Forming method of arc-surface ultra-thin composite wire
By pretreating the electrical contact layer material and the substrate layer material and thermal composite or roll welding, the mold is continuously drawn to form an arc-surface ultra-thin composite wire, the problem of waste and low utilization efficiency of precious metals in the prior art is solved. It achieves efficient conductivity and stability, suitable for high-performance electronic and electrical applications.
Patent Information
- Application Number
- CN202411076260.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, when manufacturing ultra-thin composite wires, it is difficult to accurately control the thickness of the electrical contact layer material, resulting in waste of precious metals and low utilization efficiency, and gold plating on the side of the product causes unnecessary waste.
By pre-treating the electrical contact layer material and the substrate layer material into rectangular lines, thermal composite or roller welding is performed, the mold is continuously drawn to form an arc-surface ultra-thin composite wire, precisely controlling the thickness of the composite wire, reducing the use of precious metals and increasing the use of high-quality metals Utilization.
It realizes precise control of the thickness of the electrical contact layer material, reduces the use of precious metals, improves the utilization rate of precious metals, ensures the conductivity and stability of the wire, and is suitable for high-performance electronic and electrical applications.
Smart Images

Figure CN118919166A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of gold plating and composite materials, and in particular to a method for forming an ultra-thin composite wire with a circular arc surface. Background Art
[0002] Arc surface ultra-thin composite wire is a special-shaped electrical contact material with an arc-shaped working surface, generally made of ultra-thin precious metals. This material is usually composed of two or three layers of materials. The electrical contact layer is usually composed of ultra-thin precious metals such as gold and palladium and their alloys that meet various performance requirements; the middle layer is generally composed of silver, nickel and their alloys; the base layer is usually composed of silver, copper, nickel and their alloys with good welding and conductive properties.
[0003] Electrical contact materials are key materials for electrical contact components in equipment such as automobiles, communications, industrial electronics, and household appliances. They are widely used in weak-current applications such as automotive relays, thermostats, communication relays, keyboards, micro switches, and circuit controllers that require high reliability, small size, and high integration. Their main function is to guide current and transmit information.
[0004] With the rapid development of electronic information technology, the demand for electrical contact components is increasing, resulting in an increase in the consumption of composite electrical contact materials. At the same time, the public's concern for natural resources and the environment is increasing. The gradual depletion of natural resources requires us to use resources rationally and improve the utilization and recovery rate of precious metals. Therefore, saving precious metals has become an important task. This requires designers of electrical contact components to save the use of precious metals from the product design stage, and also requires processors to improve the utilization rate of precious metals so that the cross-sectional shape of composite wires is as close to the design requirements as possible.
[0005] When manufacturing ultra-thin composite wires at present, the thickness of the electrical contact layer material is usually between 0.001-0.01 mm, and the thickness of the substrate layer material is even thicker, generally in the range of 0.1-3 mm.
[0006] Regarding the control of the thickness of the electrical contact layer material, if the gold plating process is used, although the thickness can be precisely controlled, gold will also be plated on both sides of the product, which will cause unnecessary waste, and if the gold plating time is too long, the efficiency will not be improved. Summary of the invention
[0007] The technical problem to be solved by the present invention is to overcome the defects of the prior art and provide a method for forming an ultra-thin composite wire with a circular arc surface.
[0008] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0009] The present invention provides a method for forming an ultra-thin composite wire with a circular arc surface, comprising the following steps:
[0010] Step 1): pre-processing the electrical contact layer material into a rectangular thin wire;
[0011] Step 2): pre-processing the base layer material into a rectangular wire;
[0012] Step 3): Compounding the electrical contact layer material and the substrate layer material into a composite wire;
[0013] Step 4): The composite wire is continuously drawn through a die into a desired arc-surface ultra-thin composite wire.
[0014] As a preferred technical solution of the present invention, the pretreatment in step 1) and step 2) is any combination of wire drawing and rolling, and then annealing and cleaning.
[0015] As a preferred technical solution of the present invention, the bonding method in step 3) is thermal bonding or roller welding to bond two independent wires together.
[0016] As a preferred technical solution of the present invention, in step 3), the thickness H5 of the composite wire is 90% of the sum of the thickness H2 of the material and the thickness H4 of the material.
[0017] As a preferred technical solution of the present invention, the specific operation of continuous wire drawing in step 4) is: first annealing, then multiple wire drawing using a die to gradually thin the wire, and finally cleaning.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1: The present invention precisely controls the rolling and wire drawing processes, as well as appropriate annealing treatment, so that the formed wire has good bending strength and elastic modulus, ensuring stability and durability during use. The use of precious metals such as gold, palladium and their alloys as electrical contact layers ensures that the wire has extremely low resistivity, thereby providing excellent conductive properties and is suitable for high-performance electronic and electrical applications.
[0020] 2: The present invention reduces the use of precious metals and reduces costs through precise thickness control and composite processes, especially in the use of electrical contact layers, which contributes to the sustainable use of resources, meets environmental protection requirements, and improves the utilization rate of precious metals.
[0021] 3: The present invention ensures that the arc radius and surface finish of the wire meet high standards, which helps to reduce contact resistance, improve contact performance, and meet high-precision application scenarios. The prepared wire is suitable for the fields of automobiles, communications, industrial electronics, household appliances, etc., especially for weak current occasions with high reliability requirements, small size, and high integration, such as automotive relays, thermostats, communication relays, keyboards, micro switches, circuit controllers, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0023] Figure 1 Schematic diagram of material combination in the embodiment;
[0024] Figure 2 is a cross-sectional view of the electrical contact layer material and a rectangular thin line of the present invention;
[0025] Figure 3 is a cross-sectional view of the substrate layer material and rectangular lines of the present invention;
[0026] Figure 4 is a cross-sectional view of the composite wire of the present invention;
[0027] Figure 5 This is a cross-sectional view of the arc-surface ultra-thin composite wire of the present invention;
[0028] In the figure: 1. Electric contact layer material; 2. Rectangular thin wire; 3. Base layer material; 4. Rectangular wire; 5. Composite wire; 6. Arc surface ultra-thin composite wire. DETAILED DESCRIPTION
[0029] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0030] like Figure 1-5 As shown, the present invention provides a method for forming an ultra-thin composite wire with a circular arc surface, comprising the following steps:
[0031] Step 1): pre-processing the electrical contact layer material 1 into a rectangular thin wire 2, wherein the pre-processing includes: firstly wire drawing, rolling, and then any combination of annealing and cleaning processes;
[0032] Step 2): pre-processing the base layer material 3 into a rectangular wire 4, wherein the pre-processing includes: firstly wire drawing, rolling, and then any combination of annealing and cleaning processes;
[0033] Step 3): Compound the electrical contact layer material 2 and the base layer material 4 into a composite wire 5 by thermal compounding or roller welding, so that the two independent wires are combined together, such as Figure 1 As shown;
[0034] Step 4): The composite wire 5 is continuously drawn through a die into the required arc surface ultra-thin composite wire 6, the thickness H5 of the composite wire 5 is 90% of the sum of the thickness H2 of the material 2 and the thickness H4 of the material 4, and the specific operation of continuous drawing is: first annealing, then using a die to draw multiple times to make the wire gradually thinner, and finally cleaning.
[0035] The following are examples of ultra-thin composite wires made of different materials:
[0036] Example 1
[0037] This embodiment is an ultra-thin composite wire with a circular arc surface made of gold (Au) and silver-nickel alloy (AgNi10):
[0038] Step 1: First, process the electrical contact layer material:
[0039] The incoming Au material is Φ0.2mm and needs to be flat-rolled to 1.9±0.02*0.0063mm. The process is as follows:
[0040] Treat the Au material to remove surface dirt;
[0041] Select rollers with high hardness and good surface finish to reduce the wear on the Au material;
[0042] The rolling speed is in the range of 10-30m / min, and the rolling temperature is controlled between room temperature and 200℃;
[0043] The Au material is gradually thinned to the target thickness through multiple rolling passes, and the material thickness is monitored in real time using an online thickness detection instrument to ensure that it is within the tolerance range;
[0044] After rolling is completed, the finished product is inspected in terms of appearance, size, performance, etc. to ensure that it meets the requirements;
[0045] The flat strip material after flat rolling is cleaned with deionized water to remove surface dirt and impurities, and finally vacuum dried or nitrogen protected dried, and then prepared for thermal composite treatment.
[0046] Step 2: Process the base layer material again;
[0047] The incoming material of AgNi10 is Φ3.5mm, and it is required to be drawn to 2.5*2.5mm. The process is as follows:
[0048] Perform visual inspection on the AgNi10 wire and remove the surface oxide layer and stains;
[0049] Prepare a series of wire drawing dies with decreasing diameters to gradually reduce the wire diameter;
[0050] According to the characteristics of AgNi10 material, the wire is preheated to reduce its deformation resistance;
[0051] Adjust the speed of the wire drawing machine within the range of 10-50m / min;
[0052] Use appropriate lubricants during the wire drawing process to reduce die wear and material breakage;
[0053] After AgNi10 material is drawn several times to approach the target size, a special square wire forming die is used to draw the wire into a 2.5*2.5mm square wire;
[0054] After wire drawing is completed, the finished product is inspected in terms of appearance, size, performance, etc. to ensure that it meets the requirements;
[0055] The square wire after drawing is cleaned with deionized water to avoid corrosion to the AgNi10 material. After removing tiny pollutants and grease on the surface of the square wire, hot air drying or vacuum drying is used to ensure that there is no water mark on the surface of the wire. After processing, prepare for thermal composite treatment.
[0056] Step 3: The two treated materials are thermally composited. The size of Au is 1.9*0.0063 mm, the size of AgNi10 is 2.5*2.5 mm, and Au is located above AgNi10. The size of the composite material after thermal composite is 2.5*2.256 mm. The process is as follows:
[0057] Prepare thermal lamination equipment, including a heat press, a heating device, and a pressure control device;
[0058] Place the Au film (1.9*0.0063mm) on top of the AgNi10 square wire (2.5*2.5mm);
[0059] Set the thermal composite parameters, the temperature is between 300-500℃, and the pressure is between 10-50MPa;
[0060] Heating to a predetermined temperature and maintaining it for a period of time to allow the two materials to be compounded under pressure;
[0061] After reaching the set time, slowly cool to room temperature and maintain pressure until the material is completely solidified;
[0062] After thermal compounding, the size of the composite material is 2.5*2.256mm;
[0063] Use deionized water to clean the surface of the composite material to remove oil and pollutants, and then use ultrasonic cleaning to improve the cleaning effect;
[0064] The composite material is placed in an annealing furnace for annealing. The atmosphere inside the annealing furnace is an inert gas. The annealing temperature is between 300-500°C. The heat preservation time is 1-2 hours. The composite material is slowly cooled to room temperature to eliminate internal stress.
[0065] According to the final product size requirements, a series of wire drawing dies are prepared. Appropriate lubricants are used during the wire drawing process to reduce die wear and material breakage. After wire drawing, the size decreases in sequence, and the size decreases in sequence to 2.0*1.8mm, 1.8*1.7mm, and 1.65*1.6mm;
[0066] After wire drawing is completed, use deionized water or an ultrasonic cleaner to clean the material again, and then store it after drying.
[0067] Finished product inspection data: surface finish Ra0.4, no cracks, dust, oil, burrs, etc., bending strength 220MPa, torsion test positive 8 reverse 16 without delamination, resistivity 3.72×10 -8 Ω·m.
[0068] Example 2
[0069] This embodiment is an ultra-thin composite wire with a circular arc surface made of palladium (Pd) and silver-nickel alloy (AgNi10):
[0070] Step 1: First, process the electrical contact layer material:
[0071] The incoming Pd material is Φ0.15mm and needs to be flat-rolled to 1.8±0.02*0.005mm. The process is as follows:
[0072] Treat the Pd wire to remove surface dirt;
[0073] Prepare rolls suitable for Pd material rolling, and arrange appropriate rolling passes according to wire diameter and target thickness;
[0074] The rolling speed is in the range of 10-30m / min, and the rolling temperature is controlled between room temperature and 200℃;
[0075] The Pd material is gradually thinned to the target thickness through multiple rolling passes, and the material thickness is monitored in real time using an online thickness detection instrument to ensure that it is within the tolerance range;
[0076] The flat-rolled Pd strip is placed on the conveyor belt of the annealing furnace, and the annealing temperature is set to 800°C and the speed is set to 8m / min. During the annealing process, the atmosphere in the furnace is kept as an inert gas;
[0077] After annealing, use deionized water or weak acid cleaning agent to clean the annealed Pd strip, then use ultrasonic cleaning to improve the cleaning effect, and finally use hot air drying or vacuum drying to ensure that there is no water mark on the surface of the material. After processing, prepare for thermal composite treatment.
[0078] Step 2: Process the base layer material again;
[0079] The incoming material of AgNi10 is Φ3.5mm, and it is required to be drawn to 2.2*2.2mm. The process is as follows:
[0080] Perform visual inspection on the AgNi10 wire and remove the surface oxide layer and stains;
[0081] Prepare a series of wire drawing dies with decreasing diameters to gradually reduce the wire diameter;
[0082] According to the characteristics of AgNi10 material, the wire is preheated to reduce its deformation resistance;
[0083] Adjust the speed of the wire drawing machine within the range of 10-50m / min;
[0084] Use appropriate lubricants during the wire drawing process to reduce die wear and material breakage;
[0085] After AgNi10 material is drawn several times to approach the target size, a special square wire forming die is used to draw the wire into a 2.2*2.2mm square wire;
[0086] After wire drawing is completed, the finished product is inspected in terms of appearance, size, performance, etc. to ensure that it meets the requirements;
[0087] The square wire after drawing is cleaned with deionized water to avoid corrosion to the AgNi10 material. After removing tiny pollutants and grease on the surface of the square wire, hot air drying or vacuum drying is used to ensure that there is no water mark on the surface of the wire. After processing, prepare for thermal composite treatment.
[0088] Step 3: The two treated materials are subjected to thermal composite treatment. The wire size of Pd is 1.8*0.005mm, and the wire size of AgNi10 is 2.2*2.2mm. Pd is located above AgNi10. The size of the composite material after thermal composite is 2.2*1.98mm. The process is as follows:
[0089] Prepare thermal lamination equipment, including a heat press, a heating device, and a pressure control device;
[0090] Place the Pd film (1.8*0.005mm) on top of the AgNi10 square wire (2.2*2.2mm);
[0091] Set the thermal composite parameters, the temperature is between 300-500℃, and the pressure is between 10-50MPa;
[0092] Heating to a predetermined temperature and maintaining it for a period of time to allow the two materials to be compounded under pressure;
[0093] After reaching the set time, slowly cool to room temperature and maintain pressure until the material is completely solidified;
[0094] After thermal lamination, the size of the composite material is 2.2*1.98mm;
[0095] Use deionized water to clean the surface of the composite material to remove oil and pollutants, and then use ultrasonic cleaning to improve the cleaning effect;
[0096] The composite material is placed in an annealing furnace for annealing. The atmosphere inside the annealing furnace is an inert gas. The annealing temperature is between 300-500°C. The heat preservation time is 1-2 hours. The composite material is slowly cooled to room temperature to eliminate internal stress.
[0097] According to the final product size requirements, a series of wire drawing dies are prepared. Appropriate lubricants are used during the wire drawing process to reduce die wear and material breakage. The wire drawing size is reduced in sequence, and the size is reduced in sequence to 2.0*1.7mm, 1.7*1.6mm, and 1.6*1.5mm;
[0098] After wire drawing is completed, use deionized water or an ultrasonic cleaner to clean the material again, and then store it after drying.
[0099] Finished product inspection data: surface finish Ra0.4, no cracks, dust, oil, burrs, etc., bending strength 220MPa, torsion test positive 8 reverse 16 without delamination, resistivity 6.22×10 -8 Ω·m.
[0100] Example 3
[0101] This embodiment is an ultra-thin composite wire with a circular arc surface made of gold (Au) and copper (Cu):
[0102] Step 1: First, process the electrical contact layer material:
[0103] The incoming Au material is Φ0.2mm and needs to be flat-rolled to 2.0±0.02*0.0063mm. The process is as follows:
[0104] Treat the Au material to remove surface dirt;
[0105] Select rollers with high hardness and good surface finish to reduce the wear on the Au material;
[0106] The rolling speed is in the range of 10-30m / min, and the rolling temperature is controlled between room temperature and 200℃;
[0107] The Au material is gradually thinned to the target thickness through multiple rolling passes, and the material thickness is monitored in real time using an online thickness detection instrument to ensure that it is within the tolerance range;
[0108] After rolling is completed, the finished product is inspected in terms of appearance, size, performance, etc. to ensure that it meets the requirements;
[0109] The flat strip material after flat rolling is cleaned with deionized water to remove surface dirt and impurities, and finally vacuum dried or nitrogen protected dried, and then prepared for thermal composite treatment.
[0110] Step 2: Process the base layer material again;
[0111] Cu material shaping, incoming Φ4.0mm material is drawn to 3.0*3.0mm, then to 2.4*2.4mm, and then annealed to eliminate stress during processing, and finally cleaned and prepared for thermal composite treatment;
[0112] The incoming Cu material is Φ4.0mm and needs to be drawn to 2.4*2.4mm. The process is as follows:
[0113] Perform visual inspection on the Cu wire and remove the surface oxide layer and stains;
[0114] Prepare a series of wire drawing dies with decreasing diameters to gradually reduce the wire diameter;
[0115] Adjust the speed of the wire drawing machine within the range of 10-50m / min;
[0116] Use appropriate lubricants during the wire drawing process to reduce die wear and material breakage;
[0117] After the Cu material is drawn several times to approach the target size, a special square wire forming die is used to draw the wire into a 2.4*2.4mm square wire;
[0118] After wire drawing is completed, the finished product is inspected in terms of appearance, size, performance, etc. to ensure that it meets the requirements;
[0119] The square wire after drawing is cleaned with deionized water to avoid corrosion to the Cu material. After removing tiny pollutants and grease on the surface of the square wire, it is dried with hot air or vacuum to ensure that there is no water mark on the surface of the wire. After processing, it is prepared for thermal composite treatment.
[0120] Step 3: The two treated materials are thermally composited. The size of Au is 2.0*0.0063 mm, the size of Cu is 2.4*2.4 mm, Au is located above Cu, and the size of the composite material after thermal composite is 2.5*2.256 mm. The process is as follows:
[0121] Prepare thermal lamination equipment, including a heat press, a heating device, and a pressure control device;
[0122] Place the Au film (1.9*0.0063mm) on top of the Cu square wire (2.4*2.4mm);
[0123] Set the thermal composite parameters, the temperature is between 300-500℃, and the pressure is between 10-50MPa;
[0124] Heating to a predetermined temperature and maintaining it for a period of time to allow the two materials to be compounded under pressure;
[0125] After reaching the set time, slowly cool to room temperature and maintain pressure until the material is completely solidified;
[0126] After thermal compounding, the composite material size is 2.5*2.165mm;
[0127] Use deionized water to clean the surface of the composite material to remove oil and pollutants, and then use ultrasonic cleaning to improve the cleaning effect;
[0128] The composite material is placed in an annealing furnace for annealing. The atmosphere inside the annealing furnace is inert gas. The annealing temperature is between 350-500°C. The heat preservation time is 1-2 hours. The composite material is slowly cooled to room temperature to eliminate internal stress.
[0129] According to the final product size requirements, a series of wire drawing dies are prepared. Appropriate lubricants are used during the wire drawing process to reduce die wear and material breakage. After wire drawing, the size decreases in sequence, and the size decreases in sequence to 2.2*1.9mm, 1.9*1.8mm, and 1.8*1.7mm;
[0130] After wire drawing is completed, use deionized water or an ultrasonic cleaner to clean the material again, and then store it after drying.
[0131] Finished product inspection data: surface finish Ra0.4, no cracks, dust, oil, burrs, etc., bending strength 210MPa, torsion test positive 8 reverse 16 without delamination, resistivity 2.06×10 -8 Ω·m.
[0132] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for forming an ultra-thin composite wire with an arc surface, characterized in that: The following steps are involved: Step 1): pre-processing the electrical contact layer material (1) into a rectangular thin wire (2); Step 2): pre-processing the base layer material (3) into a rectangular wire (4); Step 3): Compounding the electrical contact layer material (2) and the base layer material (4) into a composite wire (5); Step 4): The composite wire (5) is continuously drawn through a die into a desired arc-surface ultra-thin composite wire (6).
2. The method for forming an ultra-thin composite wire with an arc surface according to claim 1, characterized in that: The pretreatment in step 1) and step 2) is any combination of wire drawing and rolling, and then annealing and cleaning.
3. The method for forming an ultra-thin composite wire with an arc surface according to claim 1, characterized in that: The bonding method in step 3) is thermal bonding or roller welding, so that two independent wires are bonded together.
4. The method for forming an ultra-thin composite wire with an arc surface according to claim 3, characterized in that: In the step 3), the thickness (H5) of the composite wire (5) is 90% of the sum of the thickness (H2) of the material (2) and the thickness (H4) of the material (4).
5. The method for forming an ultra-thin composite wire with a circular arc surface according to claim 1, characterized in that: The specific operation of continuous wire drawing in step 4) is: first annealing, then multiple wire drawing using a die to gradually thin the wire, and finally cleaning.
Citation Information