Small-size high-saturation-current inductor and production process thereof

Through the use of double-layer insulating coating and specific adhesives and lubricants, combined with the T-core core and copper wire winding process, the technical difficulties of the inductor in small size, high saturation current and high strength are solved, and the technical difficulties of the inductor are realized. The efficient magnetic performance and stability improvement meet the needs of high-end applications.

CN118919203APending Publication Date: 2024-11-08SHENZHEN TOPSUN TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411043079.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-08

Smart Images

  • Figure BDA0004972850230000071
    Figure BDA0004972850230000071
Patent Text Reader

Abstract

The invention relates to the technical field of inductor preparation, and particularly discloses a small-size and high-saturation-current inductor and a production process thereof. A small-size and high-saturation-current inductor comprises a magnetic core, a winding copper wire and insulating paint, and the magnetic core is prepared from, by weight, 50-70 parts of metal magnetic powder, 1-3 parts of binder and 1-3 parts of lubricant; the metal magnetic powder is coated with a magnesium oxide insulating layer and a silicon oxide insulating layer; according to the inductor with the small size and the high saturation current, the strength and the saturation current of the inductor material are improved through the synergistic effect of all the components and the combination of all the preparation processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of inductor preparation, and in particular to an inductor with a small size and a high saturation current and a production process thereof. Background Art

[0002] In the field of mobile phones and PC applications, the stability of the power supply is crucial. Controllable saturation inductors are widely used because they can control the duty cycle and output power of the switching power supply, thereby achieving stable voltage output. However, the inductors currently on the market have disadvantages such as low saturation current and large size, which cannot meet the needs of high-end applications.

[0003] At present, there are technical difficulties in manufacturing small-sized, high-saturation current, and high-strength inductors. For one-piece molded inductors, if the molding pressure is too small, the density of the magnetic part in the inductor will be low and the initial magnetic permeability will be small, thus failing to achieve the required electromagnetic properties; if the molding pressure is too large, the winding inside the magnetic powder will be subjected to excessive extrusion pressure, and the insulation layer on the surface of the enameled copper wire will be damaged due to friction, resulting in low insulation withstand voltage or even short circuit of the product, and high risk of product reliability. Summary of the invention

[0004] In order to improve the problems of low saturation current and large size of existing inductors, the present application provides an inductor with small size and high saturation current and a production process thereof.

[0005] In the first aspect, the present application provides an inductor with a small size and a high saturation current, adopting the following technical solution: an inductor with a small size and a high saturation current, comprising a magnetic core, a wound copper wire and an insulating paint, wherein the magnetic core comprises the following raw materials in parts by weight: 50-70 parts of metal magnetic powder, 1-3 parts of a binder, and 1-3 parts of a lubricant; the metal magnetic powder is coated with a double insulating layer of magnesium oxide and silicon oxide.

[0006] By adopting the above technical solution, the metal magnetic powder is double-layered for insulation coating, which can enhance the insulation of the inductor, optimize the distribution and arrangement of the magnetic powder, increase the magnetic flux density, and thus improve the saturation current capacity of the inductor. At the same time, the double-layer design also reduces the risk of friction damage to the single-layer inductor insulation layer. The magnesium oxide and silicon oxide insulation layers have good thermal stability and can effectively reduce the temperature of the inductor when working at high currents, thereby reducing the decline in the magnetic properties of the inductor due to temperature increases, and thus improving the saturation current capacity of the inductor.

[0007] Preferably, the metal magnetic powder is FeSiCr powder.

[0008] By adopting the above technical solution, FeSiCr powder has a higher saturation flux density and can withstand a larger DC bias current, thereby improving the saturation current capability of the inductor. FeSiCr powder can provide better magnetic permeability, reduce the loss of the inductor at high frequencies, and help improve the efficiency and stability of the inductor.

[0009] Preferably, the binder is one of phenolic resin, epoxy resin and silicone resin.

[0010] By adopting the above technical solution, phenolic resin, epoxy resin and silicone resin as binders can fix and protect the core material, significantly enhance the strength of the core, and promote the core to maintain structural stability under high current and high frequency, thereby improving the mechanical strength of the inductor. Phenolic resin, epoxy resin and silicone resin as binders can enhance the filling degree and structural density of the core, reduce magnetic flux leakage, and increase the inductor saturation current.

[0011] Preferably, the lubricant is one of zinc stearate, magnesium stearate and calcium stearate.

[0012] By adopting the above technical solution, zinc stearate, magnesium stearate and calcium stearate are used as lubricants, which can reduce the friction between the magnetic core and the coil, reduce wear, ensure the integrity of the magnetic core and the coil, and improve the durability and reliability of the inductor.

[0013] Preferably, the insulating varnish comprises the following raw materials in parts by weight: 30-50 parts of epoxy resin, 30-40 parts of cellulose nitrate, 100-120 parts of solvent, and 1-5 parts of curing agent.

[0014] By adopting the above technical solution, the epoxy resin has strong adhesion, thermal stability and electrical insulation, which can protect the inductor material and improve the stability of the inductor material. The cellulose nitrate has good flexibility and insulation performance, which can reduce the cracking of the insulating paint on the surface of the inductor, and can enhance the adhesion between the insulating paint and the substrate, ensuring that the insulating paint is firmly attached to the surface of the inductor and is not easy to fall off, thereby improving the stability of the inductor insulation layer.

[0015] Preferably, the insulating varnish further comprises 20-30 parts of polyimide and 3-5 parts of epoxy coupling agent.

[0016] By adopting the above technical solution, polyimide has good heat resistance and low temperature resistance, which can enable the inductor material to maintain high stability at high and low temperatures. At the same time, polyimide can enhance the hardness and wear resistance of the insulating paint, and improve the mechanical strength and impact resistance of the inductor material. The use of epoxy coupling agent can promote the better combination of polyimide and epoxy resin, and improve the uniformity of the insulating paint.

[0017] In a second aspect, the present application provides a production process for an inductor with a small size and a high saturation current, which adopts the following technical solution: A production process of a small-size, high-saturation-current inductor includes the following specific steps: A sol-gel method is used to pre-coat a magnesium oxide insulating layer on the surface of the metal magnetic powder, and then a silicon oxide insulating layer is coated to obtain the insulation-coated metal magnetic powder. The insulation-coated metal magnetic powder, a binder, and a lubricant are mixed and pressed into shape to obtain a T-core magnetic core. After copper wire is wound on the T-core magnetic core, powder filling hot pressing and baking are performed, and then insulation paint is sprayed, paint is stripped, and electroplating is performed to obtain a finished inductor.

[0018] By adopting the above technical solution, pressing to form a T-core magnetic core and winding copper wire on the T-core magnetic core, the prepared inductor material has a firm structure and precise characteristics, which can well realize the miniaturization and integration of the inductor and improve the preparation efficiency and reliability of the inductor.

[0019] Preferably, the pressure of the T-core magnetic core during pressing is 3-10T / cm 2 The density of the T-core magnetic core after pressing is 5.5-7.5g / cm 3 .

[0020] By adopting the above technical solution, the pressing pressure of the magnetic core is adjusted within a reasonable range, which can promote the magnetic core to be better formed and have a better density.

[0021] Preferably, the metal magnetic powder is pre-treated by catalytic heat treatment, mechanical crushing and air flow crushing.

[0022] By adopting the above technical solution, the metal magnetic powder is pre-treated in advance, so that magnetic powder with a small particle size and uniform distribution can be obtained, thereby meeting the requirements of small-size inductors.

[0023] Preferably, the electroplating is to electroplating a layer of copper or silver in the electrode region of the finished inductor.

[0024] In summary, this application has the following beneficial effects: 1. Since the present application adopts double-layer insulation coating of metal magnetic powder, the insulation of the inductor can be enhanced, the magnetic flux density can be increased, and the saturation current capacity of the inductor can be improved. The magnesium oxide and silicon oxide insulation layers can be used to reduce the problem of the inductor's magnetic properties decreasing due to the increase in temperature, thereby improving the saturation current capacity of the inductor.

[0025] 2. In this application, phenolic resin, epoxy resin and silicone resin are used as binders. When added to the magnetic core material, the strength of the magnetic core can be enhanced, the magnetic core can maintain structural stability under high current and high frequency, the damage rate of the inductor during use can be reduced, and the reliability of the inductor can be improved. Zinc stearate, magnesium stearate and calcium stearate are used as lubricants to reduce friction between the magnetic core and the coil, reduce wear, ensure the integrity of the magnetic core and the coil, and improve the service life of the inductor product. DETAILED DESCRIPTION

[0026] The present application is further described in detail below with reference to the embodiments.

[0027] All raw materials in the examples are commercially available. Example

[0028] Example 1 This embodiment provides a small-size, high-saturation current inductor, including a magnetic core, a wound copper wire and an insulating paint. The magnetic core includes the following raw materials by weight: 60 kg of metal magnetic powder, 2 kg of binder, and 2 kg of lubricant. The metal magnetic powder is FeSiCr powder, and the Fe mass content of the FeSiCr powder is 78%, the Si mass content is 9%, and the Cr mass content is 11%; the binder is phenolic resin FRJ-551, the lubricant is zinc stearate, and the insulating paint is commercially available Nacheng insulating paint 1042 epoxy insulating paint.

[0029] The production process of small size, high saturation current inductor includes the following specific steps: S1: The FeSiCr powder is subjected to embrittlement heat treatment at 420°C for 60 minutes, and then mechanical grinding and air flow grinding are used to obtain FeSiCr powder with an average particle size of 10 μm; ethanol is used to dissolve magnesium diethylate, and the mass ratio of ethanol to magnesium diethylate is 20:1, and then water is added, and the mass ratio of water to ethanol is 1:20, and stirred evenly to obtain a mixed solution A, and then ammonium hydroxide is dropped into it, and heated at 50°C to form a gel, and then the gel is mixed with the FeSiCr powder, and steamed. After the solvent is evaporated, it is dried and the FeSiCr powder is heated at 500°C for 5h to coat a layer of magnesium oxide insulation layer on the surface of the metal magnetic powder; the sodium silicate aqueous solution is mixed with oil, the sodium silicate concentration in the sodium silicate aqueous solution is 2.5 mol / L, the mass ratio of the sodium silicate aqueous solution to oleic acid is 10:1, and they are stirred evenly to form a mixed solution B, and then the metal magnetic powder coated with the magnesium oxide insulation layer is added to the mixed solution B, and then sulfuric acid is dripped into it, and the water bath is heated to 60°C, and the reaction is carried out for 6h to obtain the metal magnetic powder with double-layer insulation coating.

[0030] S2: Mix the metal magnetic powder, binder and lubricant after insulation coating at 5T / cm 2 The average density was 6.5 g / cm3 The T-core magnetic core is wound with copper wire and then filled with powder. It is hot-pressed and baked at 300℃, and then sprayed with insulating paint, stripped, and electroplated with copper to obtain the finished inductor.

[0031] Example 2 The difference between Example 2 and Example 1 is that the amount of metal magnetic powder used in the magnetic core raw material is 50 kg, the amount of binder used is 1 kg, and the amount of lubricant used is 1 kg.

[0032] Example 3 The difference between Example 3 and Example 1 is that the amount of metal magnetic powder used in the magnetic core raw material is 70 kg, the amount of binder used is 3 kg, and the amount of lubricant used is 3 kg.

[0033] Example 4 The difference between Example 4 and Example 1 is that the adhesive in the magnetic core material is epoxy resin.

[0034] Example 5 The difference between Example 5 and Example 1 is that the lubricant in the magnetic core raw material is calcium stearate.

[0035] Example 6 The difference between Example 6 and Example 1 is that the insulating paint comprises the following raw materials in parts by weight: 40 kg of epoxy resin, 35 kg of cellulose nitrate, 110 kg of solvent, and 3 kg of curing agent. The curing agent is m-xylene diamine, the solvent is xylene, and the epoxy resin is E-12.

[0036] The production process of small size, high saturation current inductor includes the following specific steps: S1: Mix epoxy resin and cellulose nitrate, then add solvent and curing agent, mix and stir evenly to obtain insulating paint.

[0037] S2: The FeSiCr powder is subjected to embrittlement heat treatment at 420°C for 60 minutes, and then mechanical grinding and air flow grinding are used to obtain FeSiCr powder with an average particle size of 10 μm; ethanol is used to dissolve magnesium diethylate, and the mass ratio of ethanol to magnesium diethylate is 20:1, and then water is added, and the mass ratio of water to ethanol is 1:20, and stirred evenly to obtain a mixed solution A, and then ammonium hydroxide is dropped into it, and heated at 50°C to form a gel, and then the gel is mixed with the FeSiCr powder, and steamed. After the solvent is evaporated, it is dried and the FeSiCr powder is heated at 500°C for 5h to coat a layer of magnesium oxide insulation layer on the surface of the metal magnetic powder; the sodium silicate aqueous solution is mixed with oil, the sodium silicate concentration in the sodium silicate aqueous solution is 2.5 mol / L, the mass ratio of the sodium silicate aqueous solution to oleic acid is 10:1, and they are stirred evenly to form a mixed solution B, and then the metal magnetic powder coated with the magnesium oxide insulation layer is added to the mixed solution B, and then sulfuric acid is dripped into it, and the water bath is heated to 60°C, and the reaction is carried out for 6h to obtain the metal magnetic powder with double-layer insulation coating.

[0038] S3: Mix the metal magnetic powder, binder and lubricant after insulation coating at 5T / cm 2 The average density was 6.5 g / cm 3 The T-core magnetic core is wound with copper wire and then filled with powder. It is hot-pressed and baked at 300℃, and then sprayed with insulating paint, stripped, and electroplated with copper to obtain the finished inductor.

[0039] Example 7 The difference between Example 7 and Example 6 is that the amount of epoxy resin used in the insulating paint raw material is 30 kg, the amount of cellulose nitrate used is 40 kg, the amount of solvent used is 100 kg, and the amount of curing agent used is 1 kg.

[0040] Example 8 The difference between Example 8 and Example 6 is that the amount of epoxy resin used in the insulating paint raw material is 50 kg, the amount of cellulose nitrate used is 30 kg, the amount of solvent used is 120 kg, and the amount of curing agent used is 5 kg.

[0041] Example 9 The difference between Example 9 and Example 6 is that the insulating paint raw material further includes 25 kg of polyimide, and the polyimide is GI001.

[0042] The production process of small size, high saturation current inductor includes the following specific steps: S1: Epoxy resin, cellulose nitrate and polyimide are mixed, and then a solvent and a curing agent are added, mixed and stirred evenly to obtain an insulating paint.

[0043] S2: The FeSiCr powder is subjected to embrittlement heat treatment at 420°C for 60 minutes, and then mechanical grinding and air flow grinding are used to obtain FeSiCr powder with an average particle size of 10 μm; ethanol is used to dissolve magnesium diethylate, and the mass ratio of ethanol to magnesium diethylate is 20:1, and then water is added, and the mass ratio of water to ethanol is 1:20, and stirred evenly to obtain a mixed solution A, and then ammonium hydroxide is dropped into it, and heated at 50°C to form a gel, and then the gel is mixed with the FeSiCr powder, and steamed. After the solvent is evaporated, it is dried and the FeSiCr powder is heated at 500°C for 5h to coat a layer of magnesium oxide insulation layer on the surface of the metal magnetic powder; the sodium silicate aqueous solution is mixed with oil, the sodium silicate concentration in the sodium silicate aqueous solution is 2.5 mol / L, the mass ratio of the sodium silicate aqueous solution to oleic acid is 10:1, and they are stirred evenly to form a mixed solution B, and then the metal magnetic powder coated with the magnesium oxide insulation layer is added to the mixed solution B, and then sulfuric acid is dripped into it, and the water bath is heated to 60°C, and the reaction is carried out for 6h to obtain the metal magnetic powder with double-layer insulation coating.

[0044] S3: Mix the metal magnetic powder, binder and lubricant after insulation coating at 5T / cm 2 The average density was 6.5 g / cm 3 The T-core magnetic core is wound with copper wire and then filled with powder. It is hot-pressed and baked at 300℃, and then sprayed with insulating paint, stripped, and electroplated with copper to obtain the finished inductor.

[0045] Example 10 The difference between Example 10 and Example 9 is that the insulating paint raw material further includes 4 kg of epoxy coupling agent, wherein the epoxy coupling agent is KH560.

[0046] The production process of small size, high saturation current inductor includes the following specific steps: S1: Epoxy resin, cellulose nitrate, polyimide and epoxy coupling agent are mixed, and then solvent and curing agent are added, mixed and stirred evenly to obtain insulating paint.

[0047] S2: The FeSiCr powder is subjected to embrittlement heat treatment at 420°C for 60 minutes, and then mechanical grinding and air flow grinding are used to obtain FeSiCr powder with an average particle size of 10 μm; ethanol is used to dissolve magnesium diethylate, and the mass ratio of ethanol to magnesium diethylate is 20:1, and then water is added, and the mass ratio of water to ethanol is 1:20, and stirred evenly to obtain a mixed solution A, and then ammonium hydroxide is dropped into it, and heated at 50°C to form a gel, and then the gel is mixed with the FeSiCr powder, and steamed. After the solvent is evaporated, it is dried and the FeSiCr powder is heated at 500°C for 5h to coat a layer of magnesium oxide insulation layer on the surface of the metal magnetic powder; the sodium silicate aqueous solution is mixed with oil, the sodium silicate concentration in the sodium silicate aqueous solution is 2.5 mol / L, the mass ratio of the sodium silicate aqueous solution to oleic acid is 10:1, and they are stirred evenly to form a mixed solution B, and then the metal magnetic powder coated with the magnesium oxide insulation layer is added to the mixed solution B, and then sulfuric acid is dripped into it, and the water bath is heated to 60°C, and the reaction is carried out for 6h to obtain the metal magnetic powder with double-layer insulation coating.

[0048] S3: Mix the metal magnetic powder, binder and lubricant after insulation coating at 5T / cm 2 The average density was 6.5 g / cm 3 The T-core magnetic core is wound with copper wire and then filled with powder. It is hot-pressed and baked at 300℃, and then sprayed with insulating paint, stripped, and electroplated with copper to obtain the finished inductor.

[0049] Embodiment 11 The difference between Example 11 and Example 10 is that the amount of polyimide used in the insulating paint raw material is 20 kg, and the amount of epoxy coupling agent used is 5 kg.

[0050] Example 12 The difference between Example 12 and Example 10 is that the amount of polyimide used in the insulating paint raw material is 30 kg, and the amount of epoxy coupling agent used is 3 kg.

[0051] Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the metal magnetic powder of the magnetic core raw material is only coated with a magnesium oxide insulating layer.

[0052] The production process of small size, high saturation current inductor includes the following specific steps: S1: The FeSiCr powder is subjected to embrittlement heat treatment at 420°C for 60 minutes of holding time, and then mechanical grinding and air flow grinding are used to obtain FeSiCr powder with an average particle size of 10 μm; ethanol is used to dissolve magnesium diethoxide, and the mass ratio of ethanol to magnesium diethoxide is 20:1, and then water is added, and the mass ratio of water to ethanol is 1:20, and stirred evenly to obtain a mixed solution A, and then ammonium hydroxide is dropped into it, and heated at 50°C to form a gel, and then the gel is mixed with the FeSiCr powder, and after the solvent is evaporated, it is dried, and then the FeSiCr powder is heated at 500°C for 5 hours, that is, a layer of magnesium oxide insulating layer is coated on the surface of the metal magnetic powder.

[0053] S2: Mix the metal magnetic powder, binder and lubricant after insulation coating at 5T / cm 2 The average density was 6.5 g / cm 3 The T-core magnetic core is wound with copper wire and then filled with powder. It is hot-pressed and baked at 300℃, and then sprayed with insulating paint, stripped, and electroplated with copper to obtain the finished inductor.

[0054] Performance testing According to the small-size, high-saturation-current inductors provided in Examples 1-12 of the present application and Comparative Example 1, the following performance tests were performed, and the specific test results are shown in Table 1.

[0055] Detection Methods 1. Inductance and DC resistance At 0.25V and 100kHz, 20 samples were taken and the average inductance value of the inductance material prepared in the present application was measured using an inductance meter. The DC resistance of the inductance material prepared in the present application was measured using a DC resistance tester. The saturation current of the inductance material prepared in the present application was measured using a voltage-current method.

[0056] 2. Strength The tensile strength of the inductor material prepared in this application was tested using a universal tensile machine.

[0057] Table 1: Performance test results data table From the performance test results, it can be seen that the inductor material prepared in the present application has high strength and high saturation current capability. By comparing Comparative Example 1 with Example 1, it can be seen that the strength and saturation current of the inductor material prepared in Comparative Example 1 using a single-layer insulation layer to coat the metal magnetic powder will also be affected, which further illustrates that the single-layer insulation layer has limited effect on improving the metal magnetic powder and is also prone to reduce the saturation current of the inductor.

[0058] In Examples 6-8, the sterilization paint prepared in the present application can provide better protection for the inductor and improve the stability of the inductor performance under the synergistic effect of various components. In Examples 9-12, appropriate amounts of polyimide and epoxy coupling agent are added to the sterilization paint raw materials. From the performance test results, it can be seen that the inductor material has good strength and impact resistance, which prolongs the service life of the inductor material.

[0059] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An inductor with small size and high saturation current, characterized in that: The invention comprises a magnetic core, a wound copper wire and an insulating paint. The magnetic core comprises the following raw materials in parts by weight: 50-70 parts of metal magnetic powder, 1-3 parts of a binder and 1-3 parts of a lubricant. The metal magnetic powder is coated with a double insulating layer of magnesium oxide and silicon oxide.

2. The inductor with small size and high saturation current according to claim 1, characterized in that: The metal magnetic powder is FeSiCr powder.

3. The small-size, high-saturation-current inductor according to claim 1, characterized in that: The binder is one of phenolic resin, epoxy resin and silicone resin.

4. The inductor with small size and high saturation current according to claim 1, characterized in that: The lubricant is one of zinc stearate, magnesium stearate and calcium stearate.

5. The small-size, high-saturation-current inductor according to claim 1, characterized in that: The insulating paint comprises the following raw materials in parts by weight: 30-50 parts of epoxy resin, 30-40 parts of cellulose nitrate, 100-120 parts of solvent and 1-5 parts of curing agent.

6. The inductor with small size and high saturation current according to claim 1, characterized in that: The insulating paint also includes 20-30 parts of polyimide and 3-5 parts of epoxy coupling agent.

7. A process for producing a small-size, high-saturation-current inductor according to any one of claims 1 to 6, characterized in that: The specific steps include: A sol-gel method is used to pre-coat a magnesium oxide insulating layer on the surface of the metal magnetic powder, and then a silicon oxide insulating layer is coated to obtain the insulation-coated metal magnetic powder. The insulation-coated metal magnetic powder, a binder, and a lubricant are mixed and pressed into shape to obtain a T-core magnetic core. After copper wire is wound on the T-core magnetic core, powder filling hot pressing and baking are performed, and then insulation paint is sprayed, paint is stripped, and electroplating is performed to obtain a finished inductor.

8. The process for producing a small-size, high-saturation-current inductor according to claim 7, characterized in that: The pressure of the T-core magnetic core pressing is 3-10T / cm 2 The density of the T-core magnetic core after pressing is 5.5-7.5g / cm 3 .

9. The process for producing a small-size, high-saturation-current inductor according to claim 7, characterized in that: The metal magnetic powder is preliminarily subjected to catalytic heat treatment, mechanical crushing and air flow crushing treatment.

10. The process for producing a small-size, high-saturation-current inductor according to claim 7, characterized in that: The electroplating is to electroplating a layer of copper or silver in the electrode area of ​​the finished inductor.

Citation Information

Cited By

  • Multifunctional binder for aluminum electrolysis as well as preparation method and application of multifunctional binder

    CN119931510A