Method for detecting water absorption capacity of titanium dioxide

By detecting the water absorption of titanium dioxide and optimizing its production process, the problem of lack of detection standards in the existing technology has been solved, the performance of titanium dioxide in water-based coatings and plastics has been improved, and better dispersing performance and application effects have been achieved.

CN118913989APending Publication Date: 2024-11-08CHONGQING VANADIUM TITANIUM TECH CO LTD OF PANGANG GRP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411145007.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art lacks effective detection methods and standards to measure the water absorption of titanium dioxide, which affects its performance and application effect in aqueous coating systems.

Method used

By insulating the titanium dioxide sample in the oven and cooling it, forming a titanium dioxide solution and filtration and drying, the weight difference of the filter cake is calculated to determine the water absorption, and multiple parallel measurements are used to reduce the error to ensure the experimental data Accuracy and repeatability.

Benefits of technology

Optimized the production process of titanium dioxide, improved its dispersion performance in water, improved the hiding power of the paint and the color of the plastic, significantly enhanced its compatibility and operability in the water-based system, and met the market's high-quality products need.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118913989A_ABST
    Figure CN118913989A_ABST
Patent Text Reader

Abstract

The invention discloses a method for detecting the water absorption capacity of titanium dioxide. The method comprises the following steps: S1, carrying out heat preservation on a titanium dioxide sample to be detected in a drying oven, putting the titanium dioxide sample in a dryer, and cooling the titanium dioxide sample to room temperature; s2, putting a titanium dioxide sample to be detected into a clean beaker, dropwise adding pure water, stirring and mixing until a titanium dioxide solution is formed, and standing for 0.5-1 hour; s3, carrying out suction filtration on the titanium dioxide solution, and weighing an obtained filter cake and recording as M1; and S4, drying the filter cake in a drying oven, weighing the dried filter cake, recording as M2, and enabling the water absorption capacity to be equal to M1-M2. By detecting the water absorption capacity, the production process of the titanium dioxide can be optimized, and the water absorption capacity is more reasonable, so that the dispersion performance of the titanium dioxide in water is improved, and the application effects of the titanium dioxide serving as pigment and filler products of important sources, such as improvement of the covering power of a coating and improvement of the color and luster of plastics, are also favorably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of conventional performance detection of titanium dioxide, and in particular to a method for detecting the water absorption of titanium dioxide. Background Art

[0002] In the routine testing of titanium dioxide, one of the most common important indicators is oil absorption, which refers to the minimum mass of oil required for 100g of titanium dioxide to achieve complete wetting. It is one of the important pigment properties of titanium dioxide, which involves the filling state of titanium dioxide in the color developer and can explain its dispersion performance in the medium. However, the conventional testing indicator of water absorption for water-based coating system products has not yet been established.

[0003] Dispersibility is an important indicator that titanium dioxide and other pigment manufacturers are primarily concerned about. No matter how excellent the pigment is, if it does not have excellent dispersibility as a prerequisite, its effectiveness will be greatly reduced. Generally speaking, the lower the water absorption of titanium dioxide, the better its pigment and application performance. Therefore, the amount of water absorption of titanium dioxide also affects its water dispersibility. When titanium dioxide absorbs more water, it combines with the hydroxyl groups on the surface, weakening the surface electronegativity, weakening the high dispersibility in the two phases, and reducing the dispersion stability. As for the water absorption detection of titanium dioxide, there is no relevant national standard, nor a systematic detection method.

[0004] The significance of pigment water absorption is to determine the minimum amount of water used when grinding the pigment, that is, the minimum amount of water required to completely soak 100g of pigment. Water absorption reflects the application performance of titanium dioxide in water-based latex paint. It is an important reference data for the selection and formulation of water-based paint systems. If the water absorption in the paint is high or low, it will affect the PVC value, viscosity, drying speed and other application indicators of the system. Especially in some high PVC paints, the selection and determination of the formula must strictly control the water absorption of the pigment.

[0005] In view of this, in order to improve work efficiency and shorten the detection cycle, improvements should be made to the existing technology. Summary of the invention

[0006] The main purpose of the present invention is to provide a method for detecting the water absorption of titanium dioxide. By detecting the water absorption, the production process of titanium dioxide can be optimized to make its water absorption more reasonable, thereby improving its dispersion performance in water. It is also helpful to improve the application effect of products in which titanium dioxide is an important source of pigments and fillers, such as improving the hiding power of coatings and improving the color of plastics.

[0007] According to one aspect of the present invention, a method for detecting water absorption of titanium dioxide is provided, which comprises the following steps: S1. Keep the titanium dioxide sample to be tested warm in an oven and then place it in a desiccator to cool to room temperature; S2. Place the titanium dioxide sample to be tested in a clean beaker, add pure water and stir to mix until a titanium dioxide solution is formed, and let it stand for 0.5~1h; S3, filtering the titanium dioxide solution, and weighing the obtained filter cake and recording it as M1; S4. Dry the filter cake in an oven, weigh the dried filter cake and record it as M2. Water absorption = M1-M2.

[0008] According to one embodiment of the present invention, in steps S1 and S4, the temperature of the oven is 100-110°C.

[0009] According to an embodiment of the present invention, the method requires performing multiple parallel measurements to reduce errors.

[0010] According to one embodiment of the present invention, in step S1, the insulation time is 1 to 3 hours.

[0011] According to one embodiment of the present invention, in step S4, the drying time is 1 to 3 hours.

[0012] According to one embodiment of the present invention, the filtration includes pouring the titanium dioxide solution into a filtration funnel of a vacuum pump for filtration.

[0013] According to one embodiment of the present invention, the suction filtration includes pumping the titanium dioxide solution to the bottom of the suction filtration funnel until no water drips.

[0014] According to an embodiment of the present invention, in step S2, stirring includes stirring fully with a glass rod at a stirring speed of 2 to 3 revolutions per second, and stirring evenly within 1 to 2 minutes.

[0015] According to one embodiment of the present invention, the amount of the titanium dioxide sample to be tested is less than 100 g.

[0016] According to one embodiment of the present invention, the amount of the titanium dioxide sample to be tested ranges from 10 to 20 g.

[0017] In a method for detecting the water absorption of titanium dioxide according to an embodiment of the present invention, by detecting the water absorption, the production process of titanium dioxide can be optimized to make its water absorption more reasonable, thereby improving its dispersion performance in water, and also helping to improve the application effect of products in which titanium dioxide is an important source of pigments and fillers, such as improving the hiding power of coatings and improving the color of plastics. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the drawings required for use in the embodiment will be briefly introduced below. Obviously, the drawings described below are only some implementation cases of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 A process flow chart of a method for detecting water absorption of titanium dioxide according to the present invention is shown. DETAILED DESCRIPTION

[0020] The detailed description of the following embodiments is used to exemplify the principles of the present invention, but cannot be used to limit the scope of the present invention. The present invention can be implemented in many different forms and is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

[0021] The present invention provides these embodiments to make this disclosure thorough and complete, and fully express the scope of the present invention to those skilled in the art. It should be noted that unless otherwise specifically stated, the relative arrangement of the parts and steps, the composition of materials, numerical expressions and numerical values ​​set forth in these embodiments should be interpreted as being merely exemplary, rather than as limiting.

[0022] It should be noted that, in the description of the present invention, unless otherwise specified, the meaning of "multiple" is greater than or equal to two; the terms "upper", "lower", "left", "right", "inner", "outer", etc., indicating the orientation or positional relationship, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. When the absolute position of the object being described changes, the relative positional relationship may also change accordingly.

[0023] It should also be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances. When a specific device is described as being located between a first device and a second device, there may or may not be an intermediate device between the specific device and the first device or the second device.

[0024] All terms used in the present invention have the same meanings as those understood by those of ordinary skill in the art to which the present disclosure belongs, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries, for example, should be interpreted as having meanings consistent with their meanings in the context of the relevant technology, and should not be interpreted in an idealized or extremely formal sense, unless explicitly defined herein.

[0025] Technologies, methods, and apparatus known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, these technologies, methods, and apparatus should be considered part of the specification.

[0026] like Figure 1 As shown, the present invention provides a method for detecting the water absorption of titanium dioxide, which comprises the following steps: S1. Keep the titanium dioxide sample to be tested warm in an oven and then place it in a desiccator to cool to room temperature; S2. Place the titanium dioxide sample to be tested in a clean beaker, add pure water and stir to mix until a titanium dioxide solution is formed, and let it stand for 0.5~1h; S3, filtering the titanium dioxide solution, and weighing the obtained filter cake and recording it as M1; S4. Dry the filter cake in an oven, weigh the dried filter cake and record it as M2. Water absorption = M1-M2.

[0027] In the method for detecting the water absorption of titanium dioxide according to an embodiment of the present invention, by detecting the water absorption, the production process of titanium dioxide can be optimized to make its water absorption more reasonable, thereby improving its dispersion performance in water, and also helping to improve the application effect of products in which titanium dioxide is an important source of pigments and fillers, such as improving the hiding power of coatings, improving the color of plastics, etc.

[0028] In some specific embodiments, in steps S1 and S4, the temperature of the oven is 100-110°C. Specifically, the temperature of the oven for heat preservation and drying is 105°C. At a temperature of 105°C, the moisture in the titanium dioxide can be effectively evaporated, achieving a more thorough drying effect. Compared with higher temperatures, 105°C is a relatively mild temperature, which can prevent chemical changes or physical damage to the titanium dioxide at high temperatures, thereby maintaining its original excellent properties.

[0029] On the basis of the above embodiment, the method needs to carry out multiple parallel measurements to reduce errors. Multiple parallel measurements can ensure the accuracy and repeatability of experimental data, thereby promoting the in-depth progress of subsequent improvements. In the measurement process, due to the influence of various uncontrollable factors (such as temperature fluctuations, instrument accuracy limitations, slight differences of operators, etc.), a single measurement often has certain random errors. By carrying out multiple parallel measurements, these random errors can be dispersed into each measurement value, thereby eliminating or reducing these errors by statistical methods (such as taking the average value), and improving the accuracy of the measurement results.

[0030] In some specific embodiments, in step S1, the insulation time is 1 to 3 hours, and specifically, the insulation time is 2 hours.

[0031] Based on the above embodiment, in step S4, the drying time is 1 to 3 hours, and specifically, the drying time is 2 hours.

[0032] The free water in the titanium dioxide sample can be fully removed by 2 hours of heat preservation and drying. This free water may remain in the sample during the preparation or treatment process, which will significantly affect the measurement results of water absorption. Setting the heat preservation and drying time to 2 hours can ensure that the same standardized process is followed for each measurement. This helps to improve the repeatability and comparability of the measurement results.

[0033] In some specific embodiments, the filtration includes pouring the titanium dioxide solution into a filtration funnel of a vacuum pump for filtration. The sample that is filtered until no water drips is convenient for subsequent weighing, storage, and testing. No additional processing is required and the sample can be directly used for water absorption detection, thereby simplifying the detection process and improving work efficiency.

[0034] In some specific embodiments, the suction filtration includes pumping the titanium dioxide solution to the bottom of the suction filtration funnel until no water drips.

[0035] In some specific embodiments, in step S2, stirring includes stirring thoroughly with a glass rod at a stirring speed of 2 to 3 revolutions per second, and stirring evenly within 1 to 2 minutes.

[0036] In some specific embodiments, the amount of the titanium dioxide sample to be tested is less than 100 g.

[0037] In some specific embodiments, the amount of the titanium dioxide sample to be tested ranges from 10 to 20 g.

[0038] The detection results of the present invention are described below through specific examples.

[0039] Example 1 1. The water-based titanium dioxide sample 1 to be tested is kept in an oven at 105°C for 2 hours; 2. Take out the sample in step 1 and place it in a desiccator to cool to room temperature; 3. Accurately weigh the titanium dioxide sample in step 2 using an analytical balance and place it in a clean beaker; 4. Add pure water to the sample in step 3, stir and mix thoroughly with a glass rod until the pure water completely submerges the titanium dioxide to form a titanium dioxide solution, and let it stand for 0.5h; 5. Pour the titanium dioxide solution in step 4 into the suction funnel of a vacuum pump and filter until no water drips from the bottom of the funnel; weigh the filter cake obtained and record M1; 6. Place the obtained filter cake in an oven at 105°C and dry it for 2 hours; weigh the dried filter cake again and record the weight M2.

[0040] The above test water absorption analysis results are calculated using the following formula.

[0041] Water absorption = M1-M2 7. Perform three parallel measurements on each sample and record the data.

[0042] Example 2 1. The water-based titanium dioxide sample 2 to be tested was kept in an oven at 105°C for 2 hours; 2. Take out the sample in step 1 and place it in a desiccator to cool to room temperature; 3. Accurately weigh the titanium dioxide sample in step 2 using an analytical balance and place it in a clean beaker; 4. Add pure water to the sample in step 3, stir and mix thoroughly with a glass rod until the pure water completely submerges the titanium dioxide to form a titanium dioxide solution, and let it stand for 0.5h; 5. Pour the titanium dioxide solution in step 4 into the suction funnel of a vacuum pump and filter until no water drips from the bottom of the funnel; weigh the filter cake obtained and record M1; 6. Place the obtained filter cake in an oven at 105°C and dry it for 2 hours; weigh the dried filter cake again and record the weight M2.

[0043] The above test water absorption analysis results are calculated using the following formula.

[0044] Water absorption = M1-M2 7. Perform three parallel measurements on each sample and record the data.

[0045] Example 3 1. The water-based titanium dioxide sample 3 to be tested was kept in an oven at 105°C for 2 hours; 2. Take out the sample in step 1 and place it in a desiccator to cool to room temperature; 3. Accurately weigh the titanium dioxide sample in step 2 using an analytical balance and place it in a clean beaker; 4. Add pure water to the sample in step 3, stir and mix thoroughly with a glass rod until the pure water completely submerges the titanium dioxide to form a titanium dioxide solution, and let it stand for 0.5h; 5. Pour the titanium dioxide solution in step 4 into the suction funnel of a vacuum pump and filter until no water drips from the bottom of the funnel; weigh the filter cake obtained and record M1; 6. Place the obtained filter cake in an oven at 105°C and dry it for 2 hours; weigh the dried filter cake again and record the weight M2.

[0046] The above test water absorption analysis results are calculated using the following formula.

[0047] Water absorption = M1-M2 7. Perform three parallel measurements on each sample and record the data.

[0048] The test results of Examples 1 to 3 are shown in Table 1.

[0049] Table 1 Water absorption test results of different embodiments Sample Results Water absorption 1 (g) Water absorption 2 (g) Water absorption 3 (g) Average value (g) Standard Deviation Relative standard deviation (%) Example 1 44.58 44.48 44.35 44.47 0.12 0.26% Example 2 45.21 45.08 45.04 45.11 0.09 0.20% Example 3 44.61 44.51 44.80 44.64 0.15 0.33% As shown in Table 1, this method has good precision, operability and data reproducibility.

[0050] The present invention provides a method for detecting the water absorption of titanium dioxide, which has at least the following beneficial effects after implementation: (1) Through water absorption testing, we can carefully optimize and adjust the production process of titanium dioxide. This process not only involves precise control of multiple links such as raw material ratio, reaction conditions, and post-treatment, but also relies on advanced testing instruments and analysis methods to ensure that the surface of titanium dioxide particles can be effectively regulated so that its water absorption reaches a more scientific and reasonable range. The improved water absorption performance of the optimized titanium dioxide directly promotes the uniform dispersion and stability of the material in aqueous media, reduces agglomeration, and significantly enhances its compatibility and operability in aqueous systems.

[0051] (2) In the coating industry, the optimized titanium dioxide can more effectively enhance the hiding power of the coating, making the coating surface smoother, the color more full and lasting, while reducing the amount of pigment and reducing costs. In the field of plastic processing, the improved titanium dioxide can significantly improve the color brightness and uniformity of plastic products, giving plastics richer visual effects and texture, and meeting the market's growing demand for high-quality plastic products.

[0052] (3) Titanium dioxide with optimized water absorption may also show better performance in other industries such as papermaking, ink, and cosmetics, such as improving the whiteness and glossiness of paper, enhancing the printing clarity and stability of ink, or optimizing the texture and skin feel of cosmetics, thereby promoting technological progress and product innovation in these industries.

[0053] The above are exemplary embodiments disclosed in the present invention. The order disclosed in the above embodiments of the present invention is for description only and does not represent the advantages and disadvantages of the embodiments. However, it should be noted that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope disclosed in the embodiments of the present invention (including the claims) is limited to these examples. Various changes and modifications may be made without departing from the scope defined in the claims. The functions, steps and / or actions of the method claims according to the disclosed embodiments described herein do not need to be performed in any particular order. In addition, although the elements disclosed in the embodiments of the present invention may be described or required in individual form, they may also be understood as multiple unless explicitly limited to the singular.

[0054] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the embodiments of the present invention as described above, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.

Claims

1. A method for detecting the water absorption of titanium dioxide, It is characterized in that It includes the following steps: S1. Keep the titanium dioxide sample to be tested warm in an oven and then place it in a desiccator to cool to room temperature; S2. Place the titanium dioxide sample to be tested in a clean beaker, add pure water and stir to mix until a titanium dioxide solution is formed, and let it stand for 0.5~1h; S3, the titanium dioxide solution is filtered, and the filter cake obtained is weighed and recorded as M 1 ; S4, drying the filter cake in an oven, and weighing the dried filter cake again and recording it as M 2 , water absorption = M 1 -M 2 .

2. The method for detecting water absorption of titanium dioxide according to claim 1, It is characterized in that In steps S1 and S4, the temperature of the oven is 100-110°C.

3. The method for detecting water absorption of titanium dioxide according to claim 1, It is characterized in that The method requires multiple parallel measurements to reduce errors.

4. The method for detecting water absorption of titanium dioxide according to claim 3, It is characterized in that In step S1, the insulation time is 1 to 3 hours.

5. The method for detecting water absorption of titanium dioxide according to claim 4, It is characterized in that In step S4, the drying time is 1 to 3 hours.

6. The method for detecting water absorption of titanium dioxide according to claim 1, It is characterized in that The suction filtration includes pouring the titanium dioxide solution into the suction funnel of a vacuum pump for suction filtration.

7. The method for detecting water absorption of titanium dioxide according to claim 6, It is characterized in that The suction filtration includes pumping the titanium dioxide solution to the bottom of the suction filtration funnel until no water drips.

8. The method for detecting water absorption of titanium dioxide according to claim 1, It is characterized in that In step S2, the stirring includes stirring thoroughly with a glass rod at a stirring speed of 2 to 3 revolutions per second, and stirring evenly within 1 to 2 minutes.

9. The method for detecting water absorption of titanium dioxide according to claim 1, It is characterized in that The amount of the titanium dioxide sample to be tested is less than 100g.

10. The method for detecting water absorption of titanium dioxide according to claim 1, It is characterized in that The amount of the titanium dioxide sample to be tested ranges from 10 to 20 g.