Method for characterizing niobium content in potassium fluotantalate
By characterizing its niobium content in real time during the production process of potassium fluortanate, the problem that the existing technology cannot effectively detect the niobium content in potassium fluortanate is solved, simplifying the detection process, reducing costs and improving characterization efficiency, ensuring high Production quality of pure tantalum powder.
Patent Information
- Application Number
- CN202411018430.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art cannot effectively detect the content of niobium in potassium fluorotantalate, especially when the niobium content requirements in the production of high-purity tantalum powder are extremely low, resulting in the need to downgrade or use other products during the production process, which increases uncertainty. Sex and potential risks.
By reacting fluorotantalic acid solution with potassium chloride and hydrofluoric acid, cooling and crystallization, adjusting the pH value of the mother liquor for solid-liquid separation, obtaining tantalum hydroxide-containing precipitate, and its niobium content is analyzed by inductively coupled plasma atomic emission spectroscopy , and calculate the niobium content in potassium fluortanate based on specific formulas to achieve real-time characterization.
The detection process is simplified, costs are reduced, characterization efficiency is improved, production process conditions are allowed to be adjusted in real time, ensuring that the niobium content in potassium fluorotantalate meets the requirements, and reducing uncertainty in production.
Abstract
Description
Technical Field
[0001] The present application relates to the field of analysis, and in particular to a method for characterizing the niobium content in potassium fluorotantalate. Background Art
[0002] Potassium fluorotantalate is an important raw material for tantalum-niobium metallurgy, and is mainly used for the preparation of metallurgical or capacitor-grade tantalum powder. The method generally used in industry is to melt potassium fluorotantalate, add potassium chloride, sodium chloride, potassium fluoride, etc., and then add metallic sodium to prepare porous metal tantalum powder. This tantalum powder is used for the preparation of high-purity tantalum ingots. At present, the purity requirements for high-purity tantalum powder are increasing, and some even require the total amount of impurities in niobium, tungsten and molybdenum to be controlled within 0.1ppm (0.1 micrograms per gram). Among them, niobium is a companion element of tantalum and the main associated impurity of potassium fluorotantalate. Therefore, the requirements for the niobium content in potassium fluorotantalate, the main raw material of high-purity tantalum powder, are also further increased.
[0003] Inductively coupled plasma-mass spectrometry (ICP-MS) is usually used to detect the niobium content in potassium fluorotantalate. However, the current production of high-purity tantalum powder requires that the niobium content in high-purity potassium fluorotantalate be below 0.5ppm. ICP-MS cannot detect niobium below 0.5ppm in potassium fluorotantalate. Glow discharge mass spectrometry (GD-MS) is usually used to analyze trace elements. However, GD-MS is a method for detecting impurity elements in conductive materials. Since potassium fluorotantalate crystals cannot conduct electricity and are partially corrosive, GD-MS cannot be used to detect the niobium content in potassium fluorotantalate.
[0004] Therefore, in order to ensure that the niobium content in high-purity tantalum powder meets the content requirement of 0.5ppm or even lower (such as 0.1ppm), it is necessary to use more advanced methods to detect or characterize the niobium content in potassium fluorotantalate, so as to lay the foundation and provide basis for the subsequent production of high-purity tantalum powder.
[0005] At present, the niobium content in potassium fluorotantalate is mainly detected in actual production by measuring the niobium content A in the high-purity tantalum powder prepared from potassium fluorotantalate, and then deducing the niobium content B = A × w in potassium fluorotantalate based on the mass percentage of tantalum in potassium fluorotantalate w = 181 / 392≈0.462. However, the above method must be carried out after the production of high-purity tantalum powder is completed. Therefore, the niobium content in potassium fluorotantalate cannot be determined in advance, which leads to the inability to determine the process of producing tantalum powder by reducing potassium fluorotantalate with sodium in advance, resulting in a large number of products obtained in the production process needing to be downgraded or used for other purposes, which brings great uncertainty and potential adverse effects to production. Summary of the invention
[0006] The present application provides a method for characterizing the niobium content in potassium fluorotantalate, so as to improve the efficiency of characterizing the niobium content in potassium fluorotantalate.
[0007] The first aspect of the present application provides a method for characterizing the niobium content in potassium fluorotantalate. The potassium fluorotantalate is prepared by the following preparation method: a fluorotantalate solution, potassium chloride and hydrofluoric acid are subjected to a synthesis reaction and then cooled and crystallized to obtain a mother liquor and potassium fluorotantalate crystals. The characterization method comprises: adjusting the pH value of the mother liquor to above 8 and then performing solid-liquid separation to obtain a precipitate containing tantalum hydroxide; washing the precipitate containing tantalum hydroxide to neutrality and drying to obtain a tantalum hydroxide powder; analyzing the tantalum hydroxide powder by inductively coupled plasma atomic emission spectrometry to obtain a niobium content a in the tantalum hydroxide powder; calculating a content b by formula (1), and using the content b to characterize the niobium content in the potassium fluorotantalate.
[0008] Formula (1): b = a / n, n = 700-800.
[0009] In any embodiment of the first aspect, for the above-mentioned method for characterizing the niobium content in potassium fluorotantalate, when more than 50% of the potassium fluorotantalate crystals pass through an 80-mesh sieve, 700≤n≤750.
[0010] In any embodiment of the first aspect, for the above-mentioned method for characterizing the niobium content in potassium fluorotantalate, when 50% or more of the potassium fluorotantalate crystals fail to pass through an 80-mesh sieve, 751≤n≤800.
[0011] The second aspect of the present application provides another method for characterizing the niobium content in potassium fluorotantalate, the method comprising: heating potassium fluorotantalate and hydrofluoric acid to a predetermined temperature, keeping the mixture at a predetermined temperature for a predetermined time, cooling and crystallizing the mixture to obtain potassium fluorotantalate crystals and a mother liquor; adjusting the pH value of the mother liquor to above 8, performing solid-liquid separation to obtain a precipitate containing tantalum hydroxide; washing the precipitate containing tantalum hydroxide to neutrality, and drying the precipitate to obtain a tantalum hydroxide powder; analyzing the tantalum hydroxide powder by inductively coupled plasma atomic emission spectrometry to obtain a niobium content a in the tantalum hydroxide; calculating a content b by formula (2), and using the content b to characterize the niobium content in the potassium fluorotantalate.
[0012] Formula (2): b=a / m, 20≤m≤50.
[0013] In any embodiment of the second aspect, when more than 50% of the potassium fluorotantalate crystals pass through an 80-mesh sieve, 20≤m≤35.
[0014] In any embodiment of the second aspect, when 50% or more of the crystals of potassium fluorotantalate fail to pass through an 80-mesh sieve, 36≤m≤50.
[0015] In any embodiment of the second aspect, the ratio of potassium fluorotantalate to HF in hydrofluoric acid is 4 kg: (10-20) mol.
[0016] In any embodiment of the second aspect, for the above-mentioned method for characterizing the niobium content in potassium fluorotantalate, the predetermined temperature is 85°C-95°C.
[0017] In any embodiment of the second aspect, for the above-mentioned method for characterizing the niobium content in potassium fluorotantalate, the predetermined time is greater than or equal to 30 minutes, and more preferably 30-90 minutes.
[0018] In any embodiment of the second aspect, the pH value of the mother liquor is adjusted to between 8 and 9 with aqueous ammonia before solid-liquid separation.
[0019] The characterization method of niobium content in potassium fluorotantalate provided by the present application is based on the analysis of a large number of production and test data, and the mother liquor generated in the production process of potassium fluorotantalate can be used to characterize the niobium content in potassium fluorotantalate in real time. On the one hand, the characterization method of niobium content in potassium fluorotantalate of the present application does not need to reduce potassium fluorotantalate to tantalum powder, which greatly simplifies the detection process and reduces manpower, material and time costs; on the other hand, the characterization efficiency of the characterization method of niobium content in potassium fluorotantalate of the present application is significantly improved, and the production process conditions of potassium fluorotantalate can be adjusted in real time according to the characterization results, providing a reliable adjustment basis for reducing the niobium content in potassium fluorotantalate. DETAILED DESCRIPTION
[0020] The following embodiments further describe the implementation of the present application in detail. The detailed description of the following embodiments is used to illustrate the principle of the present application, but cannot be used to limit the scope of the present application, that is, the present application is not limited to the described embodiments.
[0021] As analyzed in the background technology of this application, in order to characterize the niobium content in potassium fluorotantalate, the prior art first determines the niobium content in the high-purity tantalum powder prepared from potassium fluorotantalate, and then infers the niobium content in potassium fluorotantalate according to the formula, and uses this data to characterize the niobium content in potassium fluorotantalate. However, this method is carried out after the production of high-purity tantalum powder is completed, and the production process is time-consuming, so it is impossible to effectively and quickly characterize the niobium content in potassium fluorotantalate. In order to solve this problem, this application provides a method for characterizing the niobium content in potassium fluorotantalate.
[0022] Since the niobium content B in potassium fluorotantalate is obtained by inversely inferring the niobium content A in the tantalum powder in the process of preparing high-purity tantalum powder using potassium fluorotantalate, the applicant of the present application has accumulated a large amount of data, and further analysis has found that the niobium content in potassium fluorotantalate is closely related to the niobium content in the mother liquor during its production process. Based on this discovery, a method for characterizing the niobium content in potassium fluorotantalate is provided in the first embodiment of the present application. Potassium fluorotantalate comes from the following preparation method: cooling and crystallizing a mother liquor and potassium fluorotantalate crystals after a synthesis reaction of fluorotantalate solution, potassium chloride and hydrofluoric acid, and the characterization method includes: adjusting the pH value of the mother liquor to above 8 and then performing solid-liquid separation to obtain a precipitate containing tantalum hydroxide; washing the precipitate containing tantalum hydroxide to neutrality and drying to obtain a tantalum hydroxide powder; analyzing the tantalum hydroxide powder by inductively coupled plasma-atomic emission spectrometry to obtain the niobium content a in the tantalum hydroxide powder; calculating the content b by formula (1), and using the content b to characterize the niobium content in potassium fluorotantalate, formula (1): b=a / n, 700≤n≤800.
[0023] The method utilizes the mother liquor generated during the production process of potassium fluorotantalate to characterize the niobium content in the produced potassium fluorotantalate in real time, thereby improving the characterization efficiency of the niobium content in the potassium fluorotantalate, and the production process conditions of the potassium fluorotantalate can be adjusted in real time according to the characterization results, providing a reliable adjustment basis for reducing the niobium content in the potassium fluorotantalate.
[0024] In the above characterization method, tantalum in the mother liquor is precipitated in the form of tantalum hydroxide. Based on the coexistence of tantalum and niobium, niobium in the mother liquor is also precipitated with tantalum hydroxide. In addition, during the above crystallization and precipitation process, niobium is gradually enriched, so its concentration is relatively high relative to the content in potassium fluorotantalate crystals, and can be determined by conventional detection method inductively coupled plasma atomic emission spectrometry (refer to GB T 15076.2-2019 Chemical Analysis Methods for Tantalum and Niobium Part 2 Determination of Niobium Content in Tantalum Inductively Coupled Plasma Atomic Emission Spectrometry). Moreover, based on the statistical analysis of a large number of experimental data, it is found that the mother liquor and potassium fluorotantalate obtained under the same crystallization conditions have the following relationship: the niobium content a in the tantalum hydroxide powder from the mother liquor obtained by the inventor of the present application by inductively coupled plasma atomic emission spectrometry and the niobium content B of potassium fluorotantalate obtained by inverse calculation using the niobium content in the tantalum powder have a linear relationship B=a / n, thereby obtaining the correlation coefficient n. Furthermore, during the test, the formula (1) b=a / n is used to calculate the content b that can characterize the niobium content in potassium fluorotantalate.
[0025] It should be noted that the above content b is only used to characterize the niobium content in potassium fluorotantalate, and does not necessarily mean that it is equal to the actual niobium content in potassium fluorotantalate. Since the content b is directly related to the niobium content A in the tantalum powder prepared from the potassium fluorotantalate, the niobium content in the tantalum powder can be calculated based on the mass percentage of tantalum in the potassium fluorotantalate. If the niobium content in the tantalum powder is too high and does not meet the application requirements, it means that the niobium content in the potassium fluorotantalate is too high and the potassium fluorotantalate preparation process needs to be adjusted; otherwise, it means that the niobium content in the potassium fluorotantalate meets the tantalum powder production requirements.
[0026] According to the findings of the applicant in the actual production process of potassium fluorotantalate, there is a close correlation between the niobium content and grain size of potassium fluorotantalate. When the grain size of potassium fluorotantalate is small, it means that the grain growth rate is fast, the impurity niobium contained and the crystal specific surface area are large, and the niobium content is high; when the grain size of potassium fluorotantalate is large, it means that the grain growth rate is slow, the impurity niobium contained is less, the specific surface area of potassium fluorotantalate crystal is also small, and the residual niobium content is low. Moreover, there is a close correlation between the grain size and the correlation coefficient n in formula (1). For example, in some embodiments of the present application, when more than 50% of the potassium fluorotantalate crystals pass through an 80-mesh sieve, 700≤n≤750; when 50% or more of the potassium fluorotantalate crystals do not pass through an 80-mesh sieve, 751≤n≤800. When the grain size is small, the value of n is small, and the corresponding potassium fluorotantalate has a higher niobium content.
[0027] The mesh numbers described in this application are based on the mesh numbers specified in the US standard, where 80 meshes correspond to a particle size of 178 μm.
[0028] According to the relationship between the grain size and the crystallization conditions known in the art, those skilled in the art can also directly select different n values according to the crystallization conditions. In some embodiments of the present application, the cooling crystallization includes: water cooling outside the jacket, and adjusting the temperature of the cooling water. According to the actual production process, the relationship between the above-mentioned grain size and the cooling crystallization conditions is summarized. When applying the characterization method of the present application, the grain size of the potassium fluorotantalate crystals can be tested without testing, and the grain size range can be directly determined according to the cooling crystallization conditions. Then, the above-mentioned value relationship can be used and directly calculated by entering the formula, thereby further improving the characterization efficiency of the characterization method of the present application.
[0029] In order to improve the precipitation efficiency of tantalum and niobium, the pH range of the obtained mother liquor can be adjusted in a targeted manner. In some embodiments of the present application, ammonia water is used to adjust the pH value of the mother liquor to between 8 and 9, so that the niobium in the mother liquor can be precipitated sufficiently and quickly.
[0030] When the inductively coupled plasma atomic emission spectrometry is used in the present application to test the niobium content in tantalum hydroxide-containing powder, the test process can refer to GB T 15076.2-2019 "Chemical Analysis Methods for Tantalum and Niobium Part 2 Determination of Niobium Content in Tantalum Inductively Coupled Plasma Atomic Emission Spectrometry", such as digesting the tantalum hydroxide-containing powder, preparing a standard solution and drawing a standard curve based on it, and using the test data and the standard curve to calculate the niobium content of the tantalum hydroxide-containing powder. In order to improve the accuracy and test efficiency of the inductively coupled plasma atomic emission spectrometry, in some embodiments of the present application, before the tantalum hydroxide-containing powder is analyzed by the inductively coupled plasma atomic emission spectrometry, the sample is calcined at 800°C for not less than 2 hours before testing.
[0031] In a second embodiment of the present application, a method for characterizing the niobium content in potassium fluorotantalate is provided, the method comprising: heating a mixture of potassium fluorotantalate and hydrofluoric acid to a predetermined temperature and keeping the mixture at a predetermined temperature for a predetermined time, followed by cooling and crystallization to obtain potassium fluorotantalate crystals and a mother liquor; adjusting the pH value of the mother liquor to above 8 and performing solid-liquid separation to obtain a precipitate containing tantalum hydroxide; washing the precipitate containing tantalum hydroxide to neutrality and drying to obtain a tantalum hydroxide powder; analyzing the tantalum hydroxide powder by inductively coupled plasma atomic emission spectrometry to obtain a niobium content a in the tantalum hydroxide powder; and calculating a content b by formula (2), wherein the content b can be used to characterize the niobium content in potassium fluorotantalate, formula (2): b=a / m, 20≤m≤50.
[0032] This method can achieve rapid characterization of the niobium content in potassium fluorotantalate crystals. Potassium fluorotantalate is dissolved in hydrofluoric acid and recrystallized. During the dissolution process, niobium in potassium fluorotantalate is also dissolved. Potassium fluorotantalate and associated niobium remain in the mother liquor after recrystallization. Tantalum hydroxide-containing powder is then obtained by precipitating the mother liquor. The niobium content in the tantalum hydroxide-containing powder is detected to characterize the niobium content in potassium fluorotantalate. There is no need to reduce potassium fluorotantalate to tantalum powder, which greatly simplifies the detection process and reduces time, manpower and material costs.
[0033] In some embodiments of the present application, the above-mentioned inductively coupled plasma-atomic emission spectrometry for testing the content a can be implemented with reference to GB T 15076.2-2019 "Chemical analysis methods for tantalum and niobium Part 2 Determination of niobium content in tantalum by inductively coupled plasma atomic emission spectrometry".
[0034] The characterization method in the second embodiment is similar in principle to the characterization method in the first embodiment, and is based on the following relationship between the mother liquor and potassium fluorotantalate obtained under the same crystallization conditions: The applicant of the present application uses inductively coupled plasma atomic emission spectrometry to measure the niobium content a in the tantalum hydroxide-containing powder from the mother liquor, and the niobium content B in the potassium fluorotantalate obtained by inversely deducing the niobium content in the tantalum powder has a linear relationship B=a / m, thereby obtaining the correlation coefficient m. Furthermore, during the test, the formula (2) b=a / m is used to calculate the content b that can characterize the niobium content in potassium fluorotantalate.
[0035] The correlation coefficient n in the above formula (1) and the correlation coefficient m in the above formula (2) have different value ranges, mainly because the precipitation environment of the mother liquid in the first embodiment and the second embodiment is different.
[0036] In some embodiments, the ratio of potassium fluorotantalate to HF in hydrofluoric acid is 4 kg:(10-20) mol.
[0037] In some embodiments, the predetermined temperature is 85° C.-95° C., and the predetermined time is greater than or equal to 30 min, and more preferably the predetermined time is 30-90 min, so that potassium fluorotantalate can be fully and quickly dissolved.
[0038] As described in the first embodiment, there is a close correlation between the purity and grain size of potassium fluorotantalate, that is, when the grain size of potassium fluorotantalate is small, it means that the grain growth rate is fast, the specific surface area is large, and there is more niobium residue on the surface and inside of potassium fluorotantalate; when the grain size of potassium fluorotantalate is large, the specific surface area is small, which means that the grain growth rate is slow, and the content of impurity niobium wrapped on the outer surface and inside is less. For the mother liquor after potassium fluorotantalate is recrystallized, there is a close correlation between the grain size and the correlation coefficient m in formula (2). For example, in some embodiments of the present application, when more than 50% of the potassium fluorotantalate crystals pass through the 80-mesh sieve, 20≤m≤35; when 50% or more of the potassium fluorotantalate crystals do not pass through the 80-mesh sieve, 36≤m≤50. When the grain size is small, the value of m is small, and the corresponding potassium fluorotantalate has a higher niobium content. The particle size corresponding to 80 mesh is also 178μm.
[0039] In order to improve the precipitation efficiency of tantalum and niobium, the pH range of the obtained mother liquor can be adjusted in a targeted manner. Therefore, in some embodiments of the present application, the characterization method of the second embodiment above uses ammonia water to adjust the pH value of the mother liquor to between 8 and 9.
[0040] The beneficial effects of the present application will be further illustrated below in combination with examples and comparative examples, but the scope of the present invention is not limited to these examples.
[0041] Example 1
[0042] 1300L of tantalate fluoro solution was added to the synthesis kettle, and then analytical grade potassium chloride and hydrofluoric acid were added, and the outer wall of 20-30°C cooling water was used for forced cooling and crystallization to obtain potassium tantalate fluoro crystals and mother liquor, and more than 60% of the obtained potassium tantalate fluoro crystals did not pass through the 80-mesh sieve.
[0043] By mixing ammonia water with the mother liquor to stabilize the pH value of the mother liquor at about 8, a tantalum hydroxide precipitate was obtained, and then the tantalum hydroxide powder was obtained by washing to neutrality and drying. The tantalum hydroxide powder was analyzed by inductively coupled plasma atomic emission spectrometry. The analysis process was carried out in accordance with GB T 15076.2-2019 "Chemical analysis methods of tantalum and niobium Part 2 Determination of niobium content in tantalum Inductively coupled plasma atomic emission spectrometry", and the niobium content in the tantalum hydroxide powder was 300ppm.
[0044] According to the relationship between the above-mentioned potassium fluorotantalate crystal passing through an 80-mesh sieve and the correlation coefficient n, n is selected as 800, and the niobium content in the potassium fluorotantalate crystal is calculated using the formula (1) b=a / n to obtain b=300 / 800=0.375ppm.
[0045] Then, this batch of potassium fluorotantalate was reduced with sodium to obtain tantalum powder. Through GD-MS analysis of the tantalum powder, the niobium content in the tantalum powder was determined to be 0.81ppm. Further, using the mass percentage of tantalum in potassium fluorotantalate w=181 / 392≈0.462 and the formula B=A×w, the niobium content in potassium fluorotantalate was calculated to be B=0.81×0.462=0.374ppm.
[0046] It can be seen that the niobium content b in the potassium fluorotantalate crystals obtained by the characterization method of the present application is basically equivalent to the niobium content B in the potassium fluorotantalate crystals calculated by using the niobium content in the tantalum powder, indicating that the characterization method of Example 1 of the present application is reliable.
[0047] Example 2
[0048] The difference from Example 1 is that the cooling crystallization conditions are changed to forced cooling crystallization using 5-15°C cooling water on the outer wall, and more than 60% of the obtained potassium fluorotantalate crystals pass through an 80-mesh sieve.
[0049] The niobium content in the tantalum hydroxide-containing powder was found to be 350 ppm by inductively coupled plasma atomic emission spectrometry.
[0050] According to the relationship between the potassium fluorotantalate crystal passing through an 80-mesh sieve and the correlation coefficient n, n was selected as 720, and the niobium content in the potassium fluorotantalate crystal was calculated using the formula (1) b=a / n to obtain b=350 / 720=0.48 ppm.
[0051] The batch of potassium fluorotantalate was then reduced with sodium to obtain tantalum powder. The niobium content in the tantalum powder was determined to be 0.96 ppm by GD-MS analysis of the tantalum powder, and the niobium content in the potassium fluorotantalate was further calculated by the formula B=A×w to be B=0.96×0.462=0.444 ppm.
[0052] It can be seen that the niobium content b in the potassium fluorotantalate crystals obtained by the characterization method of the present application is basically equivalent to the niobium content B in the potassium fluorotantalate crystals calculated by using the niobium content in tantalum powder, indicating that the characterization method of Example 2 of the present application is reliable.
[0053] Example 3
[0054] 8 kg of potassium tantalate was added to 20 L of 1.5 mol / L hydrofluoric acid, heated to 90° C. and stirred for 1 hour, then cooled and crystallized by natural air, and centrifuged to obtain potassium tantalate crystals and mother liquor, wherein more than 60% of the potassium tantalate crystals did not pass through an 80-mesh sieve.
[0055] By mixing ammonia water with the mother liquor to stabilize the pH value of the mother liquor at about 8, a tantalum hydroxide precipitate was obtained, and then the tantalum hydroxide powder was obtained by washing to neutrality and drying. The tantalum hydroxide powder was analyzed by inductively coupled plasma atomic emission spectrometry (refer to GBT 15076.2-2019 Chemical analysis method of tantalum and niobium Part 2 Determination of niobium content in tantalum), and the niobium content in the tantalum hydroxide powder was 10ppm.
[0056] Based on the relationship between the above-mentioned potassium fluorotantalate crystal passing through an 80-mesh sieve and the correlation coefficient m, m is selected to be 40, and the niobium content in the potassium fluorotantalate crystal is calculated using the formula (2) b=a / m to be 10 / 40=0.25ppm.
[0057] The batch of potassium fluorotantalate was reduced with sodium to obtain tantalum powder, and the tantalum powder was analyzed to obtain a niobium content of 0.60 ppm. Further, the mass percentage w of tantalum in potassium fluorotantalate was calculated by the formula B=A×w to obtain the niobium content in potassium fluorotantalate as B=0.60×0.462=0.28 ppm.
[0058] It can be seen that the niobium content in the potassium fluorotantalate crystals obtained by the characterization method of the present application is basically equivalent to the niobium content in the potassium fluorotantalate crystals calculated by using the niobium content in tantalum powder, indicating that the characterization method of Example 3 of the present application is reliable.
[0059] Example 4
[0060] The difference from Example 3 is that the cooling crystallization condition is changed to rapid cooling with external cooling water to obtain mother liquor and potassium tantalate fluoroate crystals, wherein more than 62% of the potassium tantalate fluoroate crystals pass through an 80-mesh sieve.
[0061] The niobium content in the tantalum hydroxide-containing powder was found to be 12 ppm by inductively coupled plasma atomic emission spectrometry.
[0062] Based on the relationship between the above-mentioned potassium fluorotantalate crystal passing through an 80-mesh sieve and the correlation coefficient m, m is selected to be 31, and the niobium content in the potassium fluorotantalate crystal is calculated using the formula (2) b=a / m to be 12 / 31=0.387 ppm.
[0063] The batch of potassium fluorotantalate was reduced with sodium to obtain tantalum powder, which was analyzed to obtain niobium content in the tantalum powder, which was 0.83 ppm. The mass percentage w of tantalum in potassium fluorotantalate was further calculated using the formula B=A×w to obtain the niobium content in potassium fluorotantalate as B=0.83×0.462=0.383 ppm.
[0064] It can be seen that the niobium content in potassium fluorotantalate obtained by the characterization method of the present application is basically equivalent to the niobium content in potassium fluorotantalate calculated by using the niobium content in tantalum powder, indicating that the characterization method of Example 4 of the present application is reliable.
[0065] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A method for characterizing the niobium content in potassium fluorotantalate, wherein the potassium fluorotantalate is prepared by the following method: a fluorotantalate solution, potassium chloride and hydrofluoric acid are subjected to a synthetic reaction and then cooled and crystallized to obtain a mother liquor and the potassium fluorotantalate crystals, wherein: The characterization method comprises: The pH value of the mother liquor is adjusted to above 8, and then solid-liquid separation is performed to obtain a precipitate containing tantalum hydroxide; washing the tantalum hydroxide-containing precipitate to neutrality and drying to obtain tantalum hydroxide-containing powder; Analyzing the tantalum hydroxide-containing powder by inductively coupled plasma atomic emission spectrometry to obtain the niobium content a in the tantalum hydroxide-containing powder; The content b is calculated using formula (1), and the content b is used to characterize the niobium content in the potassium fluorotantalate. Formula (1): b = a / n, n = 700-800.
2. The characterization method according to claim 1, characterized in that When more than 50% of the potassium fluorotantalate crystals pass through the 80-mesh sieve, 700≤n≤750; when 50% or more of the potassium fluorotantalate crystals do not pass through the 80-mesh sieve, 751≤n≤800.
3. A method for characterizing the niobium content in potassium fluorotantalate, characterized in that: The characterization method comprises: The potassium fluorotantalate and hydrofluoric acid are mixed and heated to a predetermined temperature and kept at the temperature for a predetermined time, and then cooled and crystallized to obtain potassium fluorotantalate crystals and a mother liquid; The pH value of the mother liquor is adjusted to above 8, and then solid-liquid separation is performed to obtain a precipitate containing tantalum hydroxide; washing the tantalum hydroxide-containing precipitate to neutrality and drying to obtain tantalum hydroxide-containing powder; The tantalum hydroxide powder is analyzed by inductively coupled plasma atomic emission spectrometry to obtain the niobium content a in the tantalum hydroxide; the content b is calculated by formula (2), and the niobium content in the potassium fluorotantalate is characterized by the content b. Formula (2): b=a / m, 20≤m≤50.
4. The characterization method according to claim 3, characterized in that: The ratio of the potassium fluorotantalate to the HF in the hydrofluoric acid is 4kg:(10-20)mol.
5. The characterization method according to claim 3 or 4, characterized in that: The predetermined temperature is 85°C-95°C.
6. The characterization method according to any one of claims 3 to 5, characterized in that: The predetermined time is greater than or equal to 30 minutes, and more preferably 30-90 minutes.
7. The characterization method according to any one of claims 3 to 6, characterized in that: When more than 50% of the potassium fluorotantalate crystals pass through the 80-mesh sieve, 20≤m≤35; when 50% or more of the potassium fluorotantalate crystals do not pass through the 80-mesh sieve, 36≤m≤50.
8. The characterization method according to any one of claims 3 to 7, characterized in that: The solid-liquid separation is performed after the pH value of the mother liquor is adjusted to between 8 and 9 by using aqueous ammonia.