Method for determining indium content in lead-zinc-containing material by atomic absorption spectrometry

By using nitric acid medium and air-acetylene flame conditions in atomic absorption spectrophotometry, the determination process of indium elements in lead-containing zinc materials is simplified, the extraction and interference problems in the prior art are solved, and high sensitivity and accuracy are achieved. Indium element analysis.

CN118914168APending Publication Date: 2024-11-08GANSU CHANGBA NONFERROUS METALS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411151572.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art requires complex extraction and enrichment processes when determining the content of indium in lead-containing zinc materials, and the differences in media conditions and large elemental interference are affected, which affects the accuracy and sensitivity of the measurement results.

Method used

Atomic absorption spectrophotometry was used to measure the first resonance line of indium at a wavelength of 303.9 nm in 5% nitric acid medium using air-acetylene flame conditions, simplify the sample pretreatment process, avoid the loss of indium, and pass the standard curve Determine the concentration of indium.

Benefits of technology

It realizes the determination of indium elements with high sensitivity, accuracy and precision, simplifies the analysis process and reduces sample losses. It is suitable for the rapid analysis of lead-containing zinc materials in the wet zinc smelting, and meets the production testing requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118914168A_ABST
    Figure CN118914168A_ABST
Patent Text Reader

Abstract

The invention discloses a method for determining the content of indium in a material containing lead and zinc by atomic absorption spectrometry, and belongs to the technical field of detection. The method comprises the following steps: dissolving a sample with aqua regia, determining indium by using an atomic absorption spectrophotometer in a 5% nitric acid medium under an air-acetylene flame condition, and obtaining an optimal measurement result and sensitivity by using a first resonance line of indium at the wavelength of 303.9 nm. The determination range of indium is 0.01%-5%, the linear range is 5-50 [mu] g / ml, and the adding standard recovery rate is 94%-105%. The method has the advantages of being high in accuracy, good in precision and high in analysis speed, and rapid analysis in production can be met. The method greatly simplifies a sample pretreatment process, does not need a complex and tedious extraction and enrichment process, has minimum loss of a to-be-detected sample in an analysis process, is accurate and reliable in analysis data, and meets internal control detection requirements of enterprises.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of detection technology, and specifically is a method for determining the indium content in a lead-zinc-containing material by atomic absorption spectrophotometry. Background Art

[0002] Indium minerals are mostly associated with non-ferrous metal sulfide minerals, especially zinc sulfide, followed by galena, lead oxide, tin, copper sulfide and antimony sulfide. The crude zinc, crude lead, slag, leaching slag, purification slag, solution, smoke, alloy, anode mud, etc. obtained after smelting the above-mentioned non-ferrous metal concentrates are the main enriched materials of indium. The development and research of the comprehensive recovery of the valuable element indium is an effective way for enterprises to reduce costs, increase efficiency, create benefits, and expand profitability. It plays an important role in promoting enterprises to improve their production and operation capabilities and expand profitability. Therefore, it is of great significance to explore an accurate and rapid analysis method for the detection of indium elements in zinc-containing materials.

[0003] The more common analytical methods for indium are spectrophotometry, polarography, graphite furnace atomic absorption spectrometry and flame atomic absorption spectrometry. When using spectrophotometry, polarography and graphite furnace atomic absorption spectrometry, extraction or back-extraction is required, and most of them require extraction, enrichment and separation in a hydrobromic acid medium. Even when using flame atomic absorption spectrophotometry, the selected measurement medium conditions are different, and the interference of the measurement medium and some elements has a greater impact on the measurement results. Summary of the invention

[0004] The purpose of the present invention is to provide a method for determining the indium content in lead-zinc materials by atomic absorption spectrophotometry. The intermediate materials of Chengzhou zinc smelter are used as test samples to determine the best medium and interference conditions for determining indium, and a relatively complete analytical method is established. The analytical operation is simple, the sensitivity is high, and the accuracy and precision are good. The method can be applied to the determination of the indium content in the intermediate lead-zinc materials in hydrometallurgical zinc smelting.

[0005] In the present invention, after the sample is dissolved in aqua regia, in a 5% nitric acid medium, under air-acetylene flame conditions, an atomic absorption spectrophotometer is used to determine the analytical method of indium, and the first resonance line of indium at a wavelength of 303.9nm can obtain the best measurement result and sensitivity. The determination range of indium is 0.01%-5%, the linear range is 5-50μg / ml, and the spike recovery rate is 94%-105%.

[0006] The technical solution adopted by the present invention is as follows:

[0007] The method for determining the indium content in lead-zinc materials by atomic absorption spectrophotometry comprises the following specific steps:

[0008] 1) Accurately weigh 0.2000g of lead-zinc material sample (the sample weight can be appropriately increased or decreased depending on the sample content) in a 250mL beaker, moisten the sample with water, add 15mL of concentrated hydrochloric acid, dissolve at low temperature for 2-3min, add 5ml of concentrated nitric acid and heat until nearly dry (when the sample contains high silicon content, 5-10ml of HF must be added to a polytetrafluoroethylene beaker and evaporated to nearly dry to remove a large amount of silicon), remove and cool; add 3mL of perchloric acid and 10mL of hydrobromic acid along the wall of the beaker and heat on an electric hot plate until smoke is eliminated, remove and cool, continue to add 10mL of hydrobromic acid and carefully evaporate until nearly dry; remove and cool to room temperature, add 5mL of 1+1 nitric acid and dissolve the residue with slight heat; blow water to about 50ml, heat to a slight boil to dissolve other salts;

[0009] 2) Transfer the pretreated sample into a 100ml volumetric flask, shake it to volume (maintaining 5% nitric acid medium), and dry filter it. Use air-acetylene flame, adjust the atomic absorption spectrometer to zero at a wavelength of 303.9nm with water, measure the absorbance of indium in the filtrate, subtract the absorbance of the blank sample, measure the concentration of indium according to the working curve, and calculate the result;

[0010] 3) Pipette 0mL, 0.5mL, 1mL, 2mL, 3mL, and 5mL of indium standard solution (10mg / L) into a 100mL volumetric flask, add 10mL of 5% nitric acid solution, dilute to the mark with water, and shake well; measure the absorbance of indium under the selected instrument working conditions, and draw a working curve with the concentration of indium as the abscissa and the absorbance as the ordinate. The linear range of the curve is 5.0-50μg / mL, and the correlation coefficient is r=0.9998.

[0011] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0012] 1. In the present invention, flame atomic absorption spectrometry is suitable for determining indium content above 0.005%, with high sensitivity and strong characteristic. Taking advantage of the low melting point of indium (156.4°C), the light source can be completely dissociated using a relatively small working current during analysis and determination.

[0013] 2. In the present invention, the sensitivity of indium content analysis is greatly affected by different types of acids. Experimental results show that the loss of indium can be avoided by selecting a suitable nitric acid medium.

[0014] 3. The present invention has the advantages of high accuracy, good precision and fast analysis speed, and can meet the requirements of rapid analysis in production. The sample pretreatment process is greatly simplified, and no complicated extraction and enrichment process is required. The loss of the test sample during the analysis process is minimal, and the analysis data is accurate and reliable, which meets the internal control detection requirements of the enterprise. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1It is a diagram of the standard working curve in Example 1 of the present invention. DETAILED DESCRIPTION

[0017] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the specific data in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.

[0018] In the present invention, the lead-zinc material sample is treated by dissolving with aqua regia, and during the dissolving process, ammonium fluoride, hydrobromic acid, perchloric acid and other solvents are added according to the material component characteristics to remove the interference of silicon, antimony, lead and other ions. In a 5% nitric acid medium, under the condition of air-acetylene flame, the indium content is measured by an atomic absorption spectrophotometer, and the first resonance line of indium at a wavelength of 303.9nm can obtain the best measurement result and sensitivity.

[0019] The selection of instrument working parameters has a great influence on the analysis results. The key parameters of the atomic absorption spectrophotometer test process are: wavelength: 303.9nm; spectral passband width: 0.5nm; lamp current: 2mA; acetylene flow rate 2.0L / min; air flow rate 13.5L / min.

[0020] The reagent conditions used in this example are:

[0021] Atomic absorption spectrophotometer: Agilent 280FS; hydrochloric acid: =1.19 g / ml, AR; nitric acid: ρ=1.42 g / ml, AR; nitric acid: (1+1); hydrobromic acid: AR; perchloric acid: AR; nitric acid solution: 5%;

[0022] Indium standard stock solution: Accurately weigh 1.0000 g of metallic indium (≥99.99%), dissolve it completely with 40 mL of nitric acid (1+1) at low temperature, transfer it into a 1000 ml volumetric flask, dilute it to the scale with water, and shake well; the indium content of this solution is 1 mg / ml.

[0023] Indium standard solution: Use 1000μg / ml indium standard stock solution, pipette 1ml into a 100ml volumetric flask, dilute to scale with water, and shake well. The ρ(indium) of this solution is 10μg / ml.

[0024] Embodiment 1:

[0025] This embodiment provides a method for determining the indium content in a lead-zinc material by atomic absorption spectrophotometry, comprising the following specific steps:

[0026] 1) Accurately weigh 0.2000g of sample (the sample weight can be appropriately increased or decreased depending on the sample content) in a 250mL beaker, moisten the sample with water, add 15mL of concentrated hydrochloric acid, dissolve at low temperature for 2-3min, add 5ml of concentrated nitric acid and heat until nearly dry (when the sample contains high silicon content, 5-10ml of HF must be added to a polytetrafluoroethylene beaker and evaporated to nearly dry to remove a large amount of silicon), remove and cool; add 3mL of perchloric acid and 10mL of hydrobromic acid along the wall of the beaker and heat on an electric hot plate until smoke is eliminated, remove and cool, continue to add 10mL of hydrobromic acid and carefully evaporate until nearly dry; remove and cool to room temperature, add 5mL of 1+1 nitric acid and dissolve the residue with slight heat; blow off water to about 50ml, heat to a slight boil to dissolve other salts;

[0027] 2) Transfer the pretreated sample into a 100ml volumetric flask, shake it to volume (maintaining 5% nitric acid medium), and dry filter it. Use air-acetylene flame, adjust the atomic absorption spectrometer to zero at a wavelength of 303.9nm with water, measure the absorbance of indium in the filtrate, subtract the absorbance of the blank sample, measure the concentration of indium according to the working curve, and calculate the result.

[0028] 3) Pipette 0mL, 0.5mL, 1mL, 2mL, 3mL, and 5mL of indium standard solution (10mg / L) into a 100ml volumetric flask, add 10ml of 5% nitric acid solution, dilute to the scale with water, and shake well. Measure the absorbance of indium under the selected instrument working conditions, and draw a working curve with the concentration of indium as the horizontal coordinate and the absorbance as the vertical coordinate. The linear range of the curve is 5.0-50μg / ml, and the correlation coefficient is r=0.9998.

[0029] Table 1: Spiked recovery and precision test data

[0030]

[0031] Experimental Example 1:

[0032] Take 30mg / L indium standard solution, add 1%-15% hydrochloric acid and 1%-15% nitric acid as the test medium conditions according to the test method, and measure its absorbance. The absorbance value changes of indium standard solution measured by different concentrations of hydrochloric acid and nitric acid are shown in the following table:

[0033] Table 2: Acid medium and concentration experimental test data table

[0034] Hydrochloric acid concentration (%) 1 3 5 7 10 13 15 Absorbance value 0.0561 0.0565 0.050 0.0482 0.0453 0.0422 0.0363 Nitric acid concentration (%) 1 3 5 7 10 13 15 Absorbance value 0.0566 0.0569 0.0569 0.0568 0.0568 0.0569 0.0569

[0035] As can be seen from the table above, the sensitivity of indium in nitric acid is higher than that in hydrochloric acid. When the indium standard solution is in nitric acid, the chloride ion in the sample should be less than 5%, because the presence of halogen acid can easily cause indium volatilization loss, and the generated Cl- will inhibit the absorption of indium, resulting in a low result.

[0036] The nitric acid medium has no effect on the determination of indium under different concentration conditions. In order to minimize the damage of high acidity to the instrument, this method selects 5% nitric acid medium.

[0037] Experimental Example 2:

[0038] Take the same 20mg / L indium standard solution, select 1-8mA lamp current as the instrument measurement condition according to the test method, and measure its absorbance. The changes in the test absorbance values ​​under different lamp current conditions are shown in the following table:

[0039] Table 3: Data table of absorbance values ​​measured at different lamp currents

[0040] Lamp current (mA) 1 2 3 4 5 8 Absorbance value 0.0474 0.0514 0.0500 0.0484 0.0464 0.0445

[0041] From the table above, it can be seen that the measurement stability is poor when the lamp current is 1mA, and the sensitivity of indium decreases with the increase of lamp current when the lamp current is 2-8mA. Therefore, according to the low melting point characteristics of indium, it is not advisable to use a larger lamp current when analyzing and measuring by atomic absorption spectrometry, otherwise it will cause high-temperature dissociation of indium. Through analysis and testing, it is shown that the baseline stability is poor when the indium element lamp is not preheated for a long time, so it must be preheated for more than 30 minutes, and the lamp current is 2mA as the best measurement condition. The indium lamp cannot work for a long time, generally 90 minutes is appropriate.

[0042] Experimental Example 3:

[0043] The materials selected for this test are hydrometallurgical zinc smelting purification slag and lead smoke. The matrix composition of the samples is relatively complex: the main matrix element in the lead smoke is lead, and its content is about Pb 43%; the main matrix elements in the purification slag are Pb10.8%, Zn20.5%, and Cd12.5%. Weigh 0.2000 grams of purification slag and lead smoke samples respectively, and adjust the volume to 100 ml after treatment. The total amount of lead does not exceed 100 mg, the total amount of zinc does not exceed 50 mg, and the total amount of cadmium does not exceed 30 mg. Prepare one group of indium standard series without lead, zinc, and cadmium, and the other group is an indium standard series containing 100 mg of lead, 50 mg of zinc, and 30 mg of cadmium. At the same time, measure their absorbance, and the results are shown in Table 4 below:

[0044] Table 4: Absorbance data table of matrix interference test

[0045]

[0046] According to the characteristics of the main components in the selected samples, the relative error is less than ±5% for the determination of indium content above 0.01%. After comparative testing, 100mgZn, 100mgPb, 8mgCu, 1mgSi, 2mLBr were added to every 100mL solution. - , 3mLSO4 2- , 5mL C10 4-It does not interfere with the determination of indium. When the sample contains a large amount of silicon, the sample will not be completely decomposed. The presence of a large amount of silicon will also form silica gel to absorb a small amount of In 3+ Therefore, hydrofluoric acid should be added during sample pretreatment to volatilize and remove a large amount of silicon SiF4; the sample contains As and SO4 2- If it is too high, it will interfere with the determination and cause the result to be low. Therefore, hydrobromic acid and perchloric acid should be added to generate smoke to remove a large amount of SO4 2- , As plasma is volatilized and removed.

[0047] Experimental Example 4:

[0048] Comparative experiment with extraction enrichment-graphite furnace atomic absorption spectrometry

[0049] After extraction and separation in the M IBK-HBr system, the method of graphite furnace atomic absorption spectrometry is a conventional detection method with high accuracy. The experimental data of this method is stable and highly consistent with that of graphite furnace atomic absorption spectrometry. The comparison data of related samples is shown in Table 5 below:

[0050] Table 5: Comparison data with graphite furnace atomic absorption spectrometry

[0051] Sample name Graphite furnace test results (g / t) Flame atomic absorption measurement results (g / t) Lead fume 1# 715.22 715.42 Lead fume 2# 823.72 816.09 Purification slag 380.10 370.00

[0052] The present invention demonstrates through experiments that the flame atomic absorption spectrometry for determining the indium content in lead-zinc materials has strong applicability to samples, is simple to operate, has high accuracy, good precision, and a wide linear range, can meet the needs of analyzing and detecting materials with complex components in the intermediate of wet zinc smelting, has low detection cost, and has certain application value.

Claims

1. A method for determining the indium content in lead-zinc materials by atomic absorption spectrophotometry, characterized in that: The specific steps include: 1) Accurately weigh the lead-zinc material sample and place it in a beaker, wet the sample with water, add concentrated hydrochloric acid, dissolve it at low temperature for 2-3 minutes, add concentrated nitric acid and heat it until it is almost dry, remove and cool; add perchloric acid and hydrobromic acid along the wall of the beaker and heat it on an electric hot plate until smoke is gone, remove and cool, continue to add hydrobromic acid and carefully steam until it is almost dry; remove and cool to room temperature, add nitric acid and dissolve the residue with slight heat; blow water to 50ml, heat to slight boiling to dissolve other salts; 2) Step 1) Transfer the pretreated sample into a 100ml volumetric flask, shake it to volume, and dry filter it. Use air-acetylene flame, adjust the atomic absorption spectrometer to zero at a wavelength of 303.9nm with water, measure the absorbance of indium in the filtrate, subtract the absorbance of the blank sample, measure the concentration of indium according to the working curve, and calculate the result; 3) Pipette 0mL, 0.5mL, 1mL, 2mL, 3mL, and 5mL of the indium standard solution into a 100mL volumetric flask, add 10mL of a 5% nitric acid solution, dilute to the scale with water, and shake well; determine the absorbance of indium under the selected instrument working conditions, and draw a working curve with the concentration of indium as the abscissa and the absorbance as the ordinate; the linear range of the curve is 5.0 to 50μg / ml, and the correlation coefficient is r=0.9998.

2. The method for determining the indium content in lead-zinc materials by atomic absorption spectrophotometry according to claim 1, characterized in that: In step 1), weigh 0.2000 g of a lead-zinc material sample into a 250 mL beaker; add 15 mL of concentrated hydrochloric acid; add 5 mL of concentrated nitric acid; add 3 mL of perchloric acid and 10 mL of hydrobromic acid along the wall of the beaker and heat on a hot plate until smoke is gone, remove and cool, continue to add 10 mL of hydrobromic acid and carefully evaporate until nearly dry; remove and cool to room temperature, add 5 mL of 1+1 nitric acid and dissolve the residue with slight heat.

3. The method for determining the indium content in lead-zinc materials by atomic absorption spectrophotometry according to claim 1, characterized in that: In step 3), the indium standard solution is a 10 mg / L indium standard solution.