Preparation method of thick-film silicon carbide epitaxy
Through the alternating epitaxial layer growth method, the problem of uneven distribution of N elements in the silicon carbide epitaxial is solved, and the uniformity of the thick film silicon carbide epitaxial and the reduction of device voltage are achieved, which is suitable for the manufacturing of high-power devices.
Patent Information
- Application Number
- CN202411006347.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing thick film process, the longitudinal doping concentration distribution of N elements during epitaxial growth of silicon carbide is uneven, resulting in the problem of high forward voltage of the device.
The alternating epitaxial layer growth method is adopted, including multiple nitrogen doping and non-doping growth cycles, adjusting each growth time and gas flow to improve the distribution uniformity of N elements, and forming a thick film silicon carbide epitaxial with a thickness of 100-200μm. .
It significantly improves the uniformity of the growth direction distribution of N elements in the epitaxial layer, reduces the forward voltage of the device, and is suitable for the preparation of high-power devices.
Smart Images

Figure CN118919401A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silicon carbide epitaxy, and in particular to a method for preparing thick-film silicon carbide epitaxy. Background Art
[0002] Silicon carbide epitaxial wafer refers to a silicon carbide wafer on which a single crystal thin film with certain requirements and the same crystal structure as the substrate, i.e., an epitaxial layer, is grown on the original silicon carbide substrate. Epitaxial growth mainly uses chemical vapor deposition equipment or molecular beam epitaxy equipment.
[0003] For example, CN107075728A discloses a method for epitaxial growth of silicon carbide, in which hydrocarbon gas and silicon raw material gas are supplied to a silicon carbide single crystal substrate in a manner such that a C / Si ratio is in the range of greater than 0.5 and less than 1.5, and a thermal CVD method is used to react them at a temperature of greater than 1500°C and less than 1800°C, thereby forming a silicon carbide thin film on the silicon carbide single crystal substrate.
[0004] However, since silicon carbide devices are manufactured directly on the epitaxial layer, the quality of the epitaxy directly affects the performance and yield of the device. As the voltage resistance required by the device continues to increase, the corresponding epitaxial layer thickness becomes thicker and the control difficulty becomes higher. Generally, when the voltage is around 600V, the required epitaxial layer thickness is about 6μm; when the voltage is between 1200-1700V, the required epitaxial layer thickness reaches 10-15μm. If the voltage reaches more than 10,000 volts, an epitaxial layer thickness of more than 100μm may be required. As the thickness of the epitaxial layer continues to increase, it becomes increasingly difficult to control the thickness, concentration uniformity, and defect density.
[0005] However, in order to increase the breakdown voltage, a thick epitaxial layer, good surface morphology and low doping concentration are necessary. Some high-voltage bipolar devices require an epitaxial film thickness of more than 50 μm and a doping concentration of less than 5×10 15 cm -3 For high reverse voltage high power devices, a very thick, low doping concentration epitaxial layer needs to be grown on a 4H-SiC substrate. In order to make a 10KW high power device, the thickness of the epitaxial layer must reach more than 100μm.
[0006] However, the existing thick film process is carried out by increasing the growth time on the basis of the thin film process. However, there is a serious N memory effect in the reaction chamber during the growth process of this method, which leads to uneven distribution of the actual longitudinal doping concentration of the N element during the epitaxial growth of the thick film N-type SiC, showing a trend of gradually increasing. The MCV for measuring the carrier concentration can only test the concentration at a depth of 1.5μm from the surface, while the concentration at the bottom is low, resulting in a high forward voltage of the device.
[0007] In summary, the existing thick film process still has the defect that the actual longitudinal doping concentration distribution of the N element is uneven during the epitaxial growth of the thick film N-type SiC, resulting in a high forward voltage of the device. Summary of the invention
[0008] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for preparing thick-film silicon carbide epitaxy to solve the defect that the actual longitudinal doping concentration distribution of the N element during the epitaxial growth of thick-film N-type SiC is uneven, resulting in a high forward voltage of the device.
[0009] To achieve this object, the present invention adopts the following technical solutions:
[0010] The present invention provides a method for preparing thick-film silicon carbide epitaxy, the method comprising: sequentially performing high-temperature etching, buffer layer growth, epitaxial layer growth and drift layer growth on a silicon carbide substrate to obtain thick-film silicon carbide epitaxy;
[0011] Wherein, the epitaxial layer growth includes the first nitrogen-doped growth, the first non-doped growth, the second nitrogen-doped growth, the second non-doped growth, the third nitrogen-doped growth, the third non-doped growth, the fourth nitrogen-doped growth, the fourth non-doped growth, the fifth nitrogen-doped growth, the fifth non-doped growth, the sixth nitrogen-doped growth and the sixth non-doped growth in sequence; the time of the first nitrogen-doped growth> the time of the second nitrogen-doped growth> the time of the third nitrogen-doped growth> the time of the fourth nitrogen-doped growth> the time of the fifth nitrogen-doped growth> the time of the sixth nitrogen-doped growth;
[0012] The thickness of the epitaxial layer in the thick film silicon carbide epitaxy is 100-200 μm.
[0013] The preparation method provided by the present invention adopts a specially designed epitaxial layer growth process and an alternating growth method, which significantly improves the uniformity of the concentration distribution of the N element in the growth direction during epitaxial growth, thereby avoiding the problem of high forward voltage of the device.
[0014] As a preferred technical solution of the present invention, the thick film silicon carbide epitaxy comprises a silicon carbide substrate and a buffer layer, an epitaxial layer and a drift layer sequentially arranged on the silicon carbide substrate;
[0015] Preferably, the thickness of the epitaxial layer is greater than the thickness of the drift layer and greater than the thickness of the buffer layer.
[0016] Preferably, the content of nitrogen atoms in the epitaxial layer is 1×10 15 -4×10 15 Pieces / cm 3 .
[0017] As a preferred technical solution of the present invention, the silicon carbide substrate includes a silicon carbide substrate that is biased 4° toward the <11-20> direction.
[0018] As a preferred technical solution of the present invention, the thickness of the buffer layer is 0.5-2 μm.
[0019] Preferably, the content of nitrogen atoms in the buffer layer is 1×10 17 -2×10 18 Pieces / cm 3 .
[0020] As a preferred technical solution of the present invention, the thickness of the drift layer is 3-5 μm.
[0021] Preferably, the content of nitrogen atoms in the drift layer is 1×10 15 -4×10 15 Pieces / cm 3 .
[0022] As a preferred technical solution of the present invention, the flow rate of the carrier gas in the high-temperature etching is 100-800slm.
[0023] Preferably, the temperature of the high temperature etching is 1620-1680°C.
[0024] Preferably, the high temperature etching pressure is 50-100 mbar.
[0025] Preferably, the high temperature etching time is 5-20 minutes.
[0026] As a preferred technical solution of the present invention, the flow rate of the silicon source gas during the growth of the buffer layer is 50-100 sccm.
[0027] Preferably, the flow rate of the carbon source gas during the growth of the buffer layer is 30-80 sccm.
[0028] Preferably, the flow rate of the nitrogen dopant during the growth of the buffer layer is 20-30 sccm.
[0029] Preferably, the temperature during the growth of the buffer layer is 1620-1680°C.
[0030] Preferably, the pressure during the growth of the buffer layer is 50-100 mbar.
[0031] As a preferred technical solution of the present invention, the flow rate of the silicon source gas in the first nitrogen-doped growth is 300-600 sccm.
[0032] Preferably, the flow rate of the carbon source gas in the first nitrogen-doped growth is 400-600 sccm.
[0033] Preferably, the flow rate of the nitrogen dopant in the first nitrogen doping growth is 20-30 sccm.
[0034] Preferably, the temperature of the first nitrogen-doped growth is 1620-1680°C.
[0035] Preferably, the pressure of the first nitrogen-doped growth is 50-100 mbar.
[0036] Preferably, the first nitrogen-doped growth time is 8-10 s.
[0037] Preferably, the first undoped growth is a growth process in which no doping is performed.
[0038] Preferably, the flow rate of the silicon source gas in the first undoped growth is 300-600 sccm.
[0039] Preferably, the flow rate of the carbon source gas in the first undoped growth is 400-600 sccm.
[0040] Preferably, the temperature of the first undoped growth is 1620-1680°C.
[0041] Preferably, the pressure of the first undoped growth is 50-100 mbar.
[0042] Preferably, the first undoped growth time is 3-5 s.
[0043] Preferably, the flow rate of the silicon source gas in the second nitrogen-doped growth is 300-600 sccm.
[0044] Preferably, the flow rate of the carbon source gas in the second nitrogen-doped growth is 400-600 sccm.
[0045] Preferably, the flow rate of the nitrogen dopant in the second nitrogen doping growth is 20-30 sccm.
[0046] Preferably, the temperature of the second nitrogen-doped growth is 1620-1680°C.
[0047] Preferably, the pressure of the second nitrogen-doped growth is 50-100 mbar.
[0048] Preferably, the second nitrogen-doping growth time is 7-9 s.
[0049] Preferably, the second non-doped growth is a growth process in which no doping is performed.
[0050] Preferably, the flow rate of the silicon source gas in the second undoped growth is 300-600 sccm.
[0051] Preferably, the flow rate of the carbon source gas in the second undoped growth is 400-600 sccm.
[0052] Preferably, the temperature of the second undoped growth is 1620-1680°C.
[0053] Preferably, the pressure of the second undoped growth is 50-100 mbar.
[0054] Preferably, the second undoped growth time is 3-5 s.
[0055] Preferably, the flow rate of the silicon source gas in the third nitrogen-doped growth is 300-600 sccm.
[0056] Preferably, the flow rate of the carbon source gas in the third nitrogen-doped growth is 400-600 sccm.
[0057] Preferably, the flow rate of the nitrogen dopant in the third nitrogen doping growth is 20-30 sccm.
[0058] Preferably, the temperature of the third nitrogen-doped growth is 1620-1680°C.
[0059] Preferably, the pressure of the third nitrogen-doped growth is 50-100 mbar.
[0060] Preferably, the third nitrogen-doping growth period is 6-8 seconds.
[0061] Preferably, the third undoped growth is a growth process in which no doping is performed.
[0062] Preferably, the flow rate of the silicon source gas in the third undoped growth is 300-600 sccm.
[0063] Preferably, the flow rate of the carbon source gas in the third undoped growth is 400-600 sccm.
[0064] Preferably, the temperature of the third undoped growth is 1620-1680°C.
[0065] Preferably, the third undoped growth pressure is 50-100 mbar.
[0066] Preferably, the third undoped growth period lasts for 3-5 seconds.
[0067] As a preferred technical solution of the present invention, the flow rate of the silicon source gas in the fourth nitrogen-doped growth is 300-600 sccm.
[0068] Preferably, the flow rate of the carbon source gas in the fourth nitrogen-doped growth is 400-600 sccm.
[0069] Preferably, the flow rate of the nitrogen dopant in the fourth nitrogen doping growth is 20-30 sccm.
[0070] Preferably, the temperature of the fourth nitrogen-doped growth is 1620-1680°C.
[0071] Preferably, the pressure of the fourth nitrogen-doped growth is 50-100 mbar.
[0072] Preferably, the fourth nitrogen-doped growth time is 5-7 s.
[0073] Preferably, the fourth undoped growth is a growth process in which no doping is performed.
[0074] Preferably, the flow rate of the silicon source gas in the fourth undoped growth is 300-600 sccm.
[0075] Preferably, the flow rate of the carbon source gas in the fourth undoped growth is 400-600 sccm. Preferably, the temperature of the fourth undoped growth is 1620-1680°C.
[0076] Preferably, the fourth undoped growth pressure is 50-100 mbar.
[0077] Preferably, the fourth undoped growth period lasts for 3-5 seconds.
[0078] Preferably, the flow rate of the silicon source gas in the fifth nitrogen-doped growth is 300-600 sccm.
[0079] Preferably, the flow rate of the carbon source gas in the fifth nitrogen-doped growth is 400-600 sccm.
[0080] Preferably, the flow rate of the nitrogen dopant in the fifth nitrogen doping growth is 20-30 sccm. Preferably, the temperature of the fifth nitrogen doping growth is 1620-1680°C.
[0081] Preferably, the pressure of the fifth nitrogen-doped growth is 50-100 mbar.
[0082] Preferably, the fifth nitrogen-doped growth period is 4-6 seconds.
[0083] Preferably, the fifth undoped growth is a growth process in which no doping is performed.
[0084] Preferably, the flow rate of the silicon source gas in the fifth undoped growth is 300-600 sccm.
[0085] Preferably, the flow rate of the carbon source gas in the fifth undoped growth is 400-600 sccm.
[0086] Preferably, the temperature of the fifth undoped growth is 1620-1680°C.
[0087] Preferably, the fifth undoped growth pressure is 50-100 mbar.
[0088] Preferably, the fifth undoped growth period lasts for 3-5 seconds.
[0089] Preferably, the flow rate of the silicon source gas in the sixth nitrogen-doped growth is 300-600 sccm.
[0090] Preferably, the flow rate of the carbon source gas in the sixth nitrogen-doped growth is 400-600 sccm.
[0091] Preferably, the flow rate of the nitrogen dopant in the sixth nitrogen doping growth is 20-30 sccm. Preferably, the temperature of the sixth nitrogen doping growth is 1620-1680°C.
[0092] Preferably, the pressure of the sixth nitrogen-doped growth is 50-100 mbar.
[0093] Preferably, the sixth nitrogen-doped growth period is 3-5 seconds.
[0094] Preferably, the sixth undoped growth is a growth process in which no doping is performed.
[0095] Preferably, the flow rate of the silicon source gas in the sixth undoped growth is 300-600 sccm.
[0096] Preferably, the flow rate of the carbon source gas in the sixth undoped growth is 400-600 sccm.
[0097] Preferably, the temperature of the sixth undoped growth is 1620-1680°C.
[0098] Preferably, the pressure of the sixth undoped growth is 50-100 mbar.
[0099] Preferably, the sixth undoped growth period lasts for 3-5 seconds.
[0100] Preferably, the epitaxial layer growth is performed 20-100 times.
[0101] As a preferred technical solution of the present invention, the flow rate of the silicon source gas in the drift layer growth is 300-600 sccm.
[0102] Preferably, the flow rate of the carbon source gas during the drift layer growth is 400-600 sccm.
[0103] Preferably, the flow rate of the nitrogen dopant during the growth of the drift layer is 20-30 sccm.
[0104] Preferably, the temperature at which the drift layer grows is 1620-1680°C.
[0105] Preferably, the drift layer is grown at a pressure of 50-100 mbar.
[0106] Compared with the prior art solutions, the present invention has the following beneficial effects:
[0107] The preparation process provided by the present invention realizes the preparation of thick-film silicon carbide epitaxy by setting a specific epitaxial layer growth mode. The distribution uniformity of nitrogen elements in the epitaxial layer of the obtained thick-film silicon carbide epitaxy along the growth direction is significantly improved, which is beneficial to avoiding the defect of high forward voltage of the device. BRIEF DESCRIPTION OF THE DRAWINGS
[0108] Figure 1 It is a schematic diagram of thick film silicon carbide epitaxy provided by an embodiment of the present invention.
[0109] In the figure: 1-silicon carbide substrate, 2-buffer layer, 3-epitaxial layer, 4-drift layer.
[0110] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims. DETAILED DESCRIPTION
[0111] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0112] The present invention provides a method for preparing the aforementioned thick-film silicon carbide epitaxy, the preparation method comprising: sequentially performing high-temperature etching, buffer layer growth, epitaxial layer growth and drift layer growth on a silicon carbide substrate to obtain a thick-film silicon carbide epitaxy.
[0113] The thick film silicon carbide epitaxy Figure 1 As shown, it includes a silicon carbide substrate 1 and a buffer layer 2, an epitaxial layer 3 and a drift layer 4 which are sequentially arranged on the silicon carbide substrate 1;
[0114] The thickness of the epitaxial layer 3 is greater than the thickness of the drift layer 4 and greater than the thickness of the buffer layer 2; the thickness of the epitaxial layer 3 is 100-200 μm; the content of nitrogen atoms in the epitaxial layer 3 is 1×10 15 -4×10 15 Pieces / cm 3 .
[0115] In this embodiment, the thickness of the epitaxial layer 3 is 100-200 μm, for example, 100 μm, 120 μm, 140 μm, 160 μm, 180 μm or 200 μm, etc., but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0116] In this embodiment, the content of nitrogen atoms in the epitaxial layer 3 is 1×10 15 -4×10 15 Pieces / cm 3, for example, it can be 1×10 15 Pieces / cm 3 , 1.5×10 15 Pieces / cm 3 , 2×10 15 Pieces / cm 3 , 2.5×10 15 Pieces / cm 3 , 3×10 15 Pieces / cm 3 , 3.5×10 15 Pieces / cm 3 or 4×10 15 Pieces / cm 3 The above values are not limited to the above values. Other values not listed in the above values also meet the requirements.
[0117] The silicon carbide substrate 1 includes a silicon carbide substrate that is biased 4° toward the <11-20> direction.
[0118] The thickness of the buffer layer 2 is 0.5-2 μm, for example, 0.5 μm, 0.6 μm, 0.8 μm, 1 μm, 1.2 μm, 1.4 μm, 1.6 μm, 1.8 μm or 2 μm, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0119] The content of nitrogen atoms in the buffer layer 2 is 1×10 17 -2×10 18 Pieces / cm 3 , for example, it can be 1×10 17 Pieces / cm 3 , 3×10 17 Pieces / cm 3 , 6×10 17 Pieces / cm 3 ,9×10 17 Pieces / cm 3 , 10×10 17 Pieces / cm 3 , 13×10 17 Pieces / cm 3 , 16×10 17 Pieces / cm 3 or 20×10 17 Pieces / cm 3 The above values are not limited to the above values. Other values not listed in the above values also meet the requirements.
[0120] The thickness of the drift layer 4 is 3-5 μm, for example, 3 μm, 3.2 μm, 3.4 μm, 3.6 μm, 3.8 μm, 4 μm, 4.2 μm, 4.4 μm, 4.6 μm, 4.8 μm or 5 μm, but is not limited to the listed values, and other values not listed in this range also meet the requirements.
[0121] The content of nitrogen atoms in the drift layer 4 is 1×10 15 -4×10 15 Pieces / cm 3 , for example, it can be 1×10 15 Pieces / cm 3 , 1.5×10 15 Pieces / cm 3 , 2×10 15 Pieces / cm 3 , 2.5×10 15 Pieces / cm 3 , 3×10 15 Pieces / cm 3 , 3.5×10 15 Pieces / cm 3 or 4×10 15 Pieces / cm 3 The above values are not limited to the above values. Other values not listed in the above values also meet the requirements.
[0122] Among them, the flow rate of the carrier gas in the high-temperature etching is 100-800slm, for example, it can be 100slm, 150slm, 200slm, 250slm, 300slm, 350slm, 400slm, 450slm, 800slm, 850slm, 900slm, 950slm or 1000slm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0123] Among them, the temperature of the high temperature etching is 1620-1680°C, for example, it can be 1620°C, 1630°C, 1640°C, 1650°C, 1660°C, 1670°C or 1680°C, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0124] The high temperature etching pressure is 50-100 mbar, for example, 50 mbar, 60 mbar, 70 mbar, 80 mbar, 90 mbar or 100 mbar, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0125] The high temperature etching time is 5-20 minutes, for example, 5 minutes, 10 minutes, 15 minutes or 20 minutes, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0126] Among them, the flow rate of the silicon source gas in the growth of the buffer layer is 50-100sccm, for example, it can be 50sccm, 60sccm, 70sccm, 80sccm, 90sccm or 100sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0127] Among them, the flow rate of the carbon source gas in the growth of the buffer layer is 30-80sccm, for example, it can be 30sccm, 40sccm, 50sccm, 60sccm, 70sccm or 80sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0128] Among them, the flow rate of the nitrogen dopant during the growth of the buffer layer is 20-30sccm, for example, it can be 20sccm, 22sccm, 24sccm, 26sccm, 28sccm or 300sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0129] The temperature during the growth of the buffer layer is 1620-1680°C, for example, it can be 1620°C, 1630°C, 1640°C, 1650°C, 1660°C, 1670°C or 1680°C, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0130] The pressure during the growth of the buffer layer is 50-100 mbar, for example, 50 mbar, 60 mbar, 70 mbar, 80 mbar, 90 mbar or 100 mbar, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0131] Among them, the epitaxial layer growth includes the first nitrogen-doped growth, the first non-doped growth, the second nitrogen-doped growth, the second non-doped growth, the third nitrogen-doped growth, the third non-doped growth, the fourth nitrogen-doped growth, the fourth non-doped growth, the fifth nitrogen-doped growth, the fifth non-doped growth, the sixth nitrogen-doped growth and the sixth non-doped growth in sequence; the time of the first nitrogen-doped growth>the time of the second nitrogen-doped growth>the time of the third nitrogen-doped growth>the time of the fourth nitrogen-doped growth>the time of the fifth nitrogen-doped growth>the time of the sixth nitrogen-doped growth.
[0132] Among them, the flow rate of the silicon source gas in the first nitrogen-doped growth is 300-600sccm, for example, it can be 300sccm, 350sccm, 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0133] Among them, the flow rate of the carbon source gas in the first nitrogen-doped growth is 400-600sccm, for example, it can be 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0134] Among them, the flow rate of the nitrogen dopant in the first nitrogen-doped growth is 20-30sccm, for example, it can be 20sccm, 22sccm, 24sccm, 26sccm, 28sccm or 300sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0135] Among them, the temperature of the first nitrogen-doped growth is 1620-1680°C, for example, it can be 1620°C, 1630°C, 1640°C, 1650°C, 1660°C, 1670°C or 1680°C, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0136] The pressure of the first nitrogen-doped growth is 50-100 mbar, for example, 50 mbar, 60 mbar, 70 mbar, 80 mbar, 90 mbar or 100 mbar, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0137] The time of the first nitrogen-doped growth is 8-10 s, for example, 8 s, 8.5 s, 9 s, 9.5 s or 10 s, etc., but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0138] Wherein, the first undoped growth is a growth process in which no doping is performed.
[0139] Among them, the flow rate of the silicon source gas in the first undoped growth is 300-600sccm, for example, it can be 300sccm, 350sccm, 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0140] Among them, the flow rate of the carbon source gas in the first undoped growth is 400-600sccm, for example, it can be 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0141] Among them, the temperature of the first undoped growth is 1620-1680℃, for example, it can be 1620℃, 1630℃, 1640℃, 1650℃, 1660℃, 1670℃ or 1680℃, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0142] The pressure of the first undoped growth is 50-100 mbar, for example, 50 mbar, 60 mbar, 70 mbar, 80 mbar, 90 mbar or 100 mbar, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0143] The first undoped growth time is 3-5s, for example, 3s, 3.5s, 4s, 4.5s or 5s, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0144] Among them, the flow rate of the silicon source gas in the second nitrogen-doped growth is 300-600sccm, for example, it can be 300sccm, 350sccm, 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0145] Among them, the flow rate of the carbon source gas in the second nitrogen-doped growth is 400-600sccm, for example, it can be 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0146] Among them, the flow rate of the nitrogen dopant in the second nitrogen-doped growth is 20-30sccm, for example, it can be 20sccm, 22sccm, 24sccm, 26sccm, 28sccm or 300sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0147] Among them, the temperature of the second nitrogen-doped growth is 1620-1680°C, for example, it can be 1620°C, 1630°C, 1640°C, 1650°C, 1660°C, 1670°C or 1680°C, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0148] The pressure of the second nitrogen-doped growth is 50-100 mbar, for example, 50 mbar, 60 mbar, 70 mbar, 80 mbar, 90 mbar or 100 mbar, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0149] The second nitrogen-doped growth time is 7-9s, for example, 7s, 7.5s, 8s, 8.5s or 9s, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0150] Wherein, the second non-doped growth is a growth process in which no doping is performed.
[0151] Among them, the flow rate of the silicon source gas in the second undoped growth is 300-600sccm, for example, it can be 300sccm, 350sccm, 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0152] Among them, the flow rate of the second carbon source gas in the undoped growth is 400-600sccm, for example, it can be 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0153] Among them, the temperature of the second undoped growth is 1620-1680℃, for example, it can be 1620℃, 1630℃, 1640℃, 1650℃, 1660℃, 1670℃ or 1680℃, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0154] The pressure of the second undoped growth is 50-100 mbar, for example, 50 mbar, 60 mbar, 70 mbar, 80 mbar, 90 mbar or 100 mbar, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0155] The second undoped growth time is 3-5s, for example, 3s, 3.5s, 4s, 4.5s or 5s, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0156] Among them, the flow rate of the silicon source gas in the third nitrogen-doped growth is 300-600sccm, for example, it can be 300sccm, 350sccm, 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0157] Among them, the flow rate of the carbon source gas in the third nitrogen-doped growth is 400-600sccm, for example, it can be 300sccm, 350sccm, 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0158] Among them, the flow rate of the nitrogen dopant in the third nitrogen-doped growth is 20-30sccm, for example, it can be 20sccm, 22sccm, 24sccm, 26sccm, 28sccm or 300sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0159] Among them, the temperature of the third nitrogen-doped growth is 1620-1680°C, for example, it can be 1620°C, 1630°C, 1640°C, 1650°C, 1660°C, 1670°C or 1680°C, but is not limited to the listed values, and other unlisted values in this range also meet the requirements.
[0160] The pressure of the third nitrogen-doped growth is 50-100 mbar, for example, 50 mbar, 60 mbar, 70 mbar, 80 mbar, 90 mbar or 100 mbar, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0161] The time of the third nitrogen-doped growth is 6-8 s, for example, 6 s, 6.5 s, 7 s, 7.5 s or 8 s, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0162] The third undoped growth is a growth process in which no doping is performed.
[0163] Among them, the flow rate of the silicon source gas in the third undoped growth is 300-600sccm, for example, it can be 300sccm, 350sccm, 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0164] Among them, the flow rate of the third carbon source gas in the undoped growth is 400-600sccm, for example, it can be 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0165] Among them, the temperature of the third undoped growth is 1620-1680℃, for example, it can be 1620℃, 1630℃, 1640℃, 1650℃, 1660℃, 1670℃ or 1680℃, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0166] The third undoped growth pressure is 50-100 mbar, for example, 50 mbar, 60 mbar, 70 mbar, 80 mbar, 90 mbar or 100 mbar, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0167] The third undoped growth time is 3-5s, for example, 3s, 3.5s, 4s, 4.5s or 5s, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0168] Among them, the flow rate of the silicon source gas in the fourth nitrogen-doped growth is 300-600sccm, for example, it can be 300sccm, 350sccm, 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0169] Among them, the flow rate of the carbon source gas in the fourth nitrogen-doped growth is 400-600sccm, for example, it can be 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0170] Among them, the flow rate of the nitrogen dopant in the fourth nitrogen-doped growth is 20-30sccm, for example, it can be 20sccm, 22sccm, 24sccm, 26sccm, 28sccm or 300sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0171] Among them, the temperature of the fourth nitrogen-doped growth is 1620-1680°C, for example, it can be 1620°C, 1630°C, 1640°C, 1650°C, 1660°C, 1670°C or 1680°C, but is not limited to the listed values, and other unlisted values in this range also meet the requirements.
[0172] The pressure of the fourth nitrogen-doped growth is 50-100 mbar, for example, 50 mbar, 60 mbar, 70 mbar, 80 mbar, 90 mbar or 100 mbar, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0173] The fourth nitrogen-doped growth time is 5-7s, for example, 5s, 5.5s, 6s, 6.5s or 7s, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0174] The fourth undoped growth is growth without doping.
[0175] Among them, the flow rate of the silicon source gas in the fourth undoped growth is 300-600sccm, for example, it can be 300sccm, 350sccm, 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0176] Among them, the flow rate of the carbon source gas in the fourth undoped growth is 400-600sccm, for example, it can be 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0177] Among them, the temperature of the fourth undoped growth is 1620-1680℃, for example, it can be 1620℃, 1630℃, 1640℃, 1650℃, 1660℃, 1670℃ or 1680℃, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0178] The fourth undoped growth pressure is 50-100 mbar, for example, 50 mbar, 60 mbar, 70 mbar, 80 mbar, 90 mbar or 100 mbar, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0179] The fourth undoped growth time is 3-5s, for example, 3s, 3.5s, 4s, 4.5s or 5s, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0180] Among them, the flow rate of the silicon source gas in the fifth nitrogen-doped growth is 300-600sccm, for example, it can be 300sccm, 350sccm, 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0181] Among them, the flow rate of the carbon source gas in the fifth nitrogen-doped growth is 400-600sccm, for example, it can be 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0182] Among them, the flow rate of the nitrogen dopant in the fifth nitrogen-doped growth is 20-30sccm, for example, it can be 20sccm, 22sccm, 24sccm, 26sccm, 28sccm or 300sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0183] Among them, the temperature of the fifth nitrogen-doped growth is 1620-1680°C, for example, it can be 1620°C, 1630°C, 1640°C, 1650°C, 1660°C, 1670°C or 1680°C, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0184] The fifth nitrogen-doped growth pressure is 50-100 mbar, for example, 50 mbar, 60 mbar, 70 mbar, 80 mbar, 90 mbar or 100 mbar, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0185] The fifth nitrogen-doped growth time is 4-6 s, for example, 4 s, 4.5 s, 5 s, 5.5 s, or 6 s, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0186] The fifth undoped growth is a growth process in which no doping is performed.
[0187] Among them, the flow rate of the silicon source gas in the fifth undoped growth is 300-600sccm, for example, it can be 300sccm, 350sccm, 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0188] Among them, the flow rate of the fifth carbon source gas in the undoped growth is 400-600sccm, for example, it can be 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0189] Among them, the temperature of the fifth undoped growth is 1620-1680℃, for example, it can be 1620℃, 1630℃, 1640℃, 1650℃, 1660℃, 1670℃ or 1680℃, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0190] The fifth undoped growth pressure is 50-100 mbar, for example, 50 mbar, 60 mbar, 70 mbar, 80 mbar, 90 mbar or 100 mbar, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0191] The fifth undoped growth time is 3-5s, for example, 3s, 3.5s, 4s, 4.5s or 5s, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0192] Among them, the flow rate of the silicon source gas in the sixth nitrogen-doped growth is 300-600sccm, for example, it can be 300sccm, 350sccm, 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0193] Among them, the flow rate of the carbon source gas in the sixth nitrogen-doped growth is 400-600sccm, for example, it can be 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0194] Among them, the flow rate of the nitrogen dopant in the sixth nitrogen-doped growth is 20-30sccm, for example, it can be 20sccm, 22sccm, 24sccm, 26sccm, 28sccm or 30sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0195] Among them, the temperature of the sixth nitrogen-doped growth is 1620-1680°C, for example, it can be 1620°C, 1630°C, 1640°C, 1650°C, 1660°C, 1670°C or 1680°C, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0196] The pressure of the sixth nitrogen-doped growth is 50-100 mbar, for example, 50 mbar, 60 mbar, 70 mbar, 80 mbar, 90 mbar or 100 mbar, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0197] The sixth nitrogen-doped growth time is 3-5 s, for example, 3 s, 3.5 s, 4 s, 4.5 s or 5 s, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0198] The sixth undoped growth is a growth process in which no doping is performed.
[0199] Among them, the flow rate of the silicon source gas in the sixth undoped growth is 300-600sccm, for example, it can be 300sccm, 350sccm, 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0200] Among them, the flow rate of the sixth carbon source gas in the undoped growth is 400-600sccm, for example, it can be 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0201] Among them, the temperature of the sixth undoped growth is 1620-1680℃, for example, it can be 1620℃, 1630℃, 1640℃, 1650℃, 1660℃, 1670℃ or 1680℃, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0202] The sixth undoped growth pressure is 50-100 mbar, for example, 50 mbar, 60 mbar, 70 mbar, 80 mbar, 90 mbar or 100 mbar, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0203] The sixth undoped growth time is 3-5 s, for example, 3 s, 3.5 s, 4 s, 4.5 s or 5 s, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0204] The epitaxial layer growth is performed 20-100 times, for example, 20 times, 30 times, 40 times, 50 times, 60 times, 70 times, 80 times, 90 times or 100 times.
[0205] Among them, the flow rate of the silicon source gas in the drift layer growth is 300-600sccm, for example, it can be 300sccm, 350sccm, 400sccm, 450sccm, 500sccm, 550sccm or 660sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0206] The flow rate of the carbon source gas in the drift layer growth is 400-600 sccm, for example, 400 sccm, 450 sccm, 500 sccm, 550 sccm or 660 sccm, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0207] Among them, the flow rate of the nitrogen dopant in the drift layer growth is 20-30sccm, for example, it can be 20sccm, 22sccm, 24sccm, 26sccm, 28sccm or 30sccm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0208] The temperature of the drift layer growth is 1620-1680°C, for example, 1620°C, 1630°C, 1640°C, 1650°C, 1660°C, 1670°C or 1680°C, but is not limited to the listed values, and other values not listed in the range also meet the requirements.
[0209] The pressure of the drift layer growth is 50-100 mbar, for example, 50 mbar, 60 mbar, 70 mbar, 80 mbar, 90 mbar or 100 mbar, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0210] In the present invention, the carrier gas used in the preparation process includes commonly used carrier gases in the art such as hydrogen.
[0211] In the present invention, the silicon source gas used in the preparation process includes one or a combination of at least two of SiCl4, SiHCl3, SiH2C12 or SiH3Cl, and other chlorine-containing silicon source gases commonly used in the art.
[0212] In the present invention, the carbon source gas used in the preparation process includes one or a combination of at least two of C2H2, C2H4 or C3H8 and other commonly used carbon source gases in the art.
[0213] In the present invention, the nitrogen dopant used in the preparation process includes nitrogen and / or ammonia and other N-type dopants commonly used in the art.
[0214] In the present invention, the time for the growth of the buffer layer, the epitaxial layer and the drift layer during the preparation process can be reasonably selected according to the required thickness of the layer.
[0215] Further, in order to illustrate the good effects that can be achieved by the thick film silicon carbide epitaxy provided by the present invention, actual examples are used for illustration, as follows:
[0216] Example 1
[0217] This embodiment provides a thick-film silicon carbide epitaxy, wherein the thick-film silicon carbide epitaxy comprises a silicon carbide substrate and a buffer layer, an epitaxial layer and a drift layer sequentially arranged on the silicon carbide substrate;
[0218] Wherein, the silicon carbide substrate is a silicon carbide substrate that is biased 4° toward the <11-20> direction;
[0219] The thickness of the buffer layer is 1.5 μm; the content of nitrogen atoms in the buffer layer is 1×10 18 Pieces / cm 3 ; The thickness of the epitaxial layer is 150 μm; The content of nitrogen atoms in the epitaxial layer is 3×10 15 Pieces / cm 3 ; The thickness of the drift layer is 4 μm; The content of nitrogen atoms in the drift layer is 2×10 15 Pieces / cm 3 .
[0220] The preparation process is as follows: a silicon carbide substrate is subjected to high temperature etching, buffer layer growth, epitaxial layer growth and drift layer growth in sequence to obtain a thick film silicon carbide epitaxial layer;
[0221] The flow rate of the carrier gas in the high temperature etching is 500 slm, the temperature is 1660°C, the pressure is 80 mbar, and the time is 15 min;
[0222] During the growth of the buffer layer, the flow rate of the silicon source gas is 80 sccm, the flow rate of the carbon source gas is 60 sccm, the flow rate of the nitrogen dopant is 28 sccm, the temperature is 1660° C., and the pressure is 80 mbar;
[0223] The epitaxial layer growth includes sequentially performing a first nitrogen-doped growth, a first non-doped growth, a second nitrogen-doped growth, a second non-doped growth, a third nitrogen-doped growth, a third non-doped growth, a fourth nitrogen-doped growth, a fourth non-doped growth, a fifth nitrogen-doped growth, a fifth non-doped growth, a sixth nitrogen-doped growth and a sixth non-doped growth;
[0224] In the first nitrogen-doped growth, the flow rate of the silicon source gas is 500 sccm, the flow rate of the carbon source gas is 500 sccm; the flow rate of the nitrogen dopant is 25 sccm, the temperature is 1660°C, the pressure is 80 mbar, and the time is 9 s; in the first undoped growth, no doping is performed during the growth process, the flow rate of the silicon source gas is 500 sccm, the flow rate of the carbon source gas is 500 sccm, the temperature is 1660°C, the pressure is 80 mbar, and the time is 4 s;
[0225] In the second nitrogen-doped growth, the flow rate of the silicon source gas is 500 sccm, the flow rate of the carbon source gas is 500 sccm, the flow rate of the nitrogen dopant is 25 sccm, the temperature is 1660° C., the pressure is 80 mbar, and the time is 8 s; in the second non-doped growth, no doping is performed during the growth process, the flow rate of the silicon source gas is 500 sccm, the flow rate of the carbon source gas is 500 sccm, the temperature is 1660° C., the pressure is 80 mbar, and the time is 4 s;
[0226] In the third nitrogen-doped growth, the flow rate of the silicon source gas is 500 sccm, the flow rate of the carbon source gas is 500 sccm, the flow rate of the nitrogen dopant is 25 sccm, the temperature is 1660° C., the pressure is 80 mbar, and the time is 7 s; in the third undoped growth, no doping is performed during the growth process, the flow rate of the silicon source gas is 500 sccm, the flow rate of the carbon source gas is 500 sccm, the temperature is 1660° C., the pressure is 80 mbar, and the time is 4 s;
[0227] In the fourth nitrogen-doped growth, the flow rate of the silicon source gas is 500 sccm, the flow rate of the carbon source gas is 500 sccm, the flow rate of the nitrogen dopant is 25 sccm, the temperature is 1660° C., the pressure is 80 mbar, and the time is 6 s; in the fourth undoped growth, no doping is performed during the growth process, the flow rate of the silicon source gas is 500 sccm, the flow rate of the carbon source gas is 500 sccm, the temperature is 1660° C., the pressure is 80 mbar, and the time is 4 s;
[0228] In the fifth nitrogen-doped growth, the flow rate of the silicon source gas is 500 sccm, the flow rate of the carbon source gas is 500 sccm, the flow rate of the nitrogen dopant is 25 sccm, the temperature is 1660° C., the pressure is 80 mbar, and the time is 5 s; in the fifth undoped growth, no doping is performed during the growth process, the flow rate of the silicon source gas is 500 sccm, the flow rate of the carbon source gas is 500 sccm, the temperature is 1660° C., the pressure is 80 mbar, and the time is 4 s;
[0229] In the sixth nitrogen-doped growth, the flow rate of the silicon source gas is 500 sccm, the flow rate of the carbon source gas is 500 sccm, the flow rate of the nitrogen dopant is 25 sccm, the temperature is 1660° C., the pressure is 80 mbar, and the time is 4 s; in the sixth undoped growth, no doping is performed during the growth process, the flow rate of the silicon source gas is 500 sccm, the flow rate of the carbon source gas is 500 sccm, the temperature is 1660° C., the pressure is 80 mbar, and the time is 4 s;
[0230] The epitaxial layer growth is performed 75 times;
[0231] During the growth of the drift layer, the flow rate of the silicon source gas is 500 sccm, the flow rate of the carbon source gas is 500 sccm, the flow rate of the nitrogen dopant is 25 sccm, the temperature is 1660° C., and the pressure is 80 mbar.
[0232] In this embodiment, the carrier gas used in the preparation process is hydrogen, the silicon source gas used is SiCl4 gas, the carbon source gas used is C2H2, and the nitrogen dopant used is nitrogen.
[0233] Example 2
[0234] This embodiment provides a thick-film silicon carbide epitaxy, wherein the thick-film silicon carbide epitaxy comprises a silicon carbide substrate and a buffer layer, an epitaxial layer and a drift layer sequentially arranged on the silicon carbide substrate;
[0235] Wherein, the silicon carbide substrate is a silicon carbide substrate that is biased 4° toward the <11-20> direction;
[0236] The thickness of the buffer layer is 1 μm; the content of nitrogen atoms in the buffer layer is 5×10 17 Pieces / cm 3 ; The thickness of the epitaxial layer is 120 μm; The content of nitrogen atoms in the epitaxial layer is 2×10 15 Pieces / cm 3 ; The thickness of the drift layer is 5 μm; The content of nitrogen atoms in the drift layer is 3×10 15 Pieces / cm 3 .
[0237] The preparation process is as follows: a silicon carbide substrate is subjected to high temperature etching, buffer layer growth, epitaxial layer growth and drift layer growth in sequence to obtain a thick film silicon carbide epitaxial layer;
[0238] The flow rate of the carrier gas in the high temperature etching is 100 slm, the temperature is 1620°C, the pressure is 50 mbar, and the time is 20 min;
[0239] During the growth of the buffer layer, the flow rate of the silicon source gas is 50 sccm, the flow rate of the carbon source gas is 30 sccm, the flow rate of the nitrogen dopant is 20 sccm, the temperature is 1620° C., and the pressure is 50 mbar;
[0240] The epitaxial layer growth includes sequentially performing a first nitrogen-doped growth, a first non-doped growth, a second nitrogen-doped growth, a second non-doped growth, a third nitrogen-doped growth, a third non-doped growth, a fourth nitrogen-doped growth, a fourth non-doped growth, a fifth nitrogen-doped growth, a fifth non-doped growth, a sixth nitrogen-doped growth and a sixth non-doped growth;
[0241] In the first nitrogen-doped growth, the flow rate of the silicon source gas is 600 sccm, the flow rate of the carbon source gas is 600 sccm; the flow rate of the nitrogen dopant is 30 sccm, the temperature is 1680°C, the pressure is 100 mbar, and the time is 10 s; in the first undoped growth, no doping is performed during the growth process, the flow rate of the silicon source gas is 600 sccm, the flow rate of the carbon source gas is 600 sccm, the temperature is 1680°C, the pressure is 100 mbar, and the time is 5 s;
[0242] In the second nitrogen-doped growth, the flow rate of the silicon source gas is 600 sccm, the flow rate of the carbon source gas is 600 sccm, the flow rate of the nitrogen dopant is 30 sccm, the temperature is 1680° C., the pressure is 100 mbar, and the time is 9 s; in the second non-doped growth, no doping is performed during the growth process, the flow rate of the silicon source gas is 600 sccm, the flow rate of the carbon source gas is 600 sccm, the temperature is 1680° C., the pressure is 100 mbar, and the time is 5 s;
[0243] In the third nitrogen-doped growth, the flow rate of the silicon source gas is 600 sccm, the flow rate of the carbon source gas is 600 sccm, the flow rate of the nitrogen dopant is 30 sccm, the temperature is 1680° C., the pressure is 100 mbar, and the time is 8 s; in the third undoped growth, no doping is performed during the growth process, the flow rate of the silicon source gas is 600 sccm, the flow rate of the carbon source gas is 600 sccm, the temperature is 1680° C., the pressure is 100 mbar, and the time is 5 s;
[0244] In the fourth nitrogen-doped growth, the flow rate of the silicon source gas is 600 sccm, the flow rate of the carbon source gas is 600 sccm, the flow rate of the nitrogen dopant is 30 sccm, the temperature is 1680° C., the pressure is 100 mbar, and the time is 7 s; in the fourth undoped growth, no doping is performed during the growth process, the flow rate of the silicon source gas is 600 sccm, the flow rate of the carbon source gas is 600 sccm, the temperature is 1680° C., the pressure is 100 mbar, and the time is 5 s;
[0245] In the fifth nitrogen-doped growth, the flow rate of the silicon source gas is 600 sccm, the flow rate of the carbon source gas is 600 sccm, the flow rate of the nitrogen dopant is 30 sccm, the temperature is 1680° C., the pressure is 100 mbar, and the time is 6 s; in the fifth undoped growth, no doping is performed during the growth process, the flow rate of the silicon source gas is 600 sccm, the flow rate of the carbon source gas is 600 sccm, the temperature is 1680° C., the pressure is 100 mbar, and the time is 5 s;
[0246] In the sixth nitrogen-doped growth, the flow rate of the silicon source gas is 600 sccm, the flow rate of the carbon source gas is 600 sccm, the flow rate of the nitrogen dopant is 30 sccm, the temperature is 1680° C., the pressure is 100 mbar, and the time is 5 s; in the sixth undoped growth, no doping is performed during the growth process, the flow rate of the silicon source gas is 600 sccm, the flow rate of the carbon source gas is 600 sccm, the temperature is 1680° C., the pressure is 100 mbar, and the time is 5 s;
[0247] The epitaxial layer growth is performed 60 times;
[0248] During the growth of the drift layer, the flow rate of the silicon source gas is 600 sccm, the flow rate of the carbon source gas is 600 sccm, the flow rate of the nitrogen dopant is 30 sccm, the temperature is 1680° C., and the pressure is 100 mbar.
[0249] In this embodiment, the carrier gas used in the preparation process is hydrogen, the silicon source gas used is SiHCl3, the carbon source gas used is C2H4, and the nitrogen dopant used is ammonia.
[0250] Example 3
[0251] This embodiment provides a thick-film silicon carbide epitaxy, wherein the thick-film silicon carbide epitaxy comprises a silicon carbide substrate and a buffer layer, an epitaxial layer and a drift layer sequentially arranged on the silicon carbide substrate;
[0252] Wherein, the silicon carbide substrate is a silicon carbide substrate that is biased 4° toward the <11-20> direction;
[0253] The thickness of the buffer layer is 2 μm; the content of nitrogen atoms in the buffer layer is 2×10 18 Pieces / cm3 ; The thickness of the epitaxial layer is 200 μm; The content of nitrogen atoms in the epitaxial layer is 4×10 15 Pieces / cm 3 ; The thickness of the drift layer is 3 μm; The content of nitrogen atoms in the drift layer is 4×10 15 Pieces / cm 3 .
[0254] The preparation process is as follows: a silicon carbide substrate is subjected to high temperature etching, buffer layer growth, epitaxial layer growth and drift layer growth in sequence to obtain a thick film silicon carbide epitaxial layer;
[0255] The high temperature etching process has a carrier gas flow rate of 800 slm, a temperature of 1680°C, a pressure of 100 mbar, and a time of 5 min.
[0256] During the growth of the buffer layer, the flow rate of the silicon source gas is 100 sccm, the flow rate of the carbon source gas is 80 sccm, the flow rate of the nitrogen dopant is 30 sccm, the temperature is 1680° C., and the pressure is 100 mbar;
[0257] The epitaxial layer growth includes sequentially performing a first nitrogen-doped growth, a first non-doped growth, a second nitrogen-doped growth, a second non-doped growth, a third nitrogen-doped growth, a third non-doped growth, a fourth nitrogen-doped growth, a fourth non-doped growth, a fifth nitrogen-doped growth, a fifth non-doped growth, a sixth nitrogen-doped growth and a sixth non-doped growth;
[0258] In the first nitrogen-doped growth, the flow rate of the silicon source gas is 300 sccm, the flow rate of the carbon source gas is 400 sccm, the flow rate of the nitrogen dopant is 20 sccm, the temperature is 1620° C., the pressure is 50 mbar, and the time is 8 s; in the first undoped growth, no doping is performed during the growth process, the flow rate of the silicon source gas is 300 sccm, the flow rate of the carbon source gas is 400 sccm, the temperature is 1620° C., the pressure is 50 mbar, and the time is 3 s;
[0259] In the second nitrogen-doped growth, the flow rate of the silicon source gas is 300 sccm, the flow rate of the carbon source gas is 400 sccm, the flow rate of the nitrogen dopant is 20 sccm, the temperature is 1620° C., the pressure is 50 mbar, and the time is 7 s; in the second non-doped growth, no doping is performed during the growth process, the flow rate of the silicon source gas is 300 sccm, the flow rate of the carbon source gas is 400 sccm, the temperature is 1620° C., the pressure is 50 mbar, and the time is 3 s;
[0260] In the third nitrogen-doped growth, the flow rate of the silicon source gas is 300 sccm, the flow rate of the carbon source gas is 400 sccm, the flow rate of the nitrogen dopant is 20 sccm, the temperature is 1620° C., the pressure is 50 mbar, and the time is 6 s; in the third undoped growth, no doping is performed during the growth process, the flow rate of the silicon source gas is 300 sccm, the flow rate of the carbon source gas is 400 sccm, the temperature is 1620° C., the pressure is 50 mbar, and the time is 3 s;
[0261] In the fourth nitrogen-doped growth, the flow rate of the silicon source gas is 300 sccm, the flow rate of the carbon source gas is 400 sccm, the flow rate of the nitrogen dopant is 20 sccm, the temperature is 1620° C., the pressure is 50 mbar, and the time is 5 s; in the fourth undoped growth, no doping is performed during the growth process, the flow rate of the silicon source gas is 300 sccm, the flow rate of the carbon source gas is 400 sccm, the temperature is 1620° C., the pressure is 50 mbar, and the time is 3 s;
[0262] In the fifth nitrogen-doped growth, the flow rate of the silicon source gas is 300 sccm, the flow rate of the carbon source gas is 400 sccm, the flow rate of the nitrogen dopant is 20 sccm, the temperature is 1620° C., the pressure is 50 mbar, and the time is 4 s; in the fifth undoped growth, no doping is performed during the growth process, the flow rate of the silicon source gas is 300 sccm, the flow rate of the carbon source gas is 400 sccm, the temperature is 1620° C., the pressure is 50 mbar, and the time is 3 s;
[0263] In the sixth nitrogen-doped growth, the flow rate of the silicon source gas is 300 sccm, the flow rate of the carbon source gas is 400 sccm, the flow rate of the nitrogen dopant is 20 sccm, the temperature is 1620° C., the pressure is 50 mbar, and the time is 3 s; in the sixth undoped growth, no doping is performed during the growth process, the flow rate of the silicon source gas is 300 sccm, the flow rate of the carbon source gas is 400 sccm, the temperature is 1620° C., the pressure is 50 mbar, and the time is 3 s;
[0264] The epitaxial layer growth is performed 100 times;
[0265] During the growth of the drift layer, the flow rate of the silicon source gas is 300 sccm, the flow rate of the carbon source gas is 400 sccm, the flow rate of the nitrogen dopant is 20 sccm, the temperature is 1620° C., and the pressure is 50 mbar.
[0266] In this embodiment, the carrier gas used in the preparation process is hydrogen, the silicon source gas used is SiH3Cl, the carbon source gas used is C3H8, and the nitrogen dopant used is ammonia.
[0267] Comparative Example 1
[0268] The only difference from Example 1 is that the epitaxial layer growth only performs the first nitrogen-doped growth to obtain an epitaxial layer of designed thickness.
[0269] Comparative Example 2
[0270] The only difference from Example 1 is that the first undoped growth is not performed.
[0271] Comparative Example 3
[0272] The only difference from Example 1 is that the second undoped growth is not performed.
[0273] Comparative Example 4
[0274] The only difference from Example 1 is that the third undoped growth is not performed.
[0275] Comparative Example 5
[0276] The only difference from Example 1 is that the fifth undoped growth is not performed.
[0277] Comparative Example 6
[0278] The only difference from Example 1 is that the sixth undoped growth is not performed.
[0279] Comparative Example 7
[0280] The only difference from Example 1 is that the time of the first undoped growth is 8 s.
[0281] Comparative Example 8
[0282] The only difference from Example 1 is that the time of the first undoped growth is 1 s.
[0283] Comparative Example 9
[0284] The only difference from Example 1 is that the time of the third undoped growth is 8 s.
[0285] Comparative Example 10
[0286] The only difference from Example 1 is that the time of the third undoped growth is 1 s.
[0287] Comparative Example 11
[0288] The only difference from Example 1 is that the time of the sixth undoped growth is 8 s.
[0289] Comparative Example 12
[0290] The only difference from Example 1 is that the time of the sixth undoped growth is 1 s.
[0291] Comparative Example 13
[0292] The only difference from Example 1 is that nitrogen doping is performed during the third undoped growth, and the flow rate of the nitrogen dopant is 25 sccm.
[0293] The thick film silicon carbide epitaxy obtained in the embodiment and the comparative example was tested for the uniformity of N element distribution along the growth direction, and the forward voltage of the sample device was tested according to GB / T 4586. The test results are shown in Table 1 below.
[0294] Table 1
[0295]
[0296]
[0297] As can be seen from Table 1, in the solution provided by the present invention, the N-doping uniformity of the obtained thick-film silicon carbide epitaxy is significantly improved through the design of the epitaxial layer growth process, and the forward voltage of the device using thick-film silicon carbide epitaxy is significantly reduced, and the forward voltage is ≤1.382V, which is conducive to the preparation of high-power devices.
[0298] It is stated that the present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0299] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0300] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0301] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing thick film silicon carbide epitaxy, characterized in that: The preparation method comprises: performing high temperature etching, buffer layer growth, epitaxial layer growth and drift layer growth on a silicon carbide substrate in sequence to obtain thick film silicon carbide epitaxy; Wherein, the epitaxial layer growth includes the first nitrogen-doped growth, the first non-doped growth, the second nitrogen-doped growth, the second non-doped growth, the third nitrogen-doped growth, the third non-doped growth, the fourth nitrogen-doped growth, the fourth non-doped growth, the fifth nitrogen-doped growth, the fifth non-doped growth, the sixth nitrogen-doped growth and the sixth non-doped growth in sequence; the time of the first nitrogen-doped growth> the time of the second nitrogen-doped growth> the time of the third nitrogen-doped growth> the time of the fourth nitrogen-doped growth> the time of the fifth nitrogen-doped growth> the time of the sixth nitrogen-doped growth; The thickness of the epitaxial layer in the thick film silicon carbide epitaxy is 100-200 μm.
2. The preparation method according to claim 1, characterized in that: The thick film silicon carbide epitaxy comprises a silicon carbide substrate and a buffer layer, an epitaxial layer and a drift layer sequentially arranged on the silicon carbide substrate; Preferably, the thickness of the epitaxial layer>the thickness of the drift layer>the thickness of the buffer layer; Preferably, the content of nitrogen atoms in the epitaxial layer is 1×10 15 -4×10 15 Pieces / cm 3 .
3. The preparation method according to claim 1 or 2, characterized in that: The silicon carbide substrate includes a silicon carbide substrate that is biased 4° toward a <11-20> direction.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The thickness of the buffer layer is 0.5-2 μm; Preferably, the content of nitrogen atoms in the buffer layer is 1×10 17 -2×10 18 Pieces / cm 3 .
5. The preparation method according to any one of claims 1 to 4, characterized in that: The thickness of the drift layer is 3-5 μm; Preferably, the content of nitrogen atoms in the drift layer is 1×10 15 -4×10 15 Pieces / cm 3 .
6. The preparation method according to any one of claims 1 to 5, characterized in that: The flow rate of the carrier gas in the high temperature etching is 100-800slm; Preferably, the temperature of the high temperature etching is 1620-1680°C; Preferably, the high temperature etching pressure is 50-100 mbar; Preferably, the high temperature etching time is 5-20 minutes.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The flow rate of the silicon source gas during the growth of the buffer layer is 50-100 sccm; Preferably, the flow rate of the carbon source gas during the growth of the buffer layer is 30-80 sccm; Preferably, the flow rate of the nitrogen dopant during the growth of the buffer layer is 20-30 sccm; Preferably, the temperature during the growth of the buffer layer is 1620-1680°C; Preferably, the pressure during the growth of the buffer layer is 50-100 mbar.
8. The preparation method according to any one of claims 1 to 7, characterized in that: The flow rate of the silicon source gas in the first nitrogen-doped growth is 300-600 sccm; Preferably, the flow rate of the carbon source gas in the first nitrogen-doped growth is 400-600 sccm; Preferably, the flow rate of the nitrogen dopant in the first nitrogen doping growth is 20-30 sccm; Preferably, the temperature of the first nitrogen-doped growth is 1620-1680°C; Preferably, the pressure of the first nitrogen-doped growth is 50-100 mbar; Preferably, the first nitrogen-doped growth time is 8-10s; Preferably, the first undoped growth is a growth process in which no doping is performed; Preferably, the flow rate of the silicon source gas in the first undoped growth is 300-600 sccm; Preferably, the flow rate of the carbon source gas in the first undoped growth is 400-600 sccm; Preferably, the temperature of the first undoped growth is 1620-1680°C; Preferably, the pressure of the first undoped growth is 50-100 mbar; Preferably, the first undoped growth time is 3-5s; Preferably, the flow rate of the silicon source gas in the second nitrogen-doped growth is 300-600 sccm; Preferably, the flow rate of the carbon source gas in the second nitrogen-doped growth is 400-600 sccm; Preferably, the flow rate of the nitrogen dopant in the second nitrogen doping growth is 20-30 sccm; Preferably, the temperature of the second nitrogen-doped growth is 1620-1680°C; Preferably, the pressure of the second nitrogen-doped growth is 50-100 mbar; Preferably, the second nitrogen-doping growth time is 7-9s; Preferably, the second non-doped growth is a growth process in which no doping is performed; Preferably, the flow rate of the silicon source gas in the second undoped growth is 300-600 sccm; Preferably, the flow rate of the carbon source gas in the second undoped growth is 400-600 sccm; Preferably, the temperature of the second undoped growth is 1620-1680°C; Preferably, the pressure of the second undoped growth is 50-100 mbar; Preferably, the second undoped growth time is 3-5s; Preferably, the flow rate of the silicon source gas in the third nitrogen-doped growth is 300-600 sccm; Preferably, the flow rate of the carbon source gas in the third nitrogen-doped growth is 400-600 sccm; Preferably, the flow rate of the nitrogen dopant in the third nitrogen doping growth is 20-30 sccm; Preferably, the temperature of the third nitrogen-doped growth is 1620-1680°C; Preferably, the pressure of the third nitrogen-doped growth is 50-100 mbar; Preferably, the third nitrogen-doping growth time is 6-8s; Preferably, the third undoped growth is a growth process in which no doping is performed; Preferably, the flow rate of the silicon source gas in the third undoped growth is 300-600 sccm; Preferably, the flow rate of the carbon source gas in the third undoped growth is 400-600 sccm; Preferably, the temperature of the third undoped growth is 1620-1680°C; Preferably, the pressure of the third undoped growth is 50-100 mbar; Preferably, the third undoped growth period lasts for 3-5 seconds.
9. The preparation method according to any one of claims 1 to 8, characterized in that: The flow rate of the silicon source gas in the fourth nitrogen-doped growth is 300-600 sccm; Preferably, the flow rate of the carbon source gas in the fourth nitrogen-doped growth is 400-600 sccm; Preferably, the flow rate of the nitrogen dopant in the fourth nitrogen doping growth is 20-30 sccm; Preferably, the temperature of the fourth nitrogen-doped growth is 1620-1680°C; Preferably, the pressure of the fourth nitrogen-doped growth is 50-100 mbar; Preferably, the fourth nitrogen-doped growth time is 5-7s; Preferably, the fourth undoped growth is that no doping is performed during the growth process; Preferably, the flow rate of the silicon source gas in the fourth undoped growth is 300-600 sccm; Preferably, the flow rate of the carbon source gas in the fourth undoped growth is 400-600 sccm; Preferably, the temperature of the fourth undoped growth is 1620-1680°C; Preferably, the pressure of the fourth undoped growth is 50-100 mbar; Preferably, the fourth undoped growth time is 3-5s; Preferably, the flow rate of the silicon source gas in the fifth nitrogen-doped growth is 300-600 sccm; Preferably, the flow rate of the carbon source gas in the fifth nitrogen-doped growth is 400-600 sccm; Preferably, the flow rate of the nitrogen dopant in the fifth nitrogen doping growth is 20-30 sccm; Preferably, the temperature of the fifth nitrogen-doped growth is 1620-1680°C; Preferably, the pressure of the fifth nitrogen-doped growth is 50-100 mbar; Preferably, the fifth nitrogen-doped growth time is 4-6s; Preferably, the fifth undoped growth is a growth process in which no doping is performed; Preferably, the flow rate of the silicon source gas in the fifth undoped growth is 300-600 sccm; Preferably, the flow rate of the carbon source gas in the fifth undoped growth is 400-600 sccm; Preferably, the temperature of the fifth undoped growth is 1620-1680°C; Preferably, the pressure of the fifth undoped growth is 50-100 mbar; Preferably, the fifth undoped growth time is 3-5s; Preferably, the flow rate of the silicon source gas in the sixth nitrogen-doped growth is 300-600 sccm; Preferably, the flow rate of the carbon source gas in the sixth nitrogen-doped growth is 400-600 sccm; Preferably, the flow rate of the nitrogen dopant in the sixth nitrogen doping growth is 20-30 sccm; Preferably, the temperature of the sixth nitrogen-doped growth is 1620-1680° C.; Preferably, the pressure of the sixth nitrogen-doped growth is 50-100 mbar; Preferably, the sixth nitrogen-doped growth time is 3-5s; Preferably, the sixth undoped growth is a growth process in which no doping is performed; Preferably, the flow rate of the silicon source gas in the sixth undoped growth is 300-600 sccm; Preferably, the flow rate of the carbon source gas in the sixth undoped growth is 400-600 sccm; Preferably, the temperature of the sixth undoped growth is 1620-1680°C; Preferably, the pressure of the sixth undoped growth is 50-100 mbar; Preferably, the sixth undoped growth time is 3-5s; Preferably, the epitaxial layer growth is performed 20-100 times.
10. The preparation method according to any one of claims 1 to 9, characterized in that: The flow rate of the silicon source gas during the drift layer growth is 300-600 sccm; Preferably, the flow rate of the carbon source gas in the drift layer growth is 400-600 sccm; Preferably, the flow rate of the nitrogen dopant during the growth of the drift layer is 20-30 sccm; Preferably, the temperature of the drift layer growth is 1620-1680°C; Preferably, the drift layer is grown at a pressure of 50-100 mbar.