Conductive film and preparation method thereof

By designing the relative displacement difference and groove structure of the support layer and transition layer in the conductive film, the stress concentration problem during the bending process is solved, its stability and bending performance are improved, and the risks of delamination and cracking are avoided.

CN118919130APending Publication Date: 2024-11-08ZHEJIANG RUOZHEN TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411284633.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The conductive film is prone to stress concentration during bending, resulting in risk of delamination and cracking, especially in the current collector process of lithium batteries.

Method used

A conductive film is designed, including a support layer and a transition layer of a bending region. After bending, the transition layer has a smaller relative displacement with the conductive layer, while the transition layer of a non-bending region has a larger displacement, forming a Anchor structure and groove structure to reduce stress concentration in the bending area and release stress through interlayer slippage.

Benefits of technology

It effectively reduces stress concentration in the bending area, reduces the risk of delamination and cracking, and improves the bending performance and stability of the conductive film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005042772770000011
    Figure HDA0005042772770000011
  • Figure HDA0005042772770000012
    Figure HDA0005042772770000012
Patent Text Reader

Abstract

The invention discloses a conductive film and a preparation method thereof, and belongs to the technical field of conductive films, the conductive film comprises a support layer and a transition layer formed on the surface of the support layer corresponding to a bending area, and a conductive layer is at least formed on the surface of the transition layer; the transition layer of the bending area has a first relative displacement L1 with the conductive layer after being bent, the transition layer of the non-bending area has a second relative displacement L2 with the conductive layer after being bent, and L2 is larger than L1. Compared with the prior art, the conductive film and the transition layer have relatively large relative displacement in the non-bending area, so that after bending, bending stress generated by the conductive film and the transition layer can be released through interlayer slippage of the non-bending area with large relative displacement, and the situation that stress in the bending area is excessively concentrated can be reduced to a certain extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of conductive film materials, and in particular to a conductive film and a preparation method thereof. Background Art

[0002] Conductive film is a polymer material with metal coated on the surface. Common processing methods include vacuum evaporation, which uses polymer film as a carrier to evaporate metal targets.

[0003] In its application scenarios, the conductive film is used as a current collector in a lithium battery. In the winding assembly process, the pole piece needs to be bent, and the current collector will also bend or fold during the process. Since the base film layer is a single polymer material layer, stress will be generated when bending occurs, and there may be a risk of delamination and cracking. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, one object of the present invention is to provide a conductive film that corresponds to the difference in relative displacement between the bending area and the non-bending area to avoid delamination and cracking in the bending area, and at the same time, it is easy to release the stress in the bending area.

[0005] The technical solution of the present invention is as follows:

[0006] A conductive film comprises a support layer and a transition layer formed on the surface of the support layer corresponding to the bending area, and at least a conductive layer is formed on the surface of the transition layer;

[0007] The transition layer in the bending zone has a first relative displacement L1 with the conductive layer after bending, and the transition layer in the non-bending zone has a second relative displacement L2 with the conductive layer after bending, and L2 is greater than L1.

[0008] Based on the above technical solution, since the transition layer has a relatively larger relative displacement in the non-bending area, the bending stress generated by it after bending can be released through the interlayer slippage in the non-bending area with a large relative displacement, which can reduce the excessive concentration of stress in the bending area to a certain extent.

[0009] Furthermore, the elastic modulus of the transition layer is smaller than that of the support layer.

[0010] Based on the above technical solution, a relatively small elastic modulus can be provided, which can facilitate the subsequent release of stress.

[0011] Furthermore, in the bending zone, the support layer and the transition layer form an anchoring structure.

[0012] Based on the above technical solution, the conductive film is not easily deformed in the bending zone, but is easier to deform in the non-bending zone, and the stress in the bending zone is easily released in the non-bending zone, thereby improving the problem of stress concentration in the transition layer in the bending zone.

[0013] Furthermore, a transition layer is arranged in the bending zone corresponding to the bending direction, a plurality of first grooves are arranged on the surface of the support layer corresponding to the bending zone in the bending direction, the transition layer is connected to the surface of the support layer, and part of the transition layer is arranged in the first groove to form a matching structure.

[0014] Based on the above technical solution, the transition layer in the bending area can have a smaller displacement than the transition layer in the non-bending area, so it is not easy to produce a large displacement in the bending area, making it difficult for the conductive layer to delaminate or wrinkle, and easy to release stress.

[0015] Further, the first slot is an array-shaped slot structure; and / or,

[0016] The first groove is a strip-shaped groove structure.

[0017] Based on the above technical solution, a concave structure can be formed on the surface of the support layer, so that the transition layer can be partially embedded in the surface of the support layer.

[0018] Furthermore, the groove depth of the first groove does not exceed 1 / 3 of the thickness of the support layer.

[0019] Furthermore, the groove width is not greater than 2 mm.

[0020] Based on the above technical solution, the influence of grooving on the strength of the supporting layer can be reduced.

[0021] Furthermore, a plurality of second grooves are provided in the transition layer of the non-bending region.

[0022] Based on the above technical solution, grooves are provided in the transition layer in the non-bending area, so as to further enhance the deformation capacity of the transition layer in the non-bending area.

[0023] Furthermore, the second groove is arranged inside the transition layer.

[0024] Based on the above technical solution, the second groove is not easy to interfere with the surface flatness of the transition layer, which is easy to process later. At the same time, the second groove is arranged close to the supporting layer, which is conducive to the interlayer slip near the interface, thereby facilitating the release of stress at the interface of the bending zone.

[0025] The method for preparing the conductive film comprises the following steps:

[0026] S1 provides a support layer, and forms a first groove on one side of the bending area corresponding to the bending direction;

[0027] S2 provides a transition layer, forming a matching structure with the first groove in the bending area, so that it is not easy to deform;

[0028] S3 forms a conductive layer at least on the surface of the transition layer.

[0029] Furthermore, the thickness of the support layer is set to 3-20 μm.

[0030] Furthermore, the thickness of the transition layer is set to 0.1-5 μm.

[0031] Based on the above technical solution, the support layer is selected to have an appropriate thickness. If it is too thin, it is not conducive to continuous processing and the strength cannot be guaranteed; if it is too thick, it will affect the overall thickness of the conductive film and is not conducive to thinning.

[0032] The thickness of the transition layer is set appropriately to facilitate processing, but it will not be too thick, which will lead to poor interlayer slip effect and affect stress release. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0034] Figure 1 It is a schematic diagram of the cross-sectional structure when the conductive film is flattened;

[0035] Figure 2 for Figure 1 Schematic diagram of the structure after the conductive film is bent;

[0036] In the figure:

[0037] 1-support layer; 11-first groove; 2-transition layer; 21-second groove; 3-conductive layer;

[0038] 10-bending area; 20-non-bending area.

[0039] Figure 1 The horizontal direction corresponds to the longitudinal direction of the film. DETAILED DESCRIPTION

[0040] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0041] Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.

[0042] In the prior art, due to the different bending radii of the metal layer and the polymer layer, the stress generated on the metal layer due to bending is greater. On the inner side of the bending area, due to the smaller bending radius, the stress between the base film and the conductive layer on the bending side is greater, the stress cannot be released, the stress concentration problem is more serious, and it is easy to crack or delaminate. Especially in the battery manufacturing process, there are multiple processes such as coating, rolling, and winding, as well as the thermal expansion effect during the use of the finished battery, which will aggravate the stress concentration problem at the bend.

[0043] In view of the above situation, some embodiments of the present application disclose a conductive film, including a support layer 1 and a transition layer 2 formed on the surface of the support layer 1 corresponding to the bending area 10, and at least a conductive layer 3 is formed on the surface of the transition layer 2;

[0044] Among them, the transition layer 2 in the bending area 10 has a first relative displacement L1 with the conductive layer 3 after bending, that is, for AA', and the transition layer 2 in the non-bending area 20 has a second relative displacement L2 with the conductive layer 3 after bending, that is, corresponding to BB', and satisfies L2 greater than L1.

[0045] The setting of the transition layer 2 increases the bending radius of the bending side to a certain extent; and because the transition layer 2 has a relatively larger deformation in the non-bending zone 20 and a small deformation in the bending zone 10, after bending, the stress generated in the bending zone can be released through the interlayer slippage of the non-bending zone with a large relative displacement, which can reduce the situation where the stress in the bending zone is excessively concentrated to a certain extent.

[0046] Reference Figure 1-2 By controlling the transition layer 2 to have different deformation amounts (displacement amounts) in the bending zone 10 and the non-bending zone 20 after bending.

[0047] Specifically,

[0048] In the bending area 10, corresponding to the bending direction, that is, corresponding to Figure 1 A transition layer 2 is arranged above the support layer 1, and a plurality of first grooves 11 are arranged on the surface of the support layer 1 corresponding to the bending area 10 on one side in the bending direction. When the transition layer 2 is connected to the surface of the support layer 1, the corresponding part of the transition layer 2 is arranged in the first groove 11 to form a matching structure.

[0049] In some embodiments of the present application, the first groove 11 is an array-shaped notch structure; at this time, due to the cooperation between the transition layer 2 and the support layer 1, they can cooperate with each other during the bending process, and the support layer 1 and the transition layer form a mutual anchor, so that the transition layer 2 in the bending zone 10 is relatively difficult to slip, and the generated stress can be released by sliding between the layers of the non-bending zone 20, thereby reducing the problem of easy delamination and cracking in the bending zone due to excessive concentration of stress and inability to release.

[0050] In some other embodiments of the present application, the first groove 11 may also be configured as a strip-shaped groove structure.

[0051] There is no specific limitation on the cross-sectional shape of the first groove 11 , as long as the supporting layer 1 has a concave groove structure.

[0052] In addition, the groove depth of the first groove 11 should not exceed 1 / 3 of the thickness of the supporting layer in order not to have too great an impact on the strength of the supporting layer, and the groove width is preferably not greater than 2 mm.

[0053] Considering further improving the stress release capability, the transition layer 2 of the non-bending area 20 has a second groove 21. Providing the groove in the transition layer 2 of the non-bending area 20 can further improve the deformation capability of the transition layer 2 in the non-bending area 20 and reduce the modulus, so that the stress generated in the bending area after bending can be better released through the non-bending area.

[0054] In some embodiments of the present application, the second groove 21 is arranged on the inner side of the transition layer 2 and does not penetrate outward; specifically, the second groove 21 is arranged inwardly on the connection side with the support layer 1, so that the second groove 21 has a smaller modulus on this side, thereby making it easier to produce interlayer slip.

[0055] The present application also discloses a method for preparing the above conductive film, comprising the following steps:

[0056] S1 provides a support layer 1, and forms a first groove 11 on one side of the bending area corresponding to the bending direction;

[0057] S2 provides a transition layer 2, which forms a matching structure with the first groove in the bending area to prevent deformation;

[0058] S3 forms a conductive layer 3 at least on the surface of the transition layer.

[0059] The support layer material is selected from polymer film materials, such as at least one of polyamide, polyethylene terephthalate, polyimide, polyethylene, polypropylene, polystyrene, polyvinyl chloride, acrylonitrile-butadiene-styrene copolymer, polybutylene terephthalate, poly(p-phenylene terephthalamide), polypropylene, polyoxymethylene, polytetrafluoroethylene or polycarbonate, preferably polypropylene (PP), polyethylene terephthalate (PET), polyimide (PI) or a composite film thereof; its thickness is set to 3-20 μm, preferably 4-10 μm.

[0060] The first groove 11 can be formed by hot rolling of a rolling mold, that is, a protruding die head is formed on the surface of the roller body, and the die head is made to contact the surface of the support layer in a heated state, thereby forming the first groove; of course, etching methods such as laser or chemical etching can also be selected.

[0061] The material of the transition layer 2 has a smaller elastic modulus than that of the support layer material; the transition layer material can be formed by coating, such as selecting polyvinylidene fluoride, polytetrafluoroethylene, SBR, water-based epoxy resin, polyacrylic resin, polyvinyl alcohol, etc., and coating after diluting to an appropriate viscosity with a suitable solvent; or commercially available conventional polymer film materials can be selected, and the transition layer film materials can be hot-pressed and bonded to the surface of the support layer material by hot (pressing) compounding, so that the transition layer material is partially rolled and embedded into the formed first groove 11. The thickness of the transition layer is preferably set to 0.1-5μm.

[0062] The conductive layer 3 can be formed by vacuum plating or by coating a conductive paste.

[0063] In addition, for the formation of the second groove 21, a film material can be selected and pre-processed to form the second groove corresponding to the non-bending area, wherein the second groove can be processed by a method similar to roll forming, and then further bonded to the surface of the support layer by a film thermal composite method. The roll pressure and temperature can be selected in combination with the actual film material, which belongs to the existing conventional processing means and will not be described in detail.

[0064] As for the second groove 21 being arranged in the middle of the transition layer, the second groove 21 may adopt a multi-layer composite structure, that is, one or some transition layer membrane materials are firstly bonded, and then the remaining membrane materials are composited after the second groove is formed.

[0065] The thickness of the conductive layer 3 can be set according to actual needs, such as controlling the thickness of the conductive layer according to the required square resistance. The conductive layer can be made of metal, such as copper, aluminum, nickel, chromium, etc.

[0066] In the description of the present invention, it is to be understood that the terms “center”, “longitudinal”, “lateral”, “length”, “width”, “thickness”, “up”, “down”, “front”, “back”, “left”, “right”, “vertical”, “horizontal”, “top”, “bottom”, “inside”, “outside”, “clockwise”, “counterclockwise”, “axial”, “radial”, “circumferential”, etc., indicating orientations or positional relationships based on the orientations or positional relationships shown in the drawings or conventionally expressed in the prior art, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0067] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists, A and B exist at the same time, and B exists. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0068] The term "multiple" as used in this application refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple sheets" refers to more than two sheets (including two sheets).

[0069] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A conductive film, characterized in that: It includes a support layer and a transition layer formed on the surface of the support layer corresponding to the bending area, and at least a conductive layer is formed on the surface of the transition layer; The transition layer in the bending zone has a first relative displacement L1 with the conductive layer after bending, and the transition layer in the non-bending zone has a second relative displacement L2 with the conductive layer after bending, and L2 is greater than L1.

2. The conductive film according to claim 1, wherein The elastic modulus of the transition layer is smaller than that of the supporting layer.

3. The conductive film according to claim 1 or 2, characterized in that: The support layer and the transition layer form an anchoring structure in the bending zone.

4. The conductive film according to claim 3, wherein: A transition layer is arranged in the bending area corresponding to the bending direction, a plurality of first grooves are arranged on the surface of the support layer corresponding to the bending area on one side in the bending direction, the transition layer is connected to the surface of the support layer, and part of the transition layer is arranged in the first groove to form a matching structure.

5. The conductive film according to claim 4, wherein: The first groove is a groove structure in an array shape; and / or, The first groove is a strip-shaped groove structure.

6. The conductive film according to claim 5, wherein: The depth of the first groove does not exceed 1 / 3 of the thickness of the support layer; and / or, The groove width is not greater than 2mm.

7. The conductive film according to any one of claims 2, 4 to 6, characterized in that: A plurality of second grooves are arranged in the transition layer in the non-bending region.

8. The conductive film according to claim 7, wherein: The second groove is arranged on the inner side of the transition layer.

9. A method for preparing a conductive film, characterized in that: The steps include: S1 provides a support layer, and forms a first groove on one side of the bending area corresponding to the bending direction; S2 provides a transition layer, forming a matching structure with the first groove in the bending area, so that it is not easy to deform; S3 forms a conductive layer at least on the surface of the transition layer.

10. The conductive film according to claim 9, wherein The thickness of the support layer is set to 3-20 μm; and / or, The thickness of the transition layer is set to 0.1-5 μm.

Citation Information

Cited By

  • Battery cell, battery device and electric device

    CN120749250A

  • Battery cell, battery device, and electric device

    CN120749250B