Detection method and evaluation method for pressure resistance of silicon-based negative electrode material, and application of silicon-based negative electrode material

By measuring the roll-pressure gap ratio and rebound coefficient of the silicon-based negative electrode material, a rebound curve was established, which solved the problem of the lack of effective detection of the compressive resistance of the silicon-based negative electrode material in the prior art, and achieved an accurate evaluation of its compressive resistance and Improved performance of lithium-ion batteries.

CN118913900APending Publication Date: 2024-11-08GUANGDONG KAIJIN NEW ENERGY TECH CORP LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411076039.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art lacks effective methods to detect the compressive resistance of silicon-based negative electrode materials, affecting the performance and production consistency of lithium-ion batteries.

Method used

A detection method is adopted, including coating the negative electrode slurry on empty copper foil, rolling the pressure processing, and establishing a rebound curve by measuring the rolling mass gap ratio and rebound coefficient, and determining the compression resistance parameters of the silicon-based negative electrode material. Its compressive resistance is then evaluated.

Benefits of technology

This method can accurately, simply and efficiently evaluate the compressive resistance of silicon-based negative electrode materials, identify abnormal materials, guide material optimization and process improvement, and improve the performance and production efficiency of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118913900A_ABST
    Figure CN118913900A_ABST
Patent Text Reader

Abstract

The invention provides a detection method and an evaluation method for the pressure resistance of a silicon-based negative electrode material, and application of the silicon-based negative electrode material. The detection method comprises the following steps: coating an empty copper foil with negative electrode slurry, and drying to obtain a negative electrode plate; rolling the negative pole piece under the rolling pressure, respectively measuring the thicknesses d1 and d0 of the small pole piece and the copper foil piece at the central position, weighing the masses m1 and m0 of the small pole piece and the copper foil piece, and calculating the corresponding rolling mass gap ratio P under the rolling pressure; after rolling, carrying out heat treatment on the small pole piece, then cooling, measuring the thickness d2 of the cooled small pole piece at the central position, and calculating a rebound coefficient R; the rolling pressure is sequentially increased until the two sides of the pole piece are in a wave shape, the rolling mass gap ratio P and the rebound coefficient R corresponding to the rolling pressure are obtained, a rebound curve is established, and Pt corresponding to Rt on the rebound curve is the compression resistance parameter of the silicon-based negative electrode material. The detection method is convenient and effective, and can comprehensively reflect the pressure resistance of the silicon-based negative electrode material in actual use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of material performance detection, in particular to performance detection of negative electrode materials for secondary batteries, and more particularly to a detection method and an evaluation method for the compressive resistance of silicon-based negative electrode materials, and applications thereof. Background Art

[0002] At present, secondary batteries, especially lithium-ion batteries, have been widely used in new energy vehicles. With the growing demand for high energy density, the actual specific capacity of graphite and amorphous carbon in lithium-ion batteries as negative electrode materials of batteries has approached the theoretical limit, while high-specific-capacity silicon-based negative electrode materials (theoretical specific capacity of 4200mAh / g) have significant advantages. However, due to the serious volume expansion of silicon-based negative electrode materials during the process of charging and discharging lithium insertion / extraction, the silicon-based negative electrode materials themselves will be broken, and the broken interface will repeatedly form SEI film with the electrolyte, and even fall off from the current collector copper foil, thereby accelerating the capacity decay of the battery. By rolling the pole piece, a certain amount of expansion can be resisted, thereby improving the performance of the battery. Therefore, the current requirements for the compressive resistance of silicon-based negative electrode materials are relatively high. Researchers often modify the compressive resistance and toughness of silicon-based negative electrode materials in terms of shape, structure, etc., so as to improve the compressive resistance of the material, thereby improving the expansion, initial efficiency and cycle performance of the material.

[0003] Although, as an important part of lithium-ion battery research, the compressive performance of silicon-based negative electrode materials affects the uniformity of lithium insertion and extraction and the uniformity of interface expansion thickness during charge and discharge of single cells, and also affects the consistency of R&D and production of cells. However, there is currently no ready-made technical method to provide reference for the characterization of the compressive resistance of silicon-based negative electrode materials in actual batteries, so how to detect the compressive resistance of silicon-based negative electrode materials is an urgent problem to be solved. Summary of the invention

[0004] Based on the above problems, the purpose of the present invention is to provide a detection method and evaluation method for the compressive resistance of silicon-based negative electrode materials, and applications. This detection method is convenient and effective, can accurately obtain the corresponding compressive resistance parameters of silicon-based negative electrode materials, and can comprehensively reflect the compressive resistance of silicon-based negative electrode materials in actual use, so as to evaluate the compressive resistance of silicon-based negative electrode materials, identify abnormal materials in advance, and guide the promotion and application of silicon-based negative electrode materials in lithium-ion batteries.

[0005] To achieve the above-mentioned purpose, the first aspect of the present invention provides a method for detecting the compressive resistance of a silicon-based negative electrode material. The detection method comprises:

[0006] (1) coating a negative electrode slurry on a hollow copper foil and drying the negative electrode sheet, wherein the negative electrode slurry comprises a negative electrode active material, and the negative electrode active material comprises at least a silicon-based negative electrode material;

[0007] (ii) rolling the negative electrode sheet under rolling pressure, taking the same area from the coating area and the blank area of ​​the negative electrode sheet as the small electrode sheet and the copper foil sheet, measuring the thickness of the small electrode sheet and the blank copper foil at the center as d1 and d0, respectively, and calculating the rolling mass-gap ratio P corresponding to the rolling pressure, wherein m1 is the mass of the small electrode sheet, m0 is the mass of the copper foil sheet,

[0008]

[0009] (iii) heat treating the small pole piece and then cooling it, measuring the thickness d2 of the small pole piece at the center after cooling, and calculating the rebound coefficient R,

[0010]

[0011] (iv) increasing the rolling pressure successively until a wave shape appears on both sides of the negative electrode sheet, obtaining the rolling mass-gap ratio P and the rebound coefficient R corresponding to each rolling pressure, and establishing a rebound curve with the rolling mass-gap ratio P as the abscissa and the corresponding rebound coefficient R as the ordinate. The rebound curve has R t The corresponding P t is the compressive strength parameter of the silicon-based negative electrode material, and the R t is the maximum rebound coefficient of the rebound curve at the inflection point.

[0012] In the technical solution adopted by the present invention, the pole piece containing the silicon-based negative electrode material is rolled, and the rolling pressure is increased successively. As the rolling mass-gap ratio of the pole piece increases, the compressive damage and rupture of the silicon-based negative electrode material intensify. When the rebound coefficient gradually reaches the maximum inflection point and exceeds the critical pressure of the silicon-based negative electrode material, the material begins to deform and break, and the elasticity decreases. The silicon-based negative electrode material gradually changes from elastic deformation to plastic deformation near this mass-gap ratio inflection point. Therefore, the rolling mass-gap ratio of the pole piece can truly reflect the stress of the material in actual production, and can more comprehensively reflect the compressive resistance of the silicon-based negative electrode material in actual use. The detection method can obtain the corresponding compressive resistance parameters by establishing a rebound curve of the rolling mass-gap ratio P and the rebound coefficient R. Compared with other technical methods, it is simple and efficient, low-cost, economical and environmentally friendly.

[0013] As a technical solution of the present invention, the negative electrode slurry includes a negative electrode active material, a binder, a conductive agent and a solvent.

[0014] As a technical solution of the present invention, taking the sum of the masses of the negative electrode active material, the binder and the conductive agent as 100%, the mass of the negative electrode active material accounts for 92-95%, the mass of the binder accounts for 4-6%, and the mass of the conductive agent accounts for 4-7%.

[0015] As a technical solution of the present invention, the negative electrode active material includes a carbon material and a silicon-based negative electrode material, and the mass ratio of the carbon material to the silicon-based negative electrode material is 0-89:11-100.

[0016] As a technical solution of the present invention, the silicon-based negative electrode material includes at least one of elemental silicon, silicon oxide compounds, silicon carbon compounds, silicon alloy compounds, pre-magnesium silicon oxide compounds and pre-lithium silicon oxide compounds.

[0017] As a technical solution of the present invention, the binder includes carboxymethyl cellulose and / or styrene-butadiene rubber.

[0018] As a technical solution of the present invention, the conductive agent includes at least one of conductive carbon black, conductive graphite, carbon nanotubes, graphene and vapor-grown carbon fiber.

[0019] As a technical solution of the present invention, the solvent includes water.

[0020] As a technical solution of the present invention, when preparing the negative electrode slurry, first add part of the binder to the solvent and mix evenly, then add the conductive agent to mix to obtain a conductive glue, add the negative electrode active material to the conductive glue, mix, then add the remaining binder and stir evenly.

[0021] As a technical solution of the present invention, the solid content of the negative electrode slurry is 30% to 50%.

[0022] As a technical solution of the present invention, the rolling is carried out under a rolling press.

[0023] As a technical solution of the present invention, the rotation speed of the roller press is 40nm / s to 60nm / s.

[0024] As a technical solution of the present invention, the roller press has a roller gap D between the two rollers at the start. o , 80μm≤D o <2000μm.

[0025] As a technical solution of the present invention, the adjustable roller pressing gap of the roller press is D a , 0≤D a ≤2000μm.

[0026] As a technical solution of the present invention, the rolling gap between the two rollers of the roller press is reduced in sequence by 2 μm to 15 μm so as to increase the rolling pressure in sequence.

[0027] As a technical solution of the present invention, the roller press is preheated before performing the roller pressing operation.

[0028] As a technical solution of the present invention, the power of the roller press is 200W to 400W.

[0029] As a technical solution of the present invention, the frequency of the roller press is 30 Hz to 70 Hz.

[0030] As a technical solution of the present invention, the adjustable rolling pressure of the rolling press is 2T to 4T.

[0031] As a technical solution of the present invention, the external temperature of the roller press during rolling is 25±1° C., and the humidity is 40% to 60%.

[0032] As a technical solution of the present invention, the small electrode sheet and the empty copper foil are rolled twice in both positive and negative directions under different pressures, and then the thickness at the center is tested and the average value is taken.

[0033] As a technical solution of the present invention, the coating rate is 20 cm / s to 30 cm / s.

[0034] As a technical solution of the present invention, the thickness of the negative electrode slurry after coating is 170 μm to 280 μm.

[0035] As a technical solution of the present invention, the drying temperature is 80°C to 105°C.

[0036] As a technical solution of the present invention, the shape of the small pole piece includes circle or square.

[0037] As a technical solution of the present invention, the negative electrode sheet is cut and punched into 2 to 5 small round pieces with a radius of 5.5 mm to 7.0 mm in the area coated with the negative electrode slurry as the small electrode sheet.

[0038] As a technical solution of the present invention, the negative electrode sheet is cut and punched into 2 to 5 small round pieces with a radius of 5.5 mm to 7.0 mm in the area not coated with the negative electrode slurry as the copper foil.

[0039] As a technical solution of the present invention, the measurement is performed using a screw micrometer.

[0040] As a technical solution of the present invention, the heat treatment is carried out in a vacuum drying oven.

[0041] As a technical solution of the present invention, the temperature of the heat treatment is 80°C to 105°C.

[0042] As a technical solution of the present invention, the heat treatment time is 10 hours to 15 hours.

[0043] As a technical solution of the present invention, the cooling is performed at room temperature.

[0044] As a technical solution of the present invention, the cooling time is 20 minutes to 30 minutes.

[0045] The second aspect of the present invention provides a method for evaluating the compressive resistance of a silicon-based negative electrode material, wherein the compressive resistance of the silicon-based negative electrode material is tested by the aforementioned method for testing the compressive resistance of the silicon-based negative electrode material, and the P t The obtained compressive strength parameter P t To formulate the mass-to-gap ratio specifications of qualified silicon-based negative electrode materials, and then quickly evaluate the compressive resistance of silicon-based negative electrode materials, identify abnormal materials in advance, and avoid bad materials from flowing into the next process, thereby saving production costs and speeding up production and R&D progress. The compressive resistance evaluation of materials can guide the optimization of material formulations and process parameters. At the same time, it can help R&D personnel conduct failure analysis of lithium-ion battery materials.

[0046] As a technical solution of the present invention, if 1.84g / cm<P t ≤1.92g / cm, it means that the silicon-based negative electrode material has strong compressive resistance.

[0047] As a technical solution of the present invention, if 1.66g / cm ≤ P t ≤1.84g / cm, it means that the silicon-based negative electrode material has strong compressive resistance.

[0048] As a technical solution of the present invention, if P t <1.66 g / cm, it means that the compression resistance of the silicon-based negative electrode material is poor.

[0049] A third aspect of the present invention provides an application of a silicon-based negative electrode material, wherein the silicon-based negative electrode material having a very strong or relatively strong compressive resistance evaluated by the aforementioned method for evaluating the compressive resistance of silicon-based negative electrode materials is applied to the negative electrode.

[0050] A fourth aspect of the present invention provides a secondary battery comprising a positive electrode, a negative electrode and an electrolyte, wherein the negative electrode active material used in the negative electrode comprises the silicon-based negative electrode material having very strong or relatively strong compressive resistance evaluated by the aforementioned method for evaluating the compressive resistance of silicon-based negative electrode materials.

[0051] As a technical solution of the present invention, the negative electrode active material further includes a carbon material, and the mass ratio of the carbon material to the silicon-based negative electrode material is 0-89:11-100. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 These are the rebound curves of Examples 1 to 5. DETAILED DESCRIPTION

[0053] The present invention provides a method for detecting the compressive resistance of a silicon-based negative electrode material. The compressive resistance parameters of the silicon-based negative electrode material can be obtained by using the detection method. t ) can formulate the mass-to-gap ratio specification of qualified silicon-based negative electrode materials, and then quickly evaluate the compressive resistance of silicon-based negative electrode materials. The evaluation method of the compressive resistance of silicon-based negative electrode materials can be as follows.

[0054] (I) If 1.84 g / cm<P t ≤1.92g / cm, it means that the silicon-based negative electrode material has strong compressive resistance.

[0055] (II) If 1.66g / cm ≤ P t ≤1.84g / cm, it means that the silicon-based negative electrode material has strong compressive resistance.

[0056] (III) If P t <1.66g / cm, it means that the compression resistance of the silicon-based negative electrode material is poor.

[0057] Silicon-based negative electrode materials with strong or relatively strong compressive resistance can be used as negative electrode active materials and applied to negative electrodes and secondary batteries. Silicon-based negative electrode materials can be used alone as negative electrode active materials or mixed with carbon materials, and the mass ratio of carbon materials to silicon-based negative electrode materials is 0-89:11-100, and the mass ratio of the two can be but not limited to 0:100, 9:91, 19:81, 29:71, 39:61, 49:51, 59:41, 69:31, 79:21, 89:11. Carbon materials can be but not limited to one or more of artificial graphite, natural graphite, soft carbon and hard carbon.

[0058] The method for detecting the compressive resistance of the silicon-based negative electrode material of the present invention comprises steps (1), (2), (3) and (4).

[0059] Step (1) includes coating the negative electrode slurry on a hollow copper foil and drying to obtain a negative electrode sheet.

[0060] The negative electrode slurry includes a negative electrode active material, a binder, a conductive agent and a solvent. The sum of the mass of the negative electrode active material, the binder and the conductive agent is 100%. The mass proportion of the negative electrode active material is 92-95%, the mass proportion of the binder is 4-6%, and the mass proportion of the conductive agent is 4-7%. The mass proportion of the negative electrode active material can be, but is not limited to, 92%, 93%, 94%, and 95%. The negative electrode active material includes a carbon material and a silicon-based negative electrode material, and the mass ratio of the carbon material to the silicon-based negative electrode material is 0-89:11-100, and the mass ratio of the two can be, but is not limited to, 0:100, 9:91, 19:81, 29:71, 39:61, 49:51, 59:41, 69:31, 79:21, and 89:11. The carbon material can be, but is not limited to, one or more of artificial graphite, natural graphite, soft carbon, and hard carbon. The silicon-based negative electrode material includes at least one of elemental silicon, silicon oxide compounds, silicon carbon compounds, silicon alloy compounds, pre-magnesium silicon oxide compounds and pre-lithium silicon oxide compounds. The silicon carbon compound may be ground silicon carbon or gas phase silicon carbon. The mass proportion of the binder may be, but is not limited to, 4%, 5%, 6%. The binder includes carboxymethyl cellulose and / or styrene-butadiene rubber. The mass proportion of the conductive agent may be, but is not limited to, 4%, 5%, 6%, 7%, and the conductive agent includes at least one of conductive carbon black, conductive graphite, carbon nanotubes, graphene and vapor-grown carbon fiber. The solvent includes water, and the solid content of the negative electrode slurry is 30% to 50%. The solid content may be, but is not limited to, 30%, 35%, 40%, 45%, 50%.

[0061] When preparing the negative electrode slurry, first add part of the binder to the solvent and mix evenly, then add the conductive agent to mix to obtain a conductive glue, add the negative electrode active material to the conductive glue and mix, then add the remaining binder and stir evenly. The solvent is water, the binder is carboxymethyl cellulose and styrene-butadiene rubber, the conductive agent is conductive carbon black and conductive graphite, and the negative electrode active material takes silicon-based negative electrode material and artificial graphite as examples. The preparation steps of the negative electrode slurry may include but are not limited to: first weigh deionized water according to the formula amount, then add carboxymethyl cellulose to the water, use a high-speed disperser to stir at a speed of 1500rpm to 2000rpm for 3min to 10min, then transfer to a rotation degassing machine and stir at a speed of 800rpm to 860rpm for 0.5min to 2.0min, then adjust the speed to 1500rpm to 2500rpm, stir for 1min to 5min, and then stand for 10min to 20min to prepare a clear and transparent colloid, then add conductive carbon black to the colloid and stir at a speed of 4000rpm to 5000rpm for 25min to 35min, then add conductive graphite and continue to stir at a speed of 4000rpm to 5500rpm for 10min to 25min to prepare a conductive glue. Add silicon-based negative electrode material and artificial graphite to the conductive glue and stir at a speed of 400 rpm to 5500 rpm for 10 to 25 minutes, then add styrene-butadiene rubber and continue stirring at a speed of 1200 rpm to 2000 rpm for 4 to 6 minutes, stir the dispersed slurry at a speed of 1500 rpm to 2500 rpm in a rotary mixer for 10 to 20 minutes to obtain the negative electrode slurry.

[0062] The negative electrode slurry can be coated by a conventional coating machine, and the blank copper foil can be a conventional copper foil on the market. The coating rate is 20 cm / s to 30 cm / s, which can be but not limited to 20 cm / s, 21 cm / s, 22 cm / s, 23 cm / s, 24 cm / s, 25 cm / s, 26 cm / s, 27 cm / s, 28 cm / s, 29 cm / s, 30 cm / s. The thickness of the negative electrode slurry after coating is 170 μm to 280 μm, which can be but not limited to 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, 220 μm, 230 μm, 240 μm, 250 μm, 260 μm, 270 μm, 280 μm. The drying temperature is 80°C to 105°C, and may be, but is not limited to, 80°C, 85°C, 90°C, 95°C, 100°C, or 105°C.

[0063] Step (ii) includes rolling the negative electrode sheet under rolling pressure, and then taking the same area from the coating area and the blank area of ​​the negative electrode sheet as the small electrode sheet and the copper foil sheet. The thickness of the small electrode sheet and the blank copper foil at the center position are measured as d1 and d0 respectively. The rolling mass-gap ratio P corresponding to the rolling pressure is calculated, where m1 is the mass of the small electrode sheet and m0 is the mass of the copper foil sheet.

[0064]

[0065] Under a constant temperature and humidity environment, the dried electrode sheets can be cut into multiple sets of electrode sheets with a size of 2cm×12cm for standby use. Conventional automatic cutting machines or manual cutting knives can be used for cutting. The shapes of small electrode sheets include round or square. The negative electrode slurry coating is incomplete coating and is single-sided coating, that is, there are coated areas and uncoated areas on one side of the negative electrode sheet. 2 to 5 small discs with a radius of 5.5mm to 7.0mm can be punched out in the area coated with the negative electrode slurry as small electrode sheets. 2 to 5 small discs with a radius of 5.5mm to 7.0mm can be punched out in the area not coated with the negative electrode slurry (i.e., empty copper foil) as copper foil. Conventional automatic punching machines or manual punching machines can be used for punching.

[0066] Rolling is performed on a roller press. The speed of the roller press is 40 nm / s to 60 nm / s. The speed may be, but is not limited to, 40 nm / s, 45 nm / s, 50 nm / s, 55 nm / s, and 60 nm / s. The roller press has a rolling gap D between the two rollers at the start. o , 80μm≤D o <2000μm roller gap D o It can be, but is not limited to, 80 μm, 160 μm, 240 μm, 320 μm, 400 μm, 480 μm, 560 μm, 640 μm, 720 μm, 800 μm, 880 μm, 960 μm, 1040 μm, 1120 μm, 1200 μm, 1280 μm, 1360 μm, 1440 μm, 1520 μm, 1600 μm, 1680 μm, 1760 μm, 1840 μm, 1920 μm, 2000 μm, and the roller press can be adjusted with a roller gap of D a , 0≤D a ≤2000μmD aThe roller press gap between the two rollers of the roller press decreases in sequence from 2 μm to 15 μm to increase the roller pressure in sequence. The roller press gap may be, but is not limited to, 0 μm, 100 μm, 200 μm, 300 μm, 400 μm, 500 μm, 600 μm, 700 μm, 800 μm, 900 μm, 1000 μm, 1100 μm, 1200 μm, 1300 μm, 1400 μm, 1500 μm, 1600 μm, 1700 μm, 1800 μm, 1900 μm, and 2000 μm. The roller press gap between the two rollers of the roller press decreases in sequence from 2 μm to 15 μm to increase the roller pressure in sequence. The roller press gap may be, but is not limited to, 2 μm, 4 μm, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, and 15 μm. The roller press is preheated before rolling. The power of the roller press is 200W to 400W, and the power can be but not limited to 200W, 220W, 240W, 260W, 280W, 300W, 320W, 340W, 360W, 380W, 400W. The frequency of the roller press is 30Hz to 70Hz, and can be but not limited to 30Hz, 40Hz, 50Hz, 60Hz, 70Hz. The rolling pressure of the roller press is 2T to 4T, and the adjustable pressure of the roller press can be but not limited to 2T, 3T, 4T. The external temperature of the roller press during rolling is 25±1℃, and the humidity is 40% to 60%, and the humidity can be but not limited to 40%, 45%, 50%, 55%, 60%.

[0067] After the electrode is rolled twice under each pressure, the thickness of the electrode and the copper foil at the center is tested, and the number of measurements is 2 to 4 and the average value is taken. The measurement can be made using a screw micrometer or other precision measuring instruments.

[0068] Step (iii) includes heat treating the small pole piece and then cooling it, measuring the thickness d2 of the small pole piece at the center position after cooling, and calculating the rebound coefficient R.

[0069]

[0070] The heat treatment is carried out in a vacuum drying oven at a temperature of 80°C to 105°C for 10h to 15h. As an example, the temperature of the heat treatment may be, but is not limited to, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C. The time of the heat treatment may be, but is not limited to, 10h, 11h, 12h, 13h, 14h, 15h. Cooling is carried out at room temperature for 20min to 30min. As an example, the cooling time may be, but is not limited to, 20min, 21min, 22min, 23min, 24min, 25min, 26min, 27min, 28min, 29min, 30min.

[0071] Step (iv) includes increasing the rolling pressure in sequence until a wave shape appears on both sides of the negative electrode sheet, and obtaining the rolling mass-gap ratio P and the rebound coefficient R corresponding to each rolling pressure. The rebound curve is established with the rolling mass-gap ratio P as the horizontal coordinate and the corresponding rebound coefficient R as the vertical coordinate. t The corresponding P t It is the compressive resistance parameter of silicon-based negative electrode materials, R t It is the maximum rebound coefficient of the rebound curve at the inflection point. When the rebound coefficient gradually reaches the maximum inflection point, it means that the critical pressure of the silicon-based negative electrode material is exceeded, the silicon-based negative electrode material begins to deform and break, and then the elasticity decreases. The silicon-based negative electrode material gradually changes from elastic deformation to plastic deformation near this mass-gap ratio, and the actual compressive resistance of the material can be judged in turn.

[0072] In order to better illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that the following implementation method is a further explanation of the present invention and should not be used as a limitation of the present invention.

[0073] Example 1

[0074] This embodiment is a method for testing the compressive resistance of silicon-based negative electrode materials. The testing method includes the following steps.

[0075] (i) Weigh 214.000 g of pure water, add 2.000 g of carboxymethyl cellulose to the pure water, stir with a high-speed disperser at 2000 rpm for 5 min, then transfer to a rotary degassing machine and stir at 850 rpm for 1 min, then adjust the speed to 2000 rpm and stir for 1 min and let stand for 3 min to obtain a clear and transparent colloid, then add 2.000 g of conductive carbon black to the colloid, stir at 5000 rpm for 30 min, then add 2.000 g of conductive graphite, and continue to stir at 5000 rpm for 15 min to obtain a conductive adhesive. Weigh 44.000g of the above-mentioned conductive glue, add 2.024g of spherical ground silicon and 16.376g of artificial graphite, stir at 5000rpm for 15min, add 0.80g of styrene-butadiene rubber, continue stirring at 1500rpm for 5min, then pour into a 100mL stirring cup, stir in a rotary mixer at 2000rpm for 15min to obtain the negative electrode slurry. Adjust the speed of the coater to 25cm / s, lay the empty copper foil on the coater, turn on the vacuum pump of the coater, put a 250μm coater at one end of the copper foil, evenly apply the dispersed negative electrode slurry on the inside of the coater, turn on the coater for coating, move the coated electrode to a glass slide wiped clean with alcohol, and then place it in a blast oven at 100℃ for 3h to obtain the negative electrode.

[0076] (ii) Use a paper cutter to cut out multiple groups of 2cm×12cm negative electrode sheets for standby use. Set the speed of the roller press to 50nm / s, the rolling gap between the two rollers to 83μm at the start, the power to 300W, the frequency to 50Hz, the rolling pressure to 3T, the external temperature during rolling to 25±1℃, and the humidity to 50%. After preheating the roller press for 5min, roll the electrode sheets. After rolling twice in both positive and negative directions, use a manual punching machine to cut out 3 small discs with a radius of 6mm in the coated area and the uncoated area from different positions of each group of electrode sheets, respectively, as small electrode sheets and copper foil sheets. Use a spiral micrometer to measure the thickness of each small electrode sheet and each empty copper foil at the center position as d1 and d0, and measure each 3 times and take the average of 9 times. Weigh the 3 small electrode sheets and 3 copper foil sheets respectively and take the average value, which is recorded as m1 and m0. Then calculate the roller pressure mass-gap ratio P corresponding to the roller pressure.

[0077] (III) Dry the three small electrodes in a vacuum tube drying oven at 100°C for 12 hours. After vacuum drying, take out the small electrodes and cool them for 25 minutes. Measure the thickness d2 of each small electrode at the center position. Measure each electrode 3 times and take the average of 9 times to calculate the rebound coefficient R.

[0078] (IV) The rolling gap between the upper and lower rollers of the roller press is reduced in steps of 5 μm, and the other pole pieces in step (II) are rolled at each rolling pressure until a wave shape appears on both sides of the pole piece and vertical lines are damaged on the surface of the pole piece. The rolling mass gap ratio P and the rebound coefficient R corresponding to the different rolling pressures are obtained. The mass gap ratios are 1.02 g / cm, 1.36 g / cm, and 1.53 g / cm, respectively. g / cm, 1.70g / cm, 1.75g / cm, 1.90g / cm, 2.00g / cm, 2.01g / cm, 2.02g / cm, the rebound coefficients are 0.01%, 2.00%, 2.70%, 3.10%, 3.30%, 3.90%, 3.10%, 3.09%, 3.09% respectively. The rebound curve is established with the roller mass gap ratio P as the horizontal coordinate and the corresponding rebound coefficient R as the vertical coordinate. The curve is as shown in the figure. Figure 1 shown.

[0079] Example 2

[0080] This embodiment is a method for testing the compressive resistance of silicon-based negative electrode materials. The testing method includes the following steps.

[0081] Weigh 285.000g of pure water, add 2.66g of carboxymethyl cellulose to the pure water, stir with a high-speed disperser at 2500rpm for 5min, then transfer to a rotation and revolution degassing machine and stir at 950rpm for 1min, then adjust the speed to 2000rpm and stir for 1min and let it stand for 3min to obtain a clear and transparent colloid, then add 2.630g of conductive carbon black to the colloid, stir at 5000rpm for 30min, then add 2.760g of conductive graphite, and continue to stir at 5000rpm for 15min to obtain a conductive adhesive. Weigh 44.000g of the above-mentioned conductive glue, add 2.034g of dimple-shaped ground silicon and 16.366g of artificial graphite, stir at 5000rpm for 15min, add 0.80g of styrene-butadiene rubber, continue stirring at 1500rpm for 5min, then pour into a 100mL stirring cup, stir in a self-rotating and revolving mixer at 2000rpm for 15min to obtain the negative electrode slurry. Adjust the speed of the coater to 25cm / s, lay the empty copper foil on the coater, turn on the vacuum pump of the coater, put a 250μm coater on one end of the copper foil, apply the dispersed negative electrode slurry evenly on the inside of the coater, turn on the coater for coating, move the coated electrode to a glass slide wiped clean with alcohol, and then place it in a blast oven at 100℃ for 3h to obtain the negative electrode.

[0082] (ii) Use a paper cutter to cut out multiple groups of 2cm×12cm negative electrode sheets for standby use. Set the speed of the roller press to 50nm / s, the rolling gap between the two rollers to 85μm at the start, the power to 300W, the frequency to 50Hz, the rolling pressure to 3T, the external temperature during rolling to 25±1℃, and the humidity to 50%. After preheating the roller press for 5min, roll the three small electrode sheets and the three copper foil sheets. After rolling twice in both positive and negative directions, use a manual punching machine to cut out three small discs with a radius of 6mm in the coated area and the uncoated area from different positions of each group of electrode sheets, respectively, as small electrode sheets and copper foil sheets. Use a spiral micrometer to measure the thickness of each small electrode sheet and each empty copper foil at the center position as d1 and d0, and each measurement is performed 3 times and the average value of 9 times is taken. The three small electrode sheets and the three copper foil sheets are weighed and the average value is taken, recorded as m1 and m0. Then calculate the roller pressure mass-gap ratio P corresponding to the roller pressure.

[0083] (III) Dry the three small electrodes in a vacuum tube drying oven at 100°C for 12 hours. After vacuum drying, take out the small electrodes and cool them for 25 minutes. Measure the thickness d2 of each small electrode at the center position. Measure each electrode 3 times and take the average of 9 times to calculate the rebound coefficient R.

[0084] (IV) The rolling gap between the upper and lower rollers of the roller press is reduced in increments of 5 μm, and the other pole pieces in step (II) are rolled at each rolling pressure until a wave shape appears on both sides of the pole piece and vertical lines are damaged on the surface of the pole piece. The rolling mass gap ratio P and rebound coefficient R corresponding to different rolling pressures are obtained, and the mass gap ratios are 1.03 g / cm, 1.24 g / cm, 1.37 g / cm, 1.61 g / cm, 1.71 g / cm, 1.83 g / cm, 1.98 g / cm, 2.00 g / cm, and 2.01 g / cm, respectively, and the rebound coefficients are 0.10%, 1.40%, 1.90%, 2.98%, 3.50%, 4.10%, 3.10%, 3.09%, and 3.08%, respectively. The rebound curve is established with the roller pressure mass-gap ratio P as the horizontal coordinate and the corresponding rebound coefficient R as the vertical coordinate. Figure 1 shown.

[0085] Example 3

[0086] This embodiment is a method for testing the compressive resistance of silicon-based negative electrode materials. The testing method includes the following steps.

[0087] (i) Weigh 214.000 g of pure water, add 2.000 g of carboxymethyl cellulose to the pure water, stir with a high-speed disperser at 2000 rpm for 5 min, then transfer to a rotary degassing machine and stir at 850 rpm for 1 min, then adjust the speed to 2000 rpm and stir for 1 min and let stand for 3 min to obtain a clear and transparent colloid, then add 2.000 g of conductive carbon black to the colloid, stir at 5000 rpm for 30 min, then add 2.000 g of conductive graphite, and continue to stir at 5000 rpm for 15 min to obtain a conductive adhesive. Weigh 44.000g of the above-mentioned conductive glue, add 2.024g of round-ground silicon and 16.376g of artificial graphite, stir at 5000rpm for 15min, add 0.80g of styrene-butadiene rubber, continue stirring at 1500rpm for 5min, then pour into a 100mL stirring cup, stir in a rotary mixer at 2500rpm for 15min to obtain the negative electrode slurry. Adjust the speed of the coater to 28cm / s, lay the empty copper foil on the coater, turn on the vacuum pump of the coater, put the 220μm coater at one end of the copper foil, evenly apply the dispersed negative electrode slurry on the inside of the coater, turn on the coater for coating, move the coated electrode to a glass slide wiped clean with alcohol, and then place it in a blast oven at 95℃ for 5h to obtain the negative electrode.

[0088] (ii) Use a paper cutter to cut out multiple groups of 2cm×12cm negative electrode sheets for standby use. Set the speed of the roller press to 50nm / s, the rolling gap between the two rollers to 82μm at the start, the power to 300W, the frequency to 50Hz, the rolling pressure to 3T, the external temperature during rolling to 25±1℃, and the humidity to 50%. After preheating the roller press for 5min, roll the three small electrode sheets and the three copper foil sheets. After rolling twice in both positive and negative directions, use a manual punching machine to cut out three small discs with a radius of 6mm in the coated area and the uncoated area from different positions of each group of electrode sheets, respectively, as small electrode sheets and copper foil sheets. Use a spiral micrometer to measure the thickness of each small electrode sheet and each empty copper foil at the center position as d1 and d0, and each measurement is performed 3 times and the average value of 9 times is taken. The three small electrode sheets and the three copper foil sheets are weighed and the average value is taken, recorded as m1 and m0. , and then calculate the roller pressure mass-gap ratio P corresponding to the roller pressure.

[0089] (III) Dry the three small electrodes in a vacuum tube drying oven at 100°C for 12 hours. After vacuum drying, take out the small electrodes and cool them for 25 minutes. Measure the thickness d2 of each small electrode at the center position. Measure each electrode 3 times and take the average of 9 times to calculate the rebound coefficient R.

[0090] (IV) The rolling gap between the upper and lower rollers of the roller press is reduced in increments of 5 μm. The other pole pieces in step (II) are rolled at each rolling pressure until waves appear on both sides of the pole piece and vertical lines and damage appear on the surface of the pole piece. The rolling mass gap ratio P and rebound coefficient R corresponding to the different rolling pressures are obtained. The mass gap ratios are 1.02 g / cm, 1.24 g / cm, 1.41 g / cm, 1.57 g / cm, 1.70 g / cm, 1.81 g / cm, and 1.98 g / cm, respectively. The rebound coefficients are 0.01%, 3.20%, 4.50%, 5.90%, 6.50%, 5.34%, and 5.30%, respectively. A rebound curve is established with the rolling mass gap ratio P as the horizontal coordinate and the corresponding rebound coefficient R as the vertical coordinate. The curve is as shown in FIG. Figure 1 shown.

[0091] Example 4

[0092] This embodiment is a method for testing the compressive resistance of silicon-based negative electrode materials. The testing method includes the following steps.

[0093] (i) Weigh 214.000 g of pure water, add 2.000 g of carboxymethyl cellulose to the pure water, stir with a high-speed disperser at 2000 rpm for 5 min, then transfer to a rotary degassing machine and stir at 850 rpm for 1 min, then adjust the speed to 2000 rpm and stir for 1 min and let stand for 3 min to obtain a clear and transparent colloid, then add 2.000 g of conductive carbon black to the colloid, stir at 5000 rpm for 30 min, then add 2.000 g of conductive graphite, and continue to stir at 5000 rpm for 15 min to obtain a conductive adhesive. Weigh 44.000g of the above-mentioned conductive glue, add 2.024g of irregular fumed silicon and 16.376g of artificial graphite, stir at 5000rpm for 15min, add 0.80g of styrene-butadiene rubber, continue stirring at 1500rpm for 5min, then pour into a 100mL stirring cup, stir in a self-rotating and revolving mixer at 2000rpm for 15min to obtain the negative electrode slurry. Adjust the speed of the coater to 25cm / s, lay the empty copper foil on the coater, turn on the vacuum pump of the coater, put a 250μm coater at one end of the copper foil, evenly apply the dispersed negative electrode slurry on the inside of the coater, turn on the coater for coating, move the coated electrode to a glass slide wiped clean with alcohol, and then place it in a blast oven at 100℃ for 3h to obtain the negative electrode.

[0094] (ii) Use a paper cutter to cut the negative electrode sheets into multiple groups of sheets with a specification of 2cm×12cm for standby use. Set the speed of the roller press to 55nm / s, the rolling gap between the two rollers at the beginning to 80μm, the power to 400W, the frequency to 60Hz, the rolling pressure to 4T, the external temperature during rolling to 25±1℃, and the humidity to 50%. After preheating the roller press for 5min, roll the three small electrode sheets and the three copper foil sheets. After rolling twice in both the positive and negative directions, use a manual punching machine to cut out three small discs with a radius of 6.5mm in the coated area and the uncoated area from different positions of each group of electrode sheets, as the small electrode sheets and the copper foil sheets, respectively. A screw micrometer was used to measure the thickness of each small pole piece and each empty copper foil at the center as d1 and d0, and each measurement was performed 3 times and the average value of 9 times was taken. The three small pole pieces and three copper foils were weighed respectively and the average value was taken, recorded as m1 and m0, and then the rolling mass-gap ratio P corresponding to the rolling pressure was calculated.

[0095] (III) Dry the three small electrodes in a vacuum tube drying oven at 100°C for 12 hours. After vacuum drying, take out the small electrodes and cool them for 25 minutes. Measure the thickness d2 of each small electrode at the center position. Measure each electrode 3 times and take the average of 9 times to calculate the rebound coefficient R.

[0096] (IV) The rolling gap between the upper and lower rollers of the roller press is reduced in increments of 5 μm. The other pole pieces in step (II) are rolled at each rolling pressure until waves appear on both sides of the pole piece and vertical lines and damage appear on the surface of the pole piece. The rolling mass gap ratio P and rebound coefficient R corresponding to the different rolling pressures are obtained. The mass gap ratios are 1.03 g / cm, 1.30 g / cm, 1.37 g / cm, 1.58 g / cm, 1.72 g / cm, 1.84 g / cm, and 1.96 g / cm, respectively. The rebound coefficients are 0.03%, 3.00%, 4.00%, 6.30%, 5.50%, 4.80%, and 4.71%, respectively. A rebound curve is established with the rolling mass gap ratio P as the horizontal coordinate and the corresponding rebound coefficient R as the vertical coordinate. The curve is as shown in FIG. Figure 1 shown.

[0097] Example 5

[0098] This embodiment is a method for testing the compressive resistance of silicon-based negative electrode materials. The testing method includes the following steps.

[0099] (i) Weigh 214.000 g of pure water, add 2.000 g of carboxymethyl cellulose to the pure water, stir with a high-speed disperser at 2000 rpm for 5 min, then transfer to a rotary degassing machine and stir at 850 rpm for 1 min, then adjust the speed to 2000 rpm and stir for 1 min and let stand for 3 min to obtain a clear and transparent colloid, then add 2.000 g of conductive carbon black to the colloid, stir at 5000 rpm for 30 min, then add 2.000 g of conductive graphite, and continue to stir at 5000 rpm for 15 min to obtain a conductive adhesive. Weigh 44.000g of the above-mentioned conductive glue, add 2.024g of porous fumed silicon and 16.376g of artificial graphite, stir at 5000rpm for 15min, add 0.80g of styrene-butadiene rubber, continue stirring at 1500rpm for 5min, then pour into a 100mL stirring cup, stir in a rotary mixer at 2000rpm for 15min to obtain the negative electrode slurry. Adjust the speed of the coater to 25cm / s, lay the empty copper foil on the coater, turn on the vacuum pump of the coater, put a 250μm coater at one end of the copper foil, apply the dispersed negative electrode slurry evenly on the inside of the coater, turn on the coater for coating, move the coated electrode to a glass slide wiped clean with alcohol, and then place it in a blast oven at 100℃ for 3h to obtain the negative electrode.

[0100] (ii) Use a paper cutter to cut out multiple groups of 2cm×12cm negative electrode sheets for standby use. Set the speed of the roller press to 50nm / s, the rolling gap between the two rollers to 82μm at the start, the power to 300W, the frequency to 50Hz, the rolling pressure to 3T, the external temperature during rolling to 25±1℃, and the humidity to 50%. After preheating the roller press for 5min, roll the three small electrode sheets and the three copper foil sheets. After rolling twice in both positive and negative directions, use a manual punching machine to cut out three small discs with a radius of 6mm in the coated area and the uncoated area from different positions of each group of electrode sheets, respectively, as small electrode sheets and copper foil sheets. Use a spiral micrometer to measure the thickness of each small electrode sheet and each empty copper foil at the center position as d1 and d0, and each measurement is performed 3 times and the average value of 9 times is taken. The three small electrode sheets and the three copper foil sheets are weighed and the average value is taken, recorded as m1 and m0. Then calculate the roller pressure mass-gap ratio P corresponding to the roller pressure.

[0101] (III) Dry the three small electrodes in a vacuum tube drying oven at 100°C for 14 hours. After vacuum drying, take out the small electrodes and cool them for 30 minutes. Measure the thickness d2 of each small electrode at the center position. Measure each electrode 3 times and take the average of 9 times to calculate the rebound coefficient R.

[0102] (IV) The rolling gap between the upper and lower rollers of the roller press is reduced in increments of 6 μm. The other pole pieces in step (II) are rolled at each rolling pressure until waves appear on both sides of the pole piece and vertical lines and damage appear on the surface of the pole piece. The rolling mass gap ratio P and rebound coefficient R corresponding to the different rolling pressures are obtained. The mass gap ratios are 1.03 g / cm, 1.25 g / cm, 1.30 g / cm, 1.51 g / cm, 1.61 g / cm, 1.73 g / cm, and 1.84 g / cm, respectively. The rebound coefficients are 0.01%, 2.99%, 3.45%, 6.00%, 5.45%, 4.90%, and 4.86%, respectively. A rebound curve is established with the rolling mass gap ratio P as the horizontal coordinate and the corresponding rebound coefficient R as the vertical coordinate. The curve is as shown in FIG. Figure 1 shown.

[0103] Depend on Figure 1From the results, it can be seen that the pole piece mass-gap ratio corresponding to the highest inflection point of the coefficient of rebound of the spherical ground silicon material in Example 1 is 1.88g / cm to 1.92g / cm. The pole piece mass-gap ratio corresponding to the highest inflection point of the coefficient of rebound of the dimple-shaped ground silicon material in Example 2 is 1.80g / cm to 1.84g / cm. The pole piece mass-gap ratio corresponding to the highest inflection point of the coefficient of rebound of the quasi-circular ground silicon material in Example 3 is 1.66g / cm to 1.70g / cm. The pole piece mass-gap ratio corresponding to the highest inflection point of the coefficient of rebound of the irregular gas phase silicon material in Example 4 is 1.58g / cm to 1.62g / cm. The pole piece mass-gap ratio corresponding to the highest inflection point of the coefficient of rebound of the porous gas phase silicon material in Example 5 is 1.50g / cm to 1.54g / cm. It shows that the pole piece mass gap corresponding to the inflection point of the coefficient of rebound of Examples 1 to 5 gradually decreases, and its compressive resistance gradually deteriorates.

[0104] In order to further verify the rationality of the method for detecting the compressive resistance of the silicon-based negative electrode material of the present invention, the silicon-based negative electrode materials in Examples 1 to 5 were used as negative electrode active materials to make button batteries for electrochemical performance testing. The test conditions are as follows and the test results are shown in Table 1.

[0105] (I) First charge and discharge performance test: The silicon materials tested in Examples 1 to 5 were used as active materials, mixed with binder polyvinylidene fluoride and conductive agent (Super-P) in a mass ratio of 70:15:15, and an appropriate amount of N-methylpyrrolidone (NMP) was added as a solvent to prepare a slurry, which was coated on a copper foil, and vacuum dried and rolled to prepare a negative electrode sheet. A metal lithium sheet was used as a counter electrode, 1 mol / L LiPF6 and a three-component mixed solvent of EC:DMC:EMC=1:1:1 (v / v / v) were used to form an electrolyte, a polypropylene microporous membrane was used as a diaphragm, and a CR2032 button cell was assembled in a glove box filled with inert gas. The charge and discharge test of the button cell was carried out on the LANHE battery test system of Landian Electronics Co., Ltd. At room temperature, the battery is discharged at a constant current of 0.1C to a voltage of 0.01V, then discharged at a constant current of 0.02C to a voltage of 0.01V, and charged at a constant current of 0.1C to a voltage of 1.5V. The capacities charged and discharged to 1.5V are the first charge capacity and the first discharge capacity, respectively, and the ratio of the first charge capacity to the first discharge capacity is the first coulomb efficiency.

[0106] (II) Cycle performance test: The negative electrode active material containing silicon material detected in Examples 1 to 5 is mixed with the aqueous dispersion of binder carboxymethyl cellulose (CMC, solid content 50%), conductive agent (SuperP), conductive graphite, and styrene-butadiene rubber (SBR) in a mass ratio of 93:2:1:2:2, and an appropriate amount of water is added as a solvent to form a slurry, which is coated on a copper foil, and vacuum dried and rolled to prepare a negative electrode sheet. Using metallic lithium as the counter electrode, using a 1 mol / L LiPF6 three-component mixed solvent and an electrolyte mixed according to EC:DMC:EMC=1:1:1 (volume ratio), using a polypropylene microporous membrane as a diaphragm, and assembling a CR2032 button cell with a capacity of 500mAh / g in a glove box filled with inert gas. The charge and discharge test of the button cell was carried out on the battery test equipment system of Blue Electric Electronics Co., Ltd., at room temperature, 0.2C constant current charge and discharge, and the charge and discharge voltage was limited to 0.01V~1.5V. Record the reversible capacity of the first week. Then, the battery was charged and discharged at a constant current of 0.5C, and the charge and discharge voltage was limited to 0.01V ~ 1.5V. After 50 cycles, the thickness of the negative electrode at the beginning and after 50 cycles was tested, and the full-charge expansion rate after 50 cycles and the reversible capacity retention rate after 50 cycles were calculated.

[0107] Table 1 Electrochemical performance test results

[0108]

[0109] The results in Table 1 show that the electrochemical properties of the silicon-based negative electrode materials tested in Examples 1 to 5 are used as negative electrode active materials in lithium-ion batteries. The electrochemical properties are as follows: Example 1 is better, Example 2 is second, Example 3 is in the middle, Example 4 is slightly inferior, and Example 5 is slightly worse. Therefore, the compressive performance of the silicon-based negative electrode material is consistent with the overall trend of the electrochemical performance.

[0110] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for detecting the compressive resistance of a silicon-based negative electrode material, characterized in that: include: (1) coating a negative electrode slurry on a hollow copper foil and drying the negative electrode sheet, wherein the negative electrode slurry comprises a negative electrode active material, and the negative electrode active material comprises at least a silicon-based negative electrode material; (ii) rolling the negative electrode sheet under rolling pressure, taking the same area from the coating area and the blank area of ​​the negative electrode sheet as the small electrode sheet and the copper foil sheet, measuring the thickness of the small electrode sheet and the blank copper foil at the center as d1 and d0, respectively, and calculating the rolling mass-gap ratio P corresponding to the rolling pressure, wherein m1 is the mass of the small electrode sheet, m0 is the mass of the copper foil sheet, (iii) heat treating the small pole piece and then cooling it, measuring the thickness d2 of the small pole piece at the center after cooling, and calculating the rebound coefficient R, (iv) increasing the rolling pressure successively until a wave shape appears on both sides of the negative electrode sheet, obtaining the rolling mass-gap ratio P and the rebound coefficient R corresponding to each rolling pressure, and establishing a rebound curve with the rolling mass-gap ratio P as the abscissa and the corresponding rebound coefficient R as the ordinate. The rebound curve has R t The corresponding P t is the compressive strength parameter of the silicon-based negative electrode material, and the R t is the maximum rebound coefficient of the rebound curve at the inflection point.

2. The method for detecting the compressive resistance of silicon-based negative electrode materials according to claim 1, characterized in that: The negative electrode slurry includes a negative electrode active material, a binder, a conductive agent and a solvent.

3. The method for detecting the compressive resistance of silicon-based negative electrode materials according to claim 2, characterized in that: Includes at least one of the following features ① to ⑧: ① Taking the sum of the mass of the negative electrode active material, the binder and the conductive agent as 100%, the mass of the negative electrode active material accounts for 92-95%, the mass of the binder accounts for 4-6%, and the mass of the conductive agent accounts for 4-7%; ② The negative electrode active material includes a carbon material and a silicon-based negative electrode material, and the mass ratio of the carbon material to the silicon-based negative electrode material is 0-89:11-100; ③ The silicon-based negative electrode material includes at least one of elemental silicon, silicon oxide compounds, silicon carbon compounds, silicon alloy compounds, pre-magnesium silicon oxide compounds and pre-lithium silicon oxide compounds; ④ The binder includes carboxymethyl cellulose and / or styrene-butadiene rubber; ⑤ The conductive agent includes at least one of conductive carbon black, conductive graphite, carbon nanotubes, graphene and vapor-grown carbon fiber; ⑥ The solvent includes water; ⑦ When preparing the negative electrode slurry, first add part of the binder to the solvent and mix evenly, then add the conductive agent to mix to obtain a conductive glue, add the negative electrode active material to the conductive glue, then add the remaining binder and stir evenly; ⑧The solid content of the negative electrode slurry is 30% to 50%.

4. The method for detecting the compressive resistance of silicon-based negative electrode materials according to claim 1, characterized in that: The rolling is performed under a roller press.

5. The method for detecting the compressive resistance of silicon-based negative electrode materials according to claim 4, characterized in that: The invention comprises at least one of the following features (I) to (X): (I) the rotation speed of the roller press is 40 nm / s to 60 nm / s; (II) The roller press has a roller gap D between the two rollers at the start. o , 80μm≤D o <2000μm; (III) The adjustable roller pressing gap of the roller press is D a , 0μm≤D a ≤2000μm; (IV) the rolling gap between the two rollers of the roller press is reduced in sequence by 2 μm to 15 μm so as to increase the rolling pressure in sequence; (V) the roller press is preheated before the roller press operation is performed; (VI) the power of the roller press is 200W to 400W; (VII) the frequency of the roller press is 30 Hz to 70 Hz; (VIII) the adjustable rolling pressure of the rolling press is 2T to 4T; (IX) The external temperature of the roller press during rolling is 25±1° C. and the humidity is 40% to 60%; (X) The thickness of the small electrode at the center is tested after rolling twice in both forward and reverse directions under different pressures, and the average value is taken.

6. The method for detecting the compressive resistance of silicon-based negative electrode materials according to claim 1, characterized in that: The invention comprises at least one of the following features (1) to (12): (1) The coating rate is 20 cm / s to 30 cm / s; (2) The thickness of the negative electrode slurry after coating is 170 μm to 280 μm; (3) The drying temperature is 80°C to 105°C; (4) The shape of the small pole piece includes a circle or a square; (5) The negative electrode sheet is cut and punched into 2 to 5 small discs with a radius of 5.5 mm to 7.0 mm in the area coated with the negative electrode slurry as the small electrode sheet; (6) The negative electrode sheet is cut and punched into 2 to 5 small discs with a radius of 5.5 mm to 7.0 mm in the area not coated with the negative electrode slurry as the copper foil; (7) The measurement is performed using a micrometer screw; (8) The heat treatment is carried out in a vacuum drying oven; (9) The temperature of the heat treatment is 80°C to 105°C; (10) The heat treatment time is 10 to 15 hours; (11) The cooling is carried out at room temperature; (12) The cooling time is 20 min to 30 min.

7. A method for evaluating the compressive resistance of silicon-based negative electrode materials, characterized in that: The compression resistance of the silicon-based negative electrode material is tested by the method for testing the compression resistance of the silicon-based negative electrode material according to any one of claims 1 to 6, and the P t , (I) If 1.84 g / cm<P t ≤1.92g / cm, it means that the silicon-based negative electrode material has strong compressive resistance; (II) If 1.66g / cm ≤ P t ≤1.84g / cm, it means that the silicon-based negative electrode material has strong compressive resistance; (III) If P t <1.66 g / cm, it means that the compression resistance of the silicon-based negative electrode material is poor.

8. An application of a silicon-based negative electrode material, characterized in that: The silicon-based negative electrode material having very strong or relatively strong compression resistance evaluated by the method for evaluating the compression resistance of silicon-based negative electrode materials according to claim 7 is used in the negative electrode.

9. A secondary battery, characterized in that: The invention comprises a positive electrode, a negative electrode and an electrolyte, wherein the negative electrode active material used in the negative electrode comprises the silicon-based negative electrode material having very strong or relatively strong compression resistance evaluated by the method for evaluating the compression resistance of silicon-based negative electrode materials according to claim 7.

10. The secondary battery according to claim 9, characterized in that: The negative electrode active material further includes a carbon material, and the mass ratio of the carbon material to the silicon-based negative electrode material is 0-89:11-100.