Metallographic etchant and metallographic structure display method
The metallographic erosive agent prepared by ammonium chloride, ammonium bicarbonate and deionized water corrodes the grain boundaries of Hastelloy at low risk, solving the problems of operation difficulty and risk in the existing technology, and realizing the metallographic structure Clearly display and study.
Patent Information
- Application Number
- CN202410970995.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
The corrosion methods used in the prior art for metallographic research of Hastelloy have problems of difficulty and high risk, especially the use of high temperature and high pressure corrosion agents such as sulfuric acid and perchloric acid.
Using metallographic erosive agent prepared from ammonium chloride, ammonium bicarbonate and deionized water, the metallographic erosion is decomposed by heating in a hydrothermal kettle to form CO2 and NH3, forming ammonium carbamate and cyanate, destroying the passivation film, and etching the grain boundaries first. Show metallographic structure.
The metallographic display with low risk, convenient operation and good erosion effect is achieved. The grain boundary is clear under microscopic observation, which is suitable for metallographic research of Hastelloy.
Smart Images

Figure HDA0004953202320000011 
Figure HDA0004953202320000012 
Figure HDA0004953202320000021
Abstract
Description
Technical Field
[0001] The invention relates to a metallographic etching agent, in particular to a metallographic etching agent and a metallographic structure display method, belonging to the technical field of metallographic corrosion. Background Art
[0002] HC276 has good corrosion resistance and can resist corrosion from a variety of strong acids, strong alkalis and oxidants. HC276 also has excellent high-temperature stability and can maintain its performance in high-temperature environments up to 1000°C, making it an ideal material for manufacturing high-temperature equipment, furnaces and pipelines.
[0003] In addition, HC276 has excellent mechanical properties, including high strength, high toughness and good processability. These advantages make it widely used in chemical, petroleum, marine engineering, pharmaceutical, electric power and medical fields, with broad application prospects.
[0004] In order to determine the influence of microstructure on material properties, the microstructure of Hastelloy needs to be studied.
[0005] Patent CN110687117A uses different etching solutions and corrodes the metallographic sample in three steps. The metallographic structure is clear and the grain boundaries are easy to distinguish. However, the corrosion process is highly risky, especially the need to heat 98% sulfuric acid to above 90°C, which is difficult and risky to operate.
[0006] Authorized patent CN113640090B uses a one-step method to etch the metallographic structure of high-temperature alloys. The resulting metallographic structure is clear, with obvious boundaries such as grain boundaries, and can better reflect the actual situation of the structure. However, the etching agent used in this method is concentrated hydrochloric acid, which is difficult and risky to operate.
[0007] Patent publication CN109468678A uses an electrolytic method to observe the metallographic structure of a high-melting-point high-entropy alloy, and can clearly observe the dendrite structure and tissue defects. However, the electrolyte in this method uses a perchloric acid solution, which has high operating difficulty and risk. Summary of the invention
[0008] The technical problem to be solved by the present invention is to provide a metallographic etching agent which is easy to operate, risk-free and has good etching effect for the metallographic research of Hastelloy materials.
[0009] In order to solve the above technical problems, the present invention discloses a metallographic etchant, which comprises the following components: ammonium chloride, ammonium bicarbonate, and deionized water are prepared in proportion. The etchant formula used in the present invention replaces the etchant formulas of hydrochloric acid, nitric acid, sulfuric acid, etc., and can achieve the purpose of corroding grain boundaries and displaying the metallographic structure of Hastelloy alloy.
[0010] As a preferred solution, the metallographic etching agent of the present invention comprises the following components mixed:
[0011] Ammonium chloride 10-25wt%;
[0012] Ammonium bicarbonate 40-65wt%;
[0013] Deionized water 25-35wt%.
[0014] The ammonium bicarbonate reagent used in the etchant of the present invention has the advantages of mild medium, easy operation and low risk compared to strong corrosive media such as hydrochloric acid, nitric acid and sulfuric acid. After the ammonium bicarbonate reagent is heated to 60°C in a hydrothermal kettle, it decomposes to form CO2, NH3 and H2O. The decomposed CO2 and NH3 react again in the hydrothermal kettle to form ammonium carbamate NH4COONH2, which has strong reducing properties and can destroy the passivation film. In addition, ammonium bicarbonate will also decompose to form cyanate CNO-, which also has strong reducing properties and also damages the passivation film. The passivation film is destroyed under the action of chloride ions, ammonium carbamate, cyanate, etc. Under the complexation of NH3, the surface passivation film dissolves and preferentially destroys the passivation film in the grain boundary area, eventually causing the grain boundary to be corroded, showing the metallographic structure of Hastelloy alloy. The general change process is as follows:
[0015] NH4HCO3 = NH3 + H2O + CO2 (1)
[0016] 2NH3 + CO2 = NH4COONH2 (2)
[0017] 2NH4HCO3 = NH4 + +CNO - +3H2O +CO2 (3)
[0018] In conjunction with the use of an etchant, the present invention further provides a metallographic structure display method, that is, using the metallographic etchant described above to perform closed immersion on the pretreated metallographic sample, preferably using a hydrothermal kettle, to display the metallographic structure.
[0019] According to the metallographic structure display method, the immersion time is 30 to 60 minutes, so that the corrosive agent can fully corrode the grain boundaries of the metallographic sample, and the immersion temperature is 65° C. to 85° C.
[0020] According to the metallographic structure display method, after immersion, the corrosive agent on the surface of the metallographic sample is immediately removed by water washing, and then the metallographic sample is rinsed with an organic alcohol solution for 10 to 20 seconds and dried.
[0021] According to the metallographic structure display method, the organic alcohol solution is preferably any one or more of ethanol, methanol, and ethylene glycol that are volatile and have good compatibility with water, and non-toxic ethanol is more preferred.
[0022] According to the metallographic structure display method, the pretreatment of the metallographic sample includes the steps of sampling, mounting, grinding, polishing, etc. The mounting can be carried out by a method known in the art, which may include cold mounting and hot mounting.
[0023] According to the metallographic structure display method, the polishing is rough grinding and fine grinding using sandpaper.
[0024] According to the metallographic structure display method, the polishing is mechanical polishing using a polishing cloth.
[0025] According to the etchant formula, the metallographic specimen used is made of Hastelloy alloy, preferably Hastelloy HC276 alloy.
[0026] According to a metallographic etching agent and a matching metallographic structure display method, as a preferred solution, the following steps are included:
[0027] 1) Cut and obtain Hastelloy alloy samples with a size of about 5mm×5mm×2mm, and use cold mounting to mount the samples for the convenience of the next step of polishing; the cold mounting material is phenolic resin or epoxy resin;
[0028] 2) After embedding, the sample is grinded from coarse to fine with water-resistant sandpaper of different grain sizes using a metallographic pre-grinding machine; water is continuously added during the grinding process, and one grinding is completed when the directions of the scratches are all consistent. The sandpaper is replaced for the next grinding, and the grinding direction is perpendicular to the direction of the last scratch; the above steps are repeated until a sample with extremely shallow scratches and a bright surface is obtained; after the pre-grinding is completed, the sample is chamfered to prevent the impact on the subsequent mechanical polishing;
[0029] 3) The ground sample is mechanically polished. During the polishing process, the polishing spray is sprayed and water is dripped into the center of the polishing disc to avoid polishing marks or polishing surface. At the end of polishing, the polishing cloth is cleaned and polished with running water to remove residual diamond particles and dirt.
[0030] 4) After the polished sample is dried with a hair dryer, the sample is directly immersed in the prepared metallographic etching solution, and immersed in a closed water-heated kettle for 30 to 60 minutes. The oven is heated to 65 to 85°C for etching. After the etching is completed, the sample is taken out and the etching solution is immediately rinsed off with water;
[0031] 5) Rinse the sample surface with an organic alcohol solution for 10 to 20 seconds, rinse off the water, blow dry with a hair dryer, and then observe the microscopic metallographic structure.
[0032] Compared with the prior art, the present invention has the following advantages:
[0033] 1. The etchant in the present invention uses ammonium bicarbonate reagent instead of hydrochloric acid, nitric acid and sulfuric acid reagents, and the operation risk is low;
[0034] 2. The etchant in the present invention uses ammonium bicarbonate reagent, which has the advantage of better etch effect compared with electrolytic etching, aqua regia and other reagents;
[0035] 3. The etchant has little erosion on the inside of the grain, the grain boundary is clearly displayed, it is not easy to be over-eroded, and the erosion effect is good;
[0036] 4. The corrosion reproducibility and stability are good, which is very suitable for the metallographic display of Hastelloy.
[0037] Instruction Manual
[0038] Figure 1 This is a microscopic observation picture of the metallographic structure in Example 1 at a scale of 200 μm;
[0039] Figure 2 This is a microscopic observation picture of the metallographic structure in Example 2 at a scale of 200 μm;
[0040] Figure 3 This is a microscopic observation picture of the metallographic structure in Example 3 at a scale of 200 μm. DETAILED DESCRIPTION
[0041] The present invention is further described below through the accompanying drawings and specific embodiments. The embodiments of the present invention are only used to illustrate the present invention and do not limit the scope of the present invention.
[0042] [Example 1]
[0043] A metallographic etching agent is prepared from ammonium chloride, ammonium bicarbonate and deionized water in a mass ratio of 10:65:25.
[0044] The metallographic etchant prepared in this embodiment is used to display the metallographic structure of HC276 Hastelloy alloy. The specific method is as follows:
[0045] 1) Cut the HC276 Hastelloy alloy specimen with the size of 5mm×5mm×2mm and use cold mounting material to mount the specimen for the convenience of the next step of grinding;
[0046] 2) Place the mounted sample on a metallographic pre-grinding machine and grind it from coarse to fine with 120# water-resistant sandpaper, 400# water-resistant sandpaper, 600# water-resistant sandpaper, 1200# water-resistant sandpaper, and 2000# water-resistant sandpaper, respectively, at a speed of 500r / min; add water to cool it during the grinding process, and when the directions of the scratches are all consistent, one grinding is completed, and the sandpaper is replaced for the next grinding, and the grinding direction is perpendicular to the direction of the previous scratch; repeat the above steps until the grinding with 2000# water-resistant sandpaper is completed, and a sample with extremely shallow scratches and a bright surface is obtained;
[0047] 3) The ground sample is mechanically polished (rotation speed 300r / min), with diamond spray polishing agent as the polishing spray, sprayed during the polishing process, and water is injected into the center of the polishing disc in a drop-by-drop manner to avoid polishing marks or polishing surface; at the end of polishing, the polishing cloth is cleaned and polished with running water to remove residual diamond particles and dirt;
[0048] 4) After the polished sample is dried with a hair dryer, the sample is directly immersed in the prepared metallographic etching solution, and immersed in a closed water-heated kettle for 40 minutes. The oven is heated to 65°C for etching. After the etching is completed, the sample is taken out and the etching solution is immediately rinsed off with water;
[0049] 5) Rinse the sample surface with methanol solution for 10 to 20 seconds, rinse off the water, blow dry with a hair dryer, and then observe the microscopic metallographic structure.
[0050] [Example 2]
[0051] A metallographic etching agent is prepared from ammonium chloride, ammonium bicarbonate and deionized water in a mass ratio of 25:50:25.
[0052] The metallographic etchant prepared in this embodiment is used to display the metallographic structure of HC276 Hastelloy alloy. The specific method is as follows:
[0053] 1) Cut the HC276 Hastelloy alloy specimen with the size of 5mm×5mm×2mm and use cold mounting material to mount the specimen for the convenience of the next step of grinding;
[0054] 2) Place the mounted sample on a metallographic pre-grinding machine and grind it from coarse to fine with 120# water-resistant sandpaper, 400# water-resistant sandpaper, 600# water-resistant sandpaper, 1200# water-resistant sandpaper, and 2000# water-resistant sandpaper, respectively, at a speed of 500r / min; add water to cool it during the grinding process, and when the directions of the scratches are all consistent, one grinding is completed, and the sandpaper is replaced for the next grinding, and the grinding direction is perpendicular to the direction of the previous scratch; repeat the above steps until the grinding with 2000# water-resistant sandpaper is completed, and a sample with extremely shallow scratches and a bright surface is obtained;
[0055] 3) The ground sample is mechanically polished (rotation speed 300r / min), with diamond spray polishing agent as the polishing spray, sprayed during the polishing process, and water is injected into the center of the polishing disc in a drop-by-drop manner to avoid polishing marks or polishing surface; at the end of polishing, the polishing cloth is cleaned and polished with running water to remove residual diamond particles and dirt;
[0056] 4) After the polished sample is dried with a hair dryer, the sample is directly immersed in the prepared metallographic etching solution, and is sealed in a hydrothermal kettle for 50 minutes. The oven is heated to 75°C for etching. After the etching is completed, the sample is taken out and the etching solution is immediately rinsed off with water;
[0057] 5) Rinse the sample surface with ethanol solution for 10 to 20 seconds, rinse off the water, blow dry with a hair dryer, and then observe the microscopic metallographic structure.
[0058] [Example 3]
[0059] A metallographic etching agent is prepared from ammonium chloride, ammonium bicarbonate and deionized water in a mass ratio of 25:40:35.
[0060] The metallographic etchant prepared in this embodiment is used to display the metallographic structure of HC276 Hastelloy alloy. The specific method is as follows:
[0061] 1) Cut the HC276 Hastelloy alloy specimen with the size of 5mm×5mm×2mm and use cold mounting material to mount the specimen for the convenience of the next step of grinding;
[0062] 2) Place the mounted sample on a metallographic pre-grinding machine and grind it from coarse to fine with 120# water-resistant sandpaper, 400# water-resistant sandpaper, 600# water-resistant sandpaper, 1200# water-resistant sandpaper, and 2000# water-resistant sandpaper, respectively, at a speed of 500r / min; add water to cool it during the grinding process, and when the directions of the scratches are all consistent, one grinding is completed, and the sandpaper is replaced for the next grinding, and the grinding direction is perpendicular to the direction of the previous scratch; repeat the above steps until the grinding with 2000# water-resistant sandpaper is completed, and a sample with extremely shallow scratches and a bright surface is obtained;
[0063] 3) The ground sample is mechanically polished (rotation speed 300r / min), with diamond spray polishing agent as the polishing spray, sprayed during the polishing process, and water is injected into the center of the polishing disc in a drop-by-drop manner to avoid polishing marks or polishing surface; at the end of polishing, the polishing cloth is cleaned and polished with running water to remove residual diamond particles and dirt;
[0064] 4) After the polished sample is dried with a hair dryer, the sample is directly immersed in the prepared metallographic etching solution, and immersed in a closed water-heated kettle for 60 minutes. The oven is heated to 85°C for etching. After the etching is completed, the sample is taken out and the etching solution is immediately rinsed off with water;
[0065] 5) Rinse the sample surface with ethylene glycol solution for 10 to 20 seconds, rinse off the water, blow dry with a hair dryer, and then observe the microscopic metallographic structure.
Claims
1. A metallographic etching agent comprising the following components: ammonium chloride, ammonium bicarbonate, and deionized water.
2. The metallographic etching agent according to claim 1, characterized in that: It is obtained by mixing the following components: Ammonium chloride 10-25wt%; Ammonium bicarbonate 40-65wt%; Deionized water 25-35wt%.
3. A metallographic structure display method, characterized in that: The pretreated metallographic sample is immersed in the metallographic etching agent according to claim 1 or 2 to reveal the metallographic structure.
4. The metallographic structure display method according to claim 3, characterized in that: The soaking time is 30 to 60 minutes.
5. The metallographic structure display method according to claim 3 or 4, characterized in that: The soaking is soaking in a closed container.
6. The metallographic structure display method according to claim 5, characterized in that: The closed immersion container used is a hydrothermal kettle with a temperature of 65°C to 85°C.
7. The metallographic structure display method according to any one of claims 3 to 6, characterized in that: After the immersion is completed, the sample is taken out and washed with water to remove the corrosive agent on the surface of the metallographic sample. The metallographic sample is then rinsed with an organic alcohol solution, preferably for 10 to 20 seconds, and dried.
8. The metallographic structure display method according to claim 7, characterized in that: The organic alcohol solution is any one or more of ethanol, methanol and ethylene glycol.
9. The metallographic structure display method according to any one of claims 3 to 8, characterized in that: The pretreatment steps of the metallographic sample include sampling, mounting, grinding and polishing; preferably, the metallographic sample is Hastelloy HC276 alloy.
10. The metallographic structure display method according to claim 9, characterized in that: The polishing includes coarse grinding and fine grinding, and / or the polishing is mechanical polishing.
Citation Information
Patent Citations
Electrolytic corrosion solution used for high-melting-point high-entropy alloy and use method of electrolytic corrosion solution
CN109468678A
Metallographic etching agents for wrought superalloy, and metallographic structure display method for wrought superalloy
CN110687117A
A GH4141 high temperature alloy metallographic structure corrosive agent and corrosion method