ni-Cu-O thermosensitive film prepared in Example 1 of the present invention.
[0044] Figure 5 This is an AFM image of the Mn-Co-Ni-Cu-O thermosensitive film prepared in Example 1 of the present invention.
[0045] Figure 6 This is a TEM image of the Mn-Co-Ni-Cu-O thermosensitive film prepared in Example 1 of the present invention.
[0046] Figure 7 This is the macroscopic morphology of the Mn-Co-Ni-Cu-O thermosensitive film prepared in Comparative Example 1 of the present invention.
[0047] Figure 8The temperature-resistance relationship diagram of the negative temperature coefficient thermistor temperature sensor prepared in Example 1 of the present invention; wherein devices 1 and 2 are two randomly selected from the prepared devices, and the solid lines corresponding to devices 1 and 2 are their actual measured temperature-resistance data; the fitting lines of devices 1 and 2 respectively represent the actual measured temperature-resistance data of devices 1 and 2. DETAILED DESCRIPTION
[0048] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0049] In addition, in order to better illustrate the present invention, numerous specific details are provided in the specific embodiments below. It should be understood by those skilled in the art that the present invention can also be implemented without certain specific details. In some embodiments, raw materials, elements, methods, means, etc. well known to those skilled in the art are not described in detail, so as to highlight the main purpose of the present invention.
[0050] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.
[0051] The invention provides a negative temperature coefficient thermosensitive film, comprising a platinum wire electrode, a Mn-Co-Ni-Cu-O thermosensitive film, insulating silicon dioxide and a single crystal silicon substrate, wherein the Mn-Co-Ni-Cu-O thermosensitive film has a spinel structure, which can be regarded as a cubic close packing formed by oxygen ions, and the structure of its unit cell is AB2O4, wherein the A ions occupy the oxygen tetrahedral voids formed by four oxygen atoms, and the B ions occupy the oxygen octahedral voids formed by six oxygen atoms; the thermosensitive properties of the spinel structure thermosensitive material largely depend on the jumping conductivity between the variable valence cations located in the oxygen octahedron in the crystal structure. In the oxygen octahedral structure of the Mn-Co-Ni-Cu-O thermosensitive film, some oxygen ions will be separated to obtain a certain concentration of oxygen vacancies, and the oxygen vacancies will not only provide additional electrons, but also lead to the deviation of the stoichiometric ratio of the material, the change of the valence state of the metal cations and the distortion of the oxygen octahedron, etc., effectively improving and regulating the physical properties of the material and improving the thermosensitive properties of the film. Experiments show that the negative temperature coefficient thermistor film resistor of the present invention is less than 500Ω, has excellent thermal sensitivity and temperature measurement accuracy, ensures the use effect of the thermistor sensor, and is conducive to the application of negative temperature coefficient thermistor film in the field of integrated circuits.
[0052] In a first aspect, the present invention provides an embodiment of a negative temperature coefficient thermistor temperature sensor, such as Figure 1 As shown, it includes a single crystal silicon substrate block 1' and a negative temperature coefficient thermistor film 3 grown on a silicon dioxide layer 10 of the single crystal silicon substrate block 1'. The negative temperature coefficient thermistor film 3 is a Mn-Co-Ni-Cu-O thermistor film having a spinel structure.
[0053] The single crystal silicon substrate block 1' refers to a small block formed by dividing a single crystal silicon substrate block. When it is used, silver glue is used to stick 80 μm diameter platinum wires on both sides of the negative temperature coefficient thermistor film to form electrodes.
[0054] Further, the thickness of the negative temperature coefficient thermistor film 3 is ≥7 μm, optionally ≥7.5 μm, optionally ≥7.7 μm, and the resistance thereof is less than 700Ω, optionally less than 500Ω.
[0055] Furthermore, the size of the negative temperature coefficient thermistor film 3 is (2-10) mm×(2-10) mm, and optionally 5 mm×5 mm.
[0056] Furthermore, the negative temperature coefficient thermistor film 3 is formed by multiple depositions using a Mn-Co-Ni-Cu-O alloy target by a physical deposition coating method; optionally, the physical deposition coating method includes magnetron sputtering, laser molecular beam epitaxy or electron beam evaporation; optionally, the deposition times are at least twice.
[0057] Furthermore, in the negative temperature coefficient thermistor film 3, the mass ratio of Mn, Co, Ni, Cu and O is (28-32): (28-32): (14-16): (0.1-2.5): (20-28), optionally (28-30): (28-30): (15-15.5): (0.5-2): (23-28), optionally 30: 30: (15-15.5): (0.5-2): (23-24).
[0058] Furthermore, the structure of the spinel unit cell is AB2O4, wherein the A ions occupy the oxygen tetrahedral voids formed by four oxygen atoms, and the B ions occupy the oxygen octahedral voids formed by six oxygen atoms.
[0059] In a second aspect, the present invention provides an embodiment of a single crystal silicon substrate 1 for preparing the negative temperature coefficient thermistor temperature sensor described in the first aspect, such as Figure 2 As shown, the single crystal silicon substrate 1 is cut with grooves 2 interlaced vertically and horizontally to form a plurality of small units (one small unit corresponds to a single crystal silicon substrate block 1 ′), which are used to be divided into a plurality of single crystal silicon substrate blocks 1 ′ along the grooves 2 .
[0060] Further, the depth of the groove 2 on the single crystal silicon substrate 1 is 160 μm to 320 μm; optionally, the depth of the groove 2 is 1 / 4 to 1 / 2 of the thickness of the single crystal silicon substrate, and optionally 1 / 3;
[0061] Further, the plurality of small units are a plurality of square units, and optionally the size of the square units is (2-10) mm×(2-10) mm, and optionally 5 mm×5 mm.
[0062] Furthermore, the present invention provides a preferred preparation method, which is as follows:
[0063] Example 1
[0064] The manufacturing method of the negative temperature coefficient thermistor temperature sensor of this embodiment is carried out according to the following steps:
[0065] 1) Pretreatment of the Mn-Co-Ni-Cu-O alloy target: preparing a Mn-Co-Ni-Cu-O alloy target by mixing Mn, Co, Ni, Cu and O elements in a mass fraction ratio of 30:30:15.5:0.5:24, polishing the surface of the Mn-Co-Ni-Cu-O alloy target with 300 mesh, 600 mesh, 1200 mesh and 1800 mesh silicon carbide sandpaper in sequence, cleaning and drying after polishing, removing the surface oxide layer, and obtaining a pretreated Mn-Co-Ni-Cu-O alloy target;
[0066] 2) 1 / 3 thickness cutting of single crystal silicon substrate: Use silicon wafer laser cutting machine to cut 1 / 3 thickness of single crystal silicon substrate with silicon dioxide layer, make vertical and horizontal cutting from the surface of silicon dioxide layer, and interweave horizontal and vertical grooves on the single crystal silicon substrate to form multiple 5mm×5mm square blocks, but the whole is still a complete single crystal silicon wafer, see Figure 2 The 1 / 3 thickness pre-cutting of the single crystal silicon substrate in this step can optimize the technical route of preparing the thermosensitive film by magnetron sputtering and improve the production efficiency and yield rate.
[0067] 3) Pretreatment of the single crystal silicon substrate: The cut single crystal silicon substrate is immersed in acetone, anhydrous ethanol, deionized water and anhydrous ethanol in turn for ultrasonic washing twice, each washing time is 5 minutes, the single crystal silicon substrate is taken out, and the surface of the single crystal silicon substrate is dried with high-purity nitrogen to obtain a pretreated single crystal silicon substrate;
[0068] 4) Pre-sputtering of Mn-Co-Ni-Cu-O alloy target: The Mn-Co-Ni-Cu-O alloy target pretreated in step 1) is mounted on the target position at the bottom of the DC magnetron sputtering chamber, and the single crystal silicon substrate pretreated in step 3) is mounted on the substrate table at the top of the DC magnetron sputtering chamber. The chamber of the magnetron sputtering chamber is closed, and the vacuum system is turned on to evacuate the chamber. When the mechanical pump evacuates the chamber to a vacuum degree of less than 10-2 Torr, turn on the molecular pump and turn off the mechanical pump, and the chamber vacuum is pumped to less than 10 -7 Torr, the Ar gas flow rate was set to 50 sccm, the sputtering power of the alloy target was set to 240 W, and the baffle plate above the target position was extended to block the Mn-Co-Ni-Cu-O alloy target, so that the Mn-Co-Ni-Cu-O alloy target was pre-sputtered for 30 minutes to remove pollutants and impurities on the surface of the alloy target;
[0069] 5) Preparation of Mn-Co-Ni-Cu-O thermosensitive film: After the alloy target was pre-sputtered for 30 minutes, the baffle above the alloy target was withdrawn and coating was started on the single crystal silicon substrate; the Ar gas flow rate was maintained at 50 sccm and the power was maintained at 240 W. After sputtering for 200 minutes, the voltage and current were turned off, and the entire magnetron sputtering system was cooled for 60 minutes. The voltage and current were then restored and the sputtering was continued for 300 minutes. After the sputtering was completed, the voltage and current were turned off. After cooling for 40 minutes, the cavity was opened and the prepared Mn-Co-Ni-Cu-O thermosensitive film was taken out.
[0070] After this step is completed by two magnetron sputterings (200min+300min), it is measured with a multimeter and it is known that the film resistance is (0~3) kΩ. The inventor's preliminary experiments found that after one magnetron sputtering (200min), the resistance is (20-60) kΩ. The greater the resistance, the lower the temperature measurement accuracy and resolution of the thermistor film, and it may even not have negative temperature characteristics. The present invention increases the thickness of the thermistor film and reduces the resistance of the thermistor film by multiple sputtering. The present invention uses a single crystal silicon substrate with grooves to reduce the in-plane residual stress of the thermistor film to avoid cracking and falling off of the film, thereby improving the temperature measurement accuracy and accuracy of the thermistor film device, and solves the problem in the prior art that the continuously accumulated stress cannot be released after the film thickness is increased, resulting in cracking and falling off.
[0071] 6) Break the Mn-Co-Ni-Cu-O thermosensitive film together with the single crystal silicon substrate along the grooves and divide them into small pieces of 5mm×5mm (due to the vertical and horizontal grooves on the single crystal silicon substrate, most of the sputtered material enters the bottom of the groove during sputtering, and a small part adheres between the small pieces of 5mm×5mm. Because of the presence of the grooves, the single crystal silicon substrate is also easy to break along the bottom of the groove, that is, the connection between the small pieces of 5mm×5mm is weak and easy to break).
[0072] 7) Then drip liquid silver glue on both ends of each small piece of thermal film, and then use tweezers to quickly insert one end of a platinum wire with a length of 1.5cm and a diameter of 80μm into the silver glue droplet, and keep it stable for (20-30)s. After the silver glue solidifies, release the tweezers and continue to drip 1-2 drops of silver glue on the bonding end of the platinum wire. Place the entire thermistor device in a ventilated and dry place to dry for (4-5) hours. The actual photo is as follows Figure 3shown.
[0073] Example 2
[0074] The difference from Example 1 is that the ratio of the alloy target is different. Specifically, Mn, Co, Ni, Cu and O elements are prepared in a mass fraction ratio of 30:30:15:2:23 to prepare a Mn-Co-Ni-Cu-O alloy target. The remaining steps are the same as in Example 1.
[0075] Example 3
[0076] The difference from Example 1 is that the ratio of the alloy target is different. Specifically, Mn, Co, Ni, Cu and O elements are mixed in a mass fraction ratio of 28:28:15.5:0.5:28 to prepare a Mn-Co-Ni-Cu-O alloy target. The remaining steps are the same as in Example 1.
[0077] Example 4
[0078] Sputtering times
[0079] The difference from Example 1 is that the number of sputtering times is different. Specifically, only one sputtering deposition is performed, and the remaining steps are the same as those in Example 1.
[0080] In the above embodiment, the Mn—Co—Ni—Cu—O thermosensitive film may also be prepared by laser molecular beam epitaxy, electron beam evaporation or other physical deposition coating methods.
[0081] Comparative Example 1
[0082] The difference from Example 1 is that the single crystal silicon substrate is not pre-cut in step 2), the Mn-Co-Ni-Cu-O film is cut in step 6), and steps 1), 3), 4) and 5) are the same as in Example 1.
[0083] Comparative Example 2
[0084] The difference from Comparative Example 1 is that in step 5), annealing treatment is performed, the film sample is placed in an annealing furnace, the annealing oxidation treatment temperature is 700° C., the annealing time is 120 minutes, and the annealed thermosensitive film is obtained.
[0085] Comparative Example 3
[0086] The difference from Comparative Example 1 is that step 5) is sputtered only once: after the alloy target is pre-sputtered for 30 minutes, the baffle above the alloy target is withdrawn and coating on the single crystal silicon begins; the Ar gas flow rate is maintained at 50 sccm, the power is maintained at 240 W, and after sputtering for 200 minutes, the voltage and current are turned off. After cooling for 40 minutes, the cavity is opened and the prepared Mn-Co-Ni-Cu-O thermal sensitive film is taken out.
[0087] Test Example 1
[0088] The thickness of each embodiment and comparative example was measured, and the morphology of the heat-sensitive film was observed.
[0089] After testing, the thickness of the Mn-Co-Ni-Cu-O thermosensitive film of Examples 1, 2, 3, and 4 was 7.7 μm, 7.6 μm, 7.7 μm, and 2.9 μm, respectively. The film surface was intact and well bonded to the silicon dioxide layer on the single crystal silicon substrate, without cracking or falling off. The thickness of the Mn-Co-Ni-Cu-O thermosensitive film of Comparative Examples 1 and 2 was 7.7 μm and 7.8 μm, respectively. Although the thickness also exceeded 7.7 μm, the film surface cracked and fell off, as shown in FIG. Figure 7 After reducing the number of sputtering times in Comparative Example 3, the thickness of the thermal sensitive film is 2.9 μm, but it is easy to be contaminated and damaged when the single crystal silicon substrate is divided.
[0090] Test Example 2
[0091] The resistance of each embodiment and comparative example is detected by the unbalanced bridge method: this method involves the working principle and method of the bridge, including pre-adjusting the bridge balance and measuring the relationship between the resistance value and temperature of the alloy material at different temperatures. The unbalanced bridge has a high sensitivity and is suitable for measuring the resistance temperature coefficient of the alloy material. When the preset temperature is stable, the output voltage of the unbalanced bridge and the resistance value of the thermistor measured by the digital multimeter are recorded at the same time, and then this process is repeated at different temperatures to achieve a sufficient number of measurement points. After measurement, the resistance of the Mn-Co-Ni-Cu-O thermistor film of Examples 1, 2, 3, and 4 is 420Ω, 390Ω, 670Ω, and 1825Ω, respectively. The resistance of Comparative Examples 1, 2, and 3 is 430Ω, 370Ω, and 1925Ω.
[0092] The results of test examples 1 and 2 show that the Mn-Co-Ni-Cu-O thermistor films prepared in Examples 1, 2, and 3 have low resistance and are not easy to crack or fall off. The thermistor films prepared in Example 4 and Comparative Example 3 have high resistance. The thermistor film of Example 4 is not easy to crack or fall off, while the thermistor film of Comparative Example 3 is prone to crack or fall off, and the production efficiency is low. The Mn-Co-Ni-Cu-O thermistor films prepared in Comparative Examples 1 and 2 also have low resistance, but are prone to crack or fall off, and the production efficiency is low.
[0093] Test Example 3
[0094] The Mn-Co-Ni-Cu-O thermosensitive films of Examples 1 to 4 were photographed by scanning electron microscope (SEM), atomic force microscope (AFM) and transmission electron microscope (TEM), respectively. The SEM image, AFM image and TEM image of Example 1 are shown as follows: Figure 4 , 5 As shown in Figure 6, the results show that the surface of the thermosensitive film is very smooth, with a roughness of (15-20) nm and a film thickness of 7.7 μm. The thermosensitive film is composed of columnar crystals, grows densely, and the crystal structure is mainly spinel structure.
[0095] Test Example 4
[0096] The unbalanced bridge method is used to measure the relationship between resistance and temperature, and the resistance-temperature relationship line is drawn. The results are as follows: Figure 8 The results show that the thermistor has a very significant resistance-temperature linear relationship and a negative temperature coefficient characteristic.
[0097] The present invention optimizes the brittleness and plasticity of the thermosensitive film, reduces the in-plane residual stress of the thermosensitive film, and prepares a Mn-Co-Ni-Cu-O thermosensitive film with a thickness of more than 7.7 μm by introducing the Cu element, performing 1 / 3 thickness pre-cutting on a single crystal silicon substrate, and adopting two magnetron sputtering processes. The surface of the thermosensitive film is intact and well bonded to the silicon dioxide layer, and no cracking or falling off occurs; the resistance of the prepared thermosensitive film is less than 500Ω, and no annealing heat treatment is required; compared with the existing technical route, the technical route of the present application is simple and efficient, and the production efficiency and yield rate are very high.
[0098] The present invention uses silver glue to stick a platinum wire with a diameter of 80 μm to both sides of a thermosensitive film to form an electrode. It only takes tens of seconds to stick an electrode, and the time and cost costs are low. The electrode bonding scheme is very simple, and the bonding efficiency and success rate are extremely high, which is very beneficial to the actual manufacture and application of thermistor temperature sensors.
[0099] The present invention can make the Mn-Co-Ni-Cu-O thermosensitive film grown by magnetron sputtering into independent square small pieces of 5mm×5mm in area by pre-cutting the single crystal silicon substrate with 1 / 3 thickness; this scheme can reduce the residual stress generated in the growth process of the thermosensitive film, avoid cracking and falling off of the thermosensitive film, and directly break and divide the prepared thermosensitive film, which is simple and efficient.
[0100] The negative temperature coefficient thermistor of the present invention comprises a platinum wire electrode, a Mn-Co-Ni-Cu-O thermistor film, insulating silicon dioxide and a single crystal substrate, wherein the Mn-Co-Ni-Cu-O thermistor film has a spinel structure, which can be regarded as a cubic close packing formed by oxygen ions, and the structure of its unit cell is AB2O4, wherein the A ions occupy the oxygen tetrahedral voids composed of four oxygen atoms, and the B ions occupy the oxygen octahedral voids composed of six oxygen atoms; the thermosensitive properties of the spinel structure thermosensitive material largely depend on the jumping conductivity between the variable valence cations located in the oxygen octahedron in the crystal structure. In the oxygen octahedral structure of the Mn-Co-Ni-Cu-O thermistor film of the present invention, some oxygen ions will be separated to obtain a certain concentration of oxygen vacancies, and the oxygen vacancies will not only provide additional electrons, but also lead to the deviation of the stoichiometric ratio of the material, the change of the valence state of the metal cations and the distortion of the oxygen octahedron, etc., effectively improving and regulating the physical properties of the material and improving the thermosensitive properties of the film.
[0101] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A negative temperature coefficient thermistor temperature sensor, characterized in that it comprises a single crystal silicon substrate block and a negative temperature coefficient thermistor film grown on a silicon dioxide layer of the single crystal silicon substrate block, wherein the negative temperature coefficient thermistor film is a Mn-Co-Ni-Cu-O thermistor film having a spinel structure; In the negative temperature coefficient thermistor film, the mass ratio of Mn, Co, Ni, Cu and O is (28-32): (28-32): (14-16): (0.1-2.5): (20-28).
2. The negative temperature coefficient thermistor temperature sensor according to claim 1, characterized in that: The thickness of the negative temperature coefficient thermistor film is ≥7 μm, optionally ≥7.5 μm, optionally ≥7.7 μm; And / or, the resistance of the negative temperature coefficient thermistor film is less than 700Ω, optionally less than 500Ω; And / or, the size of the negative temperature coefficient thermistor film is (2-10) mm×(2-10) mm, optionally 5 mm×5 mm; And / or, platinum wires are bonded to both sides of the negative temperature coefficient thermistor film, and optionally, silver glue is used for bonding.
3. The negative temperature coefficient thermistor temperature sensor according to claim 1 or 2, characterized in that: The negative temperature coefficient thermistor film is formed by multiple depositions of a Mn-Co-Ni-Cu-O alloy target material by a physical deposition coating method; optionally, the physical deposition coating method includes a magnetron sputtering method, a laser molecular beam epitaxy method or an electron beam evaporation method; optionally, the deposition times are at least twice; And / or, in the negative temperature coefficient thermistor film, the mass ratio of Mn, Co, Ni, Cu, and O is (28-30): (28-30): (15-15.5): (0.5-2): (23-28), and optionally 30: 30: (15-15.5): (0.5-2): (23-24); And / or, the structure of the spinel structure unit cell is AB2O4, wherein the A ions occupy the oxygen tetrahedral voids formed by four oxygen atoms, and the B ions occupy the oxygen octahedral voids formed by six oxygen atoms.
4. A single crystal silicon substrate for preparing a negative temperature coefficient thermistor temperature sensor according to any one of claims 1 to 3, characterized in that: The single crystal silicon substrate is cut with grooves interlaced vertically and horizontally to form a plurality of small units, which are used to be divided into a plurality of single crystal silicon substrate blocks along the grooves.
5. The single crystal silicon substrate according to claim 4, characterized in that: The groove depth on the single crystal silicon substrate is 160 μm to 320 μm; optionally, the groove depth is 1 / 4 to 1 / 2 of the thickness of the single crystal silicon substrate, and optionally 1 / 3; And / or, the plurality of small units are a plurality of square units, and optionally the size of the square units is (2-10) mm×(2-10) mm, and optionally 5 mm×5 mm.
6. A method for manufacturing a negative temperature coefficient thermistor film, characterized in that: The steps include: 1) Pre-treat the Mn-Co-Ni-Cu-O alloy target to remove the surface oxide layer and pollutants; 2) pretreating the single crystal silicon substrate according to claim 4 or 5 to remove surface impurities and contaminants; 3) Physical deposition coating is performed on the single crystal silicon substrate pretreated in step 2) by using the Mn-Co-Ni-Cu-O alloy target pretreated in step 1), at least twice, to obtain a negative temperature coefficient thermistor film.
7. The manufacturing method according to claim 6, characterized in that: In step 3), the method of physical deposition coating includes: when coating begins, in an inert atmosphere, performing a first sputtering coating, then cooling, performing a second sputtering coating, and cooling; and so on, obtaining a negative temperature coefficient thermistor film by at least two sputtering coatings; Optionally, the first sputtering coating time is (150-250) min, optionally 200 min; Optionally, the second sputtering coating time is (250-350) min, optionally 300 min; Optionally, the power of the sputtering coating is (200-260) W, optionally 240 W; Optionally, the inert atmosphere is argon or helium; Optionally, the flow rate of the inert atmosphere is (48-52) sccm, optionally 50 sccm; Optionally, the sputtering vacuum degree is (10 -7 ~10 -8 )Torr, optionally 10 -7 Torr.
8. The manufacturing method according to claim 6 or 7, characterized in that: In step 3), before starting the coating, the Mn-Co-Ni-Cu-O alloy target is pre-sputtered to remove pollutants and impurities on the surface of the target; And / or, it also includes a segmentation step: segmenting the negative temperature coefficient thermistor film obtained in step 3), optionally segmenting along the corresponding part of the groove of the single crystal silicon substrate.
9. A method for manufacturing a negative temperature coefficient thermistor temperature sensor according to any one of claims 1 to 3, characterized in that: Liquid silver glue is added to both sides of a negative temperature coefficient thermistor film of suitable size prepared by the manufacturing method described in any one of claims 6 to 8, and a platinum wire electrode is inserted into the liquid silver glue, stabilized, cured, and dried to obtain a negative temperature coefficient thermistor temperature sensor.
10. Application of a negative temperature coefficient thermistor temperature sensor as claimed in any one of claims 1 to 3, a single crystal silicon substrate as claimed in claim 4 or 5, a negative temperature coefficient thermistor film prepared by the manufacturing method as claimed in any one of claims 6 to 8, and a negative temperature coefficient thermistor temperature sensor prepared by the manufacturing method as claimed in claim 9 in integrated circuits, advanced manufacturing, and micro-nano processing.
Citation Information
Patent Citations
Chip thermistor and manufacturing method thereof
CN102800449A
Vacuum sputtering electrode of ceramic thermistor and manufacturing method thereof
CN105006316A
Metal-doped amorphous carbon film temperature-sensing element and preparation method therefor
CN105241569A
Titanium-ruthenium co-doped vanadium dioxide thermo-sensitive thin film material and preparation method thereof
CN107686973A
High-resistance temperature coefficient vanadium dioxide film and low-temperature deposition method thereof
CN108070835A
Cited By
A negative temperature coefficient thermistor temperature sensor, its manufacturing method and application
CN118913470B