Isotropic lanthanum-cerium-yttrium-iron-boron bonded magnetic powder and preparation method thereof
By optimizing the proportions and boron compositions of lanthanum, cerium, yttrium and boron compositions, combined with vacuum induction fast quenching technology, lanthanum cerium yttrium iron boron bonded magnetic powder without praseodymium neodymium dysprosium is developed, which solves the cost-effectiveness and magnetic performance of existing magnetic powder materials. The problem of stability achieves high-performance and low-cost magnetic components production.
Patent Information
- Application Number
- CN202411340346.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-08
AI Technical Summary
The existing magnetic powder materials have shortcomings in terms of cost-effectiveness and magnetic properties. The development and application of high-abundance lanthanum, cerium, and yttrium rare earth metals have not been fully utilized, resulting in high production costs of magnetic components and unstable magnetic properties.
By optimizing the doping combination of lanthanum, cerium, yttrium, boron composition and high melting point metal, combined with vacuum induction fast quenching technology, isotropic lanthanum cerium yttrium iron boron bonded magnetic powder without praseodymium neodymium dysprosium and rare precious metals and The manufacturing method is to form magnetic powder mainly composed of lanthanum, cerium and yttrium, with high magnetic energy accumulation and low price.
Achieve cost-effective magnetic powder material, fills the performance gap between bonded ferrite and neodymium iron boron powder, provides a stable low-cost magnetic component solution, meets the working needs within 100°C, and is optimized through process Improves thermal demagnetization performance.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the preparation of rare earth materials, and in particular to the composition and preparation method of a rare earth lanthanum, cerium, yttrium, iron and boron bonded magnetic powder material. Background Art
[0002] Bonded magnetic powder (such as ferrite bonded magnetic powder and NdFeB bonded magnetic powder) is widely used in the production of magnetic components such as computer hardware, home appliances, automobiles and consumer electronics because of its high resistance, convenient one-piece molding, and can be made into thin-walled magnetic rings and multi-pole magnetization.
[0003] The market needs a magnetic powder with high cost performance. Isotropic ferrite bonded magnetic powder has low price, but also low magnetic properties, usually around 1-2 magnetic energy products. NdFeB bonded magnetic powder usually has magnetic properties around 8-16 magnetic energy products, but high price. However, the stock of praseodymium-neodymium rare earth metals is not high, and the price fluctuates greatly, which affects its large-scale promotion and application.
[0004] At present, it has been discovered that the reserves of high-abundance lanthanum, cerium and yttrium rare earth metals are large, the prices are low and the magnetic properties are stable. The technical development and application of lanthanum, cerium and yttrium permanent magnets have become the focus of market attention. Summary of the invention
[0005] In view of the above problems, the purpose of the present invention is to disclose an isotropic lanthanum-cerium-yttrium-iron-boron bonded magnetic powder and a preparation method thereof. The present invention develops a series of bonded magnetic powders free of rare and precious metals of praseodymium, neodymium and dysprosium and a preparation method thereof by optimizing the ratio of lanthanum, cerium and yttrium, the participation of boron components, the doping combination of high melting point metals, and the combination of vacuum induction rapid quenching technology. The bonded magnetic powder has lanthanum, cerium and yttrium as main components, has a high magnetic energy product, and has a low price due to its large stock.
[0006] Therefore, the first object of the present invention is to provide an isotropic LaCeYFeB bonded magnetic powder, the main components and weight percentages of which are expressed as follows: x (La-Ce) y B z M f Fe 余 , wherein Y represents yttrium, the content x is 0-10wt%, (La-Ce) represents lanthanum-cerium mixed rare earth, the content y is 20-28.5wt%, B represents boron, the content z is 1-1.8wt%, and M represents one or a mixture of two or more of zirconium, titanium, niobium, and aluminum, and the content f is 0-5wt%.
[0007] Furthermore, the total amount of other rare earth elements allowed in the composition is ≤ 0.5 wt%.
[0008] Furthermore, in the (La—Ce) lanthanum-cerium mixed rare earth, La / (La—Ce)≤35wt%.
[0009] Furthermore, the phase structure of the magnetic powder is composed of the main phase Re 2 Fe 14 B tetragonal phase and Fe 3 B, nano-α-Fe, rare earth-rich phase; among them, the main phase Re 2 Fe 14 B The grain size is between 10-80nm.
[0010] The second object of the present invention is to provide a method for preparing the above-mentioned bonded magnetic powder, and its technical solution is:
[0011] 1) Prepare raw materials according to the following composition and content: yttrium, content is 0-10wt%, lanthanum cerium mixed rare earth, content is 20-28.5wt%, and La / (La-Ce)≤35wt%; boron, content is 1-1.8wt%, one or more of zirconium, titanium, niobium, aluminum, the total is 0-5wt%, and the rest is electrical pure iron;
[0012] 2) melting the raw materials in a vacuum furnace and casting them into ingots;
[0013] 3) placing the ingot in a vacuum induction rapid quenching furnace, spraying it onto a high-speed rotating water-cooled molybdenum wheel after melting, and throwing out alloy strips;
[0014] 4) crushing and sieving the alloy strips, and subjecting the crushed powders below the set standard mesh size to crystallization treatment;
[0015] 5) The crushed powder after crystallization treatment becomes qualified magnetic powder after passing the magnetic test.
[0016] Wherein, the vacuum induction rapid quenching furnace works in an argon atmosphere, and the working pressure is between 600-2000Pa.
[0017] The ingot is first melted in a smelting crucible, then transferred into a heat-insulating crucible for temperature adjustment, and then sprayed onto a water-cooled molybdenum wheel.
[0018] Among them, the melting crucible temperature is 200-300℃, and the insulation crucible temperature is 150-200℃.
[0019] The heat-insulating crucible is above the water-cooled molybdenum wheel and has two kinds of movements, vertical radial and horizontal radial, relative to the water-cooled molybdenum wheel. The water-cooled molybdenum wheel has two kinds of movements, rotation and axial telescopic.
[0020] Among them, the alloy strip is thrown out after being water-cooled once on the water-cooled molybdenum wheel, hits the water-cooled target, is water-cooled twice and broken once, and then falls into a collecting mechanism; after being broken twice in the collecting mechanism, it enters a rotating cooling mechanism; after being water-cooled three times and broken three times in the rotating cooling mechanism, it is discharged.
[0021] The crystallization process is carried out in a flowing argon atmosphere, the argon pressure is 0.01-0.02 MPa, the crystallization process temperature is 550-780°C, and the process speed is 60-100 Kg / Hr.
[0022] The advantages of the present invention are:
[0023] 1. The magnetic powder of the present invention does not contain rare precious metals such as praseodymium, neodymium and dysprosium, and has high cost performance, low production cost and stable price.
[0024] 2. The magnetic energy product of magnetic powder is 4-8, which fills the gap between bonded ferrite and bonded NdFeB powder.
[0025] 3. After composition optimization and process optimization, the magnetic powder has excellent thermal demagnetization performance and can meet the working requirements of magnetic components within 100°C.
[0026] 4. Magnetic powder is mainly composed of high-abundance lanthanum and cerium elements, and the problem of unbalanced use of rare earth elements has been solved with breakthrough innovations in technology and the market.
[0027] 5. The present invention uses original vacuum induction equipment for production, with advanced technology and stable quality. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the described embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.
[0029] It should also be noted that the terms used in this specification are only for describing specific embodiments and are not intended to limit certain embodiments. For example, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form; in addition, it should be understood that when the terms "comprise" and "include" are used in this specification, they indicate the presence of features, steps, operations, devices, components and / or their combinations.
[0030] In this embodiment, the present invention first introduces an isotropic lanthanum-cerium-yttrium-iron-boron bonded magnetic powder material, the main components and weight percentages of which are expressed as follows: x (La-Ce) y B z M f Fe 余, where Y represents the element yttrium, with a content of x; (La-Ce) represents the element lanthanum-cerium mixed rare earth, with a content of y; B represents the element boron, with a content of z; M represents one or more elements of zirconium, titanium, niobium, and aluminum, with a content of f; the remainder is iron, which is taken from electrical pure iron. Other rare earth elements are allowed in the magnetic powder, but the total amount cannot exceed 0.5wt%.
[0031] In this component, by weight percentage, x: 0-10wt%, y: 20-28.5wt%, z: 1-1.8wt%, f: 0-5wt%. Because the main contribution of lanthanum, cerium and yttrium is reflected, the content is higher.
[0032] It is also important to note that in the (La-Ce) lanthanum-cerium mixed rare earth, La / (La-Ce) does not exceed 35wt%; and the B element content is not less than 1wt%, which are important features of the present invention.
[0033] In addition, from the perspective of the phase structure of the material, the phase structure of the magnetic powder is mainly Re 2 Fe 14 B tetragonal phase and Fe 3 B, nano-α-Fe phase, rare earth-rich phase. Among them, the main phase Re 2 Fe 14 B The grain size is between 10-80nm.
[0034] On the other hand, the present invention provides a production method for manufacturing lanthanum, cerium, yttrium, rare earth, iron and boron bonded magnetic powder according to the above-mentioned component ratio, which comprises the following steps.
[0035] 1) Prepare the raw materials according to the above composition and content requirements, among which the yttrium content is 0-10wt%, the lanthanum-cerium mixed rare earth content is 20-28.5wt%, and La / (La-Ce)≤35wt%; the boron content is 1-1.8wt%, one or more of zirconium, titanium, niobium, and aluminum are combined, the total is 0-5wt%, and the rest is Fe, using electrical pure iron. Other rare earth elements are allowed, but the total amount cannot exceed 0.5wt%;
[0036] 2) melting the above raw materials in a vacuum furnace and casting them into ingots weighing 40-50 kg;
[0037] 3) The qualified ingot is placed in a vacuum induction rapid quenching furnace, melted under vacuum conditions, and then sprayed onto a high-speed rotating water-cooled molybdenum wheel to throw out alloy strips;
[0038] 3) The alloy strip hits the water-cooled target and breaks into pieces, then falls into the receiving mechanism, which is equipped with a crushing device;
[0039] 4) The alloy strips are quenched and crushed, and the powders below the set standard mesh size (such as 40 mesh) are sieved and crystallized;
[0040] 5) After the magnetic test confirms that it is qualified, the mixed batch is evenly mixed to become the finished magnetic powder.
[0041] Furthermore, the vacuum induction quenching furnace can work under a constant argon atmosphere with a working pressure between 600-2000 Pa. The alloy structure and properties obtained under argon protection are better.
[0042] Furthermore, the ingot is first melted in a melting crucible, then transferred to a heat-insulating crucible for temperature adjustment, and then sprayed onto a water-cooled molybdenum wheel. The melting crucible temperature is preferably 200-300°C, and the heat-insulating crucible temperature is preferably 150-200°C. The heat-insulating crucible is maintained at a crucible temperature by an energized coil under electromagnetic induction.
[0043] Furthermore, the heat preservation crucible is provided with a high-frequency heating nozzle for spraying. The high-frequency heating nozzle is composed of a boron nitride nozzle and a graphite sleeve. The boron nitride nozzle is embedded in the graphite sleeve. The graphite sleeve is heated by a high-frequency induction current, and the heat is transferred to the boron nitride nozzle, thereby ensuring the stability of the solution. Boron nitride has stable physical properties, is resistant to rapid heating and cooling, has a high melting point, and is not easy to react with rare earth metals. Among them, the nozzle throat diameter is between 0.8-1.5mm.
[0044] Furthermore, the insulating crucible is above the water-cooled molybdenum wheel. By setting the insulating crucible to perform vertical radial and horizontal radial movements relative to the water-cooled molybdenum wheel, and setting the water-cooled molybdenum wheel to perform rotational movement accompanied by axial telescopic movement, the molten alloy is evenly sprayed onto the water-cooled molybdenum wheel.
[0045] Furthermore, the linear speed of the water-cooled molybdenum wheel is controlled between 25 and 45 m / sec to ensure that the thickness of the swung thin strip is uniform and moderate.
[0046] Furthermore, the alloy strip collides with a water-cooled target, the target surface of which forms an angle of 45° with the direction in which the alloy flakes are thrown out, and the alloy flakes are shattered by the collision with the water-cooled target and fall vertically into the collecting mechanism.
[0047] Furthermore, the end of the material receiving mechanism is also connected to a rotary cooling mechanism, and the end of the rotary cooling mechanism is connected to the material receiving tank. The main body of the rotary cooling mechanism is a rotary tube, a crushing device is also arranged in the rotary tube, and a water cooling jacket is arranged on the periphery of the rotary tube.
[0048] This vacuum induction quenching process is completed under three-stage water cooling conditions: water-cooled molybdenum wheel, water-cooled target, and rotary cooling mechanism. The alloy strip is the magnetic powder obtained after three crushings by water-cooled target, collecting mechanism, and rotary cooling mechanism. Three times of water cooling and three times of crushing make the powder crushed and cooled evenly, and the obtained alloy structure has better performance.
[0049] Furthermore, the crystallization process is carried out under the protection of argon gas flowing in the crystallization furnace, and the argon gas pressure is between 0.01-0.02MPa. The crystallization process temperature is between 550-780°C. The crystallization process is carried out continuously, and the process speed is: 60-100Kg / Hr.
[0050] The present invention obtains an alloy material mainly composed of lanthanum, cerium and yttrium and supplemented by boron by reasonably setting the alloy composition and proportion. The alloy material is subjected to a high-temperature vacuum rapid quenching process to obtain thin strip fragments, the alloy phase changes, and has a very high magnetic energy product.
[0051] The following is an example of the alloy performance of the obtained lanthanum-cerium-yttrium-iron-boron bonded magnetic powder.
[0052] Wherein: the composition is expressed in weight percentage (wt%); Br: remanence, unit: KGs; Hcj: intrinsic coercivity, unit: KOe; (BH)max: maximum magnetic energy product, unit: MGOe.
[0053] Embodiment 1:
[0054] The three materials numbered 1, 2, and 3 were tested for remanence, intrinsic coercivity, and maximum magnetic energy product. The data in this table show that the magnetic properties of the three materials are very high.
[0055]
[0056] Embodiment 2:
[0057] The specified weight of magnetic powder (La-Ce: 26, B: 1.35, Zr: 2.5, Fe: rest) was added with 2wt% epoxy resin in proportion, and then dried at 60℃ to remove the solvent. The fixed weight was weighed and pressed into a Q10X10 column with a density of 6.0g / cm 3 , saturation magnetization, then measure the initial magnetic flux, and test the thermal demagnetization rate at different temperatures. The data in this table proves that the thermal demagnetization rate of the material is very good below 100°C, and the thermal demagnetization performance is excellent (the thermal demagnetization rate within 24 hours is less than 2%, but after 100°C, the thermal demagnetization rate has a substantial increase, reaching 3.88%.
[0058]
Claims
1. An isotropic lanthanum-cerium-yttrium-iron-boron bonded magnetic powder, Features: The main components and weight percentage are expressed as: Y x (La-Ce) y B z M f Fe 余 , wherein Y represents yttrium, the content x is 0-10wt%, (La-Ce) represents lanthanum-cerium mixed rare earth, the content y is 20-28.5wt%, B represents boron, the content z is 1-1.8wt%, and M represents one or a mixture of two or more of zirconium, titanium, niobium, and aluminum, and the content f is 0-5wt%.
2. The isotropic lanthanum-cerium-yttrium-iron-boron bonded magnetic powder according to claim 1, Features: The total amount of other rare earth elements allowed is ≤0.5wt%.
3. The isotropic lanthanum-cerium-yttrium-iron-boron bonded magnetic powder according to claim 1, Features: In the (La-Ce) lanthanum-cerium mixed rare earth, La / (La-Ce)≤35wt%.
4. The isotropic lanthanum-cerium-yttrium-iron-boron bonded magnetic powder according to claim 1, Features: The phase structure of the magnetic powder is composed of the main phase Re 2 Fe 14 B tetragonal phase and Fe 3 B, nano-α-Fe, rare earth-rich phase; among them, the main phase Re 2 Fe 14 B The grain size is between 10-80nm.
5. A method for preparing the isotropic lanthanum-cerium-yttrium-iron-boron bonded magnetic powder according to any one of claims 1 to 4, It is characterized in that The steps include: 1) Prepare raw materials according to the following composition and content: yttrium, content is 0-10wt%, lanthanum cerium mixed rare earth, content is 20-28.5wt%, and La / (La-Ce)≤35wt%; boron, content is 1-1.8wt%, one or more of zirconium, titanium, niobium, aluminum, the total is 0-5wt%, and the rest is electrical pure iron; 2) melting the raw materials in a vacuum furnace and casting them into ingots; 3) placing the ingot in a vacuum induction rapid quenching furnace, spraying it onto a high-speed rotating water-cooled molybdenum wheel after melting, and throwing out alloy strips; 4) crushing and sieving the alloy strips, and subjecting the crushed powders below the set standard mesh size to crystallization treatment; 5) The crushed powder after crystallization treatment becomes qualified magnetic powder after passing the magnetic test.
6. The method for preparing isotropic lanthanum-cerium-yttrium-iron-boron bonded magnetic powder according to claim 5, It is characterized in that The vacuum induction rapid quenching furnace operates in an argon atmosphere with an operating pressure between 600-2000Pa.
7. The method for preparing isotropic LaCeYFeB bonded magnetic powder according to claim 5, It is characterized in that The ingot is first melted in a smelting crucible, then transferred into a heat-insulating crucible for temperature adjustment, and then sprayed onto a water-cooled molybdenum wheel; Among them, the melting crucible temperature is 200-300℃, and the insulation crucible temperature is 150-200℃.
8. The method for preparing isotropic LaCeYFeB bonded magnetic powder according to claim 5, It is characterized in that The heat-insulating crucible is above the water-cooled molybdenum wheel and has two kinds of movements, vertical radial and horizontal radial, relative to the water-cooled molybdenum wheel. The water-cooled molybdenum wheel has two kinds of movements, rotation and axial telescopic.
9. The method for preparing isotropic LaCeYFeB bonded magnetic powder according to claim 5, It is characterized in that The alloy strip is thrown out after being water-cooled once on the water-cooled molybdenum wheel, hits the water-cooled target, is water-cooled twice and broken once, and then falls into a collecting mechanism; after being broken twice in the collecting mechanism, it enters a rotating cooling mechanism; after being water-cooled three times and broken three times in the rotating cooling mechanism, it is discharged.
10. The method for preparing isotropic LaCeYFeB bonded magnetic powder according to claim 5, It is characterized in that The crystallization treatment is carried out in a flowing argon atmosphere, the argon pressure is 0.01-0.02MPa, the crystallization treatment temperature is 550-780°C, and the treatment speed is: 60-100Kg / Hr.